Artificial stone and preparation method thereof
By mixing natural ore and used waste concrete blocks in specific proportions and using ultrasonic oscillation, microwave baking and extrusion molding processes, artificial stone with parallel distribution channels is prepared, which solves the high cost and bubble hole problems, and improves strength and resource utilization , which enhances the portability of marketing and use.
Patent Information
- Application Number
- CN202211071744.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-09-02
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2042-09-02
AI Technical Summary
The existing artificial stones are costly and prone to bubble holes, affecting strength, and failing to effectively utilize construction waste resources.
Natural ore and waste concrete blocks are used as the main raw materials, and mixed in a specific proportion after crushing and grinding, and plate-like structures with parallel distribution channels are prepared through ultrasonic oscillation, microwave baking and extrusion molding to avoid the formation of bubble holes.
It realizes efficient utilization of resources, improves product strength and cost-effectiveness, reduces the use of raw materials, and enhances the marketing and portability of products.
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of artificial stone, and in particular to an artificial stone material and a preparation method thereof. Background Art
[0002] Artificial stone is a new type of composite material, which is made by mixing resin, filler, pigment, etc. with a small amount of curing agent and undergoing a certain processing procedure. Compared with traditional building materials such as stainless steel and ceramics, artificial stone not only has diverse functions and rich colors, but also has a wider range of applications. Artificial stone products have the advantages of being non-toxic, non-radioactive, flame retardant, non-sticky, non-fouling, antibacterial and mildew-proof, wear-resistant, easy to maintain, etc., and are gradually becoming the new favorite in the decoration building materials market.
[0003] Existing artificial stones are usually solid products, which makes the cost of artificial stones higher. At the same time, it is easy for the strength of artificial stones to be reduced due to quality defects such as bubbles and holes inside the products during the preparation process, thereby affecting the use of the products. This will seriously restrict the promotion and use of artificial stone products.
[0004] In addition, my country produces a large amount of construction waste such as concrete every year. How to better utilize these construction wastes and turn them into treasure is a necessary research topic. At present, there is no literature report on the application of waste concrete in artificial stone products. Summary of the invention
[0005] The purpose of the present invention is to provide an artificial stone and a preparation method thereof, which solves the problems in the prior art that the solid artificial stone has high cost, bubbles and holes are easily present inside the product to reduce strength, and the raw materials used are single.
[0006] In order to achieve the above object, the present invention adopts the following technical solutions:
[0007] In a first aspect, the present invention provides a method for preparing an artificial stone, comprising the following steps:
[0008] (1) crushing and grinding natural ore to obtain ore particles, and crushing and grinding waste concrete blocks to obtain concrete particles;
[0009] (2) mixing ore particles and concrete particles in a weight ratio of 3 to 5:1 to obtain a mixed aggregate;
[0010] (3) The mixed aggregate, resin, hard filler, curing agent and pigment are first subjected to ultrasonic vibration mixing and microwave baking in a certain proportion, and then added to a twin-screw extruder for melt extrusion, and extruded through a mold to prepare a plate-like structure with a plurality of parallel distribution channels inside, and then cooled to 60-80° C. by air cooling, and then cut into a certain length to obtain a semi-finished stone;
[0011] (4) subjecting the obtained semi-finished stone to microwave drying, and then naturally cooling to room temperature for curing for 2 to 3 days;
[0012] (5) The surface is polished and ground to obtain the finished artificial stone product.
[0013] Preferably, in step (1), the natural ore is natural granite mining crushed stone.
[0014] Preferably, in step (1), the particle size of the ore particles is 1 to 2 mm, and the particle size of the concrete particles is 0.5 to 1 mm.
[0015] Preferably, in step (3), the resin is an unsaturated resin.
[0016] Preferably, in step (3), the hard filler is corundum powder or corundum with a particle size of 0.5 to 1 mm.
[0017] Preferably, in step (3), the ratio of the mixed aggregate to the resin, the hard filler, the curing agent and the pigment is 40-48:40-50:7-9:2:1.
[0018] Preferably, in step (3), the ultrasonic oscillation mixing process is: ultrasonic mixing treatment for 60 to 120 minutes under the condition of an ultrasonic power of 150 to 300 W.
[0019] Preferably, in step (3), the microwave baking process is: microwave heating at 80-90° C. for 20-30 min.
[0020] Preferably, in step (4), the microwave drying process is: microwave heating at 50-60° C. for 60-90 min.
[0021] In a second aspect, the present invention provides an artificial stone material prepared by the above-mentioned preparation method. The artificial stone material is in the form of a rectangular plate as a whole, and is provided with a plurality of parallel and spaced channels with circular cross-sections along the length direction.
[0022] Compared with the prior art, the present invention provides an artificial stone and a preparation method thereof, which has the following beneficial effects:
[0023] The present invention adopts natural ore and waste concrete blocks as main raw materials, can make full use of waste stones from ore mining and construction waste, realize waste recycling and improve resource utilization; and by compounding the ground ore particles and concrete particles with hard fillers in a specific ratio, the strength of the product can be greatly improved.
[0024] The artificial stone prepared by extrusion molding in the present invention has a plurality of parallel distributed channels inside, and has good thickness uniformity, thereby avoiding the generation of bubbles and holes due to excessive thickness of the product molding, and can greatly reduce the overall total weight and raw material usage costs without affecting the overall performance, thus laying a foundation for the market promotion and portability of artificial stone. DETAILED DESCRIPTION
[0025] The technical solution of the present invention will be described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0026] The present invention provides an artificial stone and a preparation method thereof. The artificial stone is prepared by the following steps:
[0027] (1) crushing and grinding natural ore to obtain ore particles with a particle size of 1 to 2 mm, and crushing and grinding waste concrete blocks to obtain concrete particles with a particle size of 0.5 to 1 mm; the natural ore is preferably natural granite mining crushed stone.
[0028] (2) The ore particles and the concrete particles are mixed in a weight ratio of 3 to 5:1 to obtain a mixed aggregate.
[0029] (3) The mixed aggregate is first subjected to ultrasonic oscillation mixing and microwave baking at a ratio of 40-48:40-50:7-9:2:1, and then added to a twin-screw extruder for melt extrusion, and extruded through a mold to prepare a plate-like structure with several parallel distribution channels inside, and then cooled to 60-80°C by air cooling, and then cut into a certain length to obtain a semi-finished stone. Among them, the resin is an unsaturated resin; the hard filler is preferably a corundum powder or corundum with a particle size of 0.5-1mm; the curing agent can be a conventional curing agent as long as it can cure the unsaturated resin; the pigment is used to give the product color. The process of ultrasonic oscillation mixing is: ultrasonic mixing treatment for 60-120 minutes under the condition of an ultrasonic power of 150-300W. The process of microwave baking is: microwave heating for 20-30 minutes under the condition of 80-90°C.
[0030] (4) The semi-finished stone is subjected to microwave heating and drying at 50-60° C. for 60-90 min, and then naturally cooled to room temperature for curing for 2-3 days.
[0031] (5) Finally, the surface is polished and ground to obtain the finished artificial stone product.
[0032] The artificial stone provided by the present invention is in the shape of a rectangular plate as a whole, and is provided with a plurality of channels with circular cross sections which are arranged in parallel and spaced apart along the length direction.
[0033] The present invention is further described in detail below through detailed examples.
[0034] Example 1
[0035] This embodiment provides an artificial stone and a preparation method thereof. The artificial stone is prepared by the following steps:
[0036] (1) crushing and grinding natural ore to obtain ore particles with a particle size of 1.5 mm, and crushing and grinding waste concrete blocks to obtain concrete particles with a particle size of 0.8 mm; the natural ore is preferably natural granite mining crushed stone.
[0037] (2) The ore particles and the concrete particles are mixed in a weight ratio of 4:1 to obtain a mixed aggregate.
[0038] (3) The mixed aggregate is first subjected to ultrasonic oscillation mixing and microwave baking at a weight ratio of 45:44:8:2:1, and then added to a twin-screw extruder for melt extrusion. The plate-like structure with multiple parallel distribution channels inside is prepared by extrusion molding through a mold, and then cooled to 60-80°C by air cooling, and then cut into a certain length to obtain a semi-finished stone. Among them, the resin is an unsaturated resin; the hard filler is preferably corundum with a particle size of 0.5-1mm; the curing agent can be a conventional curing agent as long as it can cure the unsaturated resin; the pigment is used to give the product color. Specifically, the process of ultrasonic oscillation mixing is: ultrasonic mixing treatment for 90 minutes under the condition of an ultrasonic power of 200W. The process of microwave baking is: microwave heating for 25 minutes under the condition of 85°C.
[0039] (4) The semi-finished stone is dried by microwave heating at 55° C. for 80 min, and then naturally cooled to room temperature for curing for 2 to 3 days.
[0040] (5) Finally, the surface is polished and ground to obtain the finished artificial stone. The artificial stone is in the form of a rectangular plate, and is provided with six parallel and spaced channels with circular cross-sections along the length direction.
[0041] Example 2
[0042] This embodiment provides an artificial stone and a preparation method thereof. The artificial stone is prepared by the following steps:
[0043] (1) crushing and grinding natural ore to obtain ore particles with a particle size of 1 mm, and crushing and grinding waste concrete blocks to obtain concrete particles with a particle size of 1 mm; the natural ore is preferably natural granite mining crushed stone.
[0044] (2) The ore particles and the concrete particles are mixed in a weight ratio of 3:1 to obtain a mixed aggregate.
[0045] (3) The mixed aggregate is first subjected to ultrasonic oscillation mixing and microwave baking at a weight ratio of 40:50:7:2:1 with resin, hard filler, curing agent and pigment, and then added to a twin-screw extruder for melt extrusion, and then extruded through a mold to prepare a plate-like structure with multiple parallel distribution channels inside, and then cooled to 60-80°C by air cooling, and then cut into a certain length to obtain a semi-finished stone. Among them, the resin is an unsaturated resin; the hard filler is preferably corundum with a particle size of 0.5-1mm; the curing agent can be a conventional curing agent as long as it can cure the unsaturated resin; the pigment is used to give the product color. Specifically, the process of ultrasonic oscillation mixing is: ultrasonic mixing treatment for 120 minutes under the condition of an ultrasonic power of 150W. The process of microwave baking is: microwave heating for 30 minutes under the condition of 80°C.
[0046] (4) The semi-finished stone is subjected to microwave heating and drying at 60° C. for 60 min, and then naturally cooled to room temperature for curing for 2 to 3 days.
[0047] (5) Finally, the surface is polished and ground to obtain the finished artificial stone. The artificial stone is in the form of a rectangular plate, and is provided with six parallel and spaced channels with circular cross-sections along the length direction.
[0048] Example 3
[0049] This embodiment provides an artificial stone and a preparation method thereof. The artificial stone is prepared by the following steps:
[0050] (1) crushing and grinding natural ore to obtain ore particles with a particle size of 2 mm, and crushing and grinding waste concrete blocks to obtain concrete particles with a particle size of 0.5 mm; the natural ore is preferably natural granite mining crushed stone.
[0051] (2) The ore particles and the concrete particles are mixed in a weight ratio of 5:1 to obtain a mixed aggregate.
[0052] (3) The mixed aggregate is first subjected to ultrasonic oscillation mixing and microwave baking at a weight ratio of 48:40:9:2:1, and then added to a twin-screw extruder for melt extrusion. The plate-like structure with multiple parallel distribution channels inside is prepared by extrusion molding through a mold, and then cooled to 60-80°C by air cooling, and then cut into a certain length to obtain a semi-finished stone. Among them, the resin is an unsaturated resin; the hard filler is preferably corundum with a particle size of 0.5-1mm; the curing agent can be a conventional curing agent as long as it can cure the unsaturated resin; the pigment is used to give the product color. Specifically, the process of ultrasonic oscillation mixing is: ultrasonic mixing treatment for 60 minutes under the condition of an ultrasonic power of 300W. The process of microwave baking is: microwave heating for 20 minutes under the condition of 90°C.
[0053] (4) The semi-finished stone is subjected to microwave heating and drying at 50° C. for 90 minutes, and then naturally cooled to room temperature for curing for 2 to 3 days.
[0054] (5) Finally, the surface is polished and ground to obtain the finished artificial stone. The artificial stone is in the form of a rectangular plate, and is provided with six parallel and spaced channels with circular cross-sections along the length direction.
[0055] Example 4
[0056] This embodiment provides an artificial stone and a preparation method thereof. The artificial stone is prepared by the following steps:
[0057] (1) crushing and grinding natural ore to obtain ore particles with a particle size of 1.5 mm, and crushing and grinding waste concrete blocks to obtain concrete particles with a particle size of 0.8 mm; the natural ore is preferably natural granite mining crushed stone.
[0058] (2) The ore particles and the concrete particles are mixed in a weight ratio of 4:1 to obtain a mixed aggregate.
[0059] (3) The mixed aggregate is first subjected to ultrasonic oscillation mixing and microwave baking at a weight ratio of 45:44:8:2:1, and then added to a twin-screw extruder for melt extrusion. The plate-like structure with multiple parallel distribution channels inside is prepared by extrusion molding through a mold, and then cooled to 60-80°C by air cooling, and then cut into a certain length to obtain a semi-finished stone. Among them, the resin is an unsaturated resin; the hard filler is preferably a corundum powder with a particle size of 0.5-1mm; the curing agent can be a conventional curing agent as long as it can cure the unsaturated resin; the pigment is used to give the product color. Specifically, the process of ultrasonic oscillation mixing is: ultrasonic mixing treatment for 90 minutes under the condition of an ultrasonic power of 200W. The process of microwave baking is: microwave heating for 25 minutes under the condition of 85°C.
[0060] (4) The semi-finished stone is dried by microwave heating at 55° C. for 80 min, and then naturally cooled to room temperature for curing for 2 to 3 days.
[0061] (5) Finally, the surface is polished and ground to obtain the finished artificial stone. The artificial stone is in the form of a rectangular plate, and is provided with six parallel and spaced channels with circular cross-sections along the length direction.
[0062] In order to verify the beneficial effects of the present invention, the artificial stones prepared in Examples 1 to 4 and commercially available artificial stones were tested for performance respectively, and the performance testing methods adopted were as follows: flexural strength and compressive strength were tested according to the test method of "Export Artificial Stone Inspection Method" SN / T0308-1993. The performance test results of each embodiment are shown in Table 1 below.
[0063] Table 1 Performance test results of artificial stone
[0064] Flexural strength(MPa) Compressive strength(MPa) Example 1 24.9 184 Example 2 23.7 177 Example 3 23.4 172 Example 4 24.5 181 Commercially available artificial stone 20.1 155
[0065] It can be seen from Table 1 that the strength of the artificial stone prepared by the present invention is significantly improved compared with the conventional artificial stone on the market.
[0066] In addition, the artificial stone prepared by extrusion molding of the present invention has a plurality of parallel distributed channels inside, and has good thickness uniformity, which avoids the generation of bubbles and holes due to excessive thickness of the product molding, and can greatly reduce the overall total weight and raw material usage costs without affecting the overall performance, thus laying a foundation for the market promotion and portability of artificial stone.
[0067] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.
[0068] In addition, it should be understood that although the present specification is described according to embodiments, not every embodiment contains only one independent technical solution. This narrative method of the specification is only for the sake of clarity. Those skilled in the art should regard the specification as a whole. The technical solutions in each embodiment may also be appropriately combined to form other embodiments that can be understood by those skilled in the art.
Claims
1. A method for preparing an artificial stone, characterized in that: The following steps are involved: (1) crushing and grinding natural ore to obtain ore particles with a particle size of 1-2 mm, and crushing and grinding waste concrete blocks to obtain concrete particles with a particle size of 0.5-1 mm; (2) mixing ore particles and concrete particles in a weight ratio of 3 to 5:1 to obtain mixed aggregate; (3) The mixed aggregate is first subjected to ultrasonic vibration mixing and microwave baking in a weight ratio of 40-48:40-50:7-9:2:1 with resin, hard filler, curing agent and pigment, and then added to a twin-screw extruder for melt extrusion, and extruded through a mold to prepare a plate-like structure with a plurality of parallel distribution channels inside, and then cooled to 60-80°C by air cooling, and then cut into a certain length to obtain a semi-finished stone; wherein the hard filler is corundum powder or corundum with a particle size of 0.5-1 mm; (4) The semi-finished stone is dried by microwave, and then naturally cooled to room temperature for curing for 2 to 3 days; (5) Surface polishing and grinding will give the finished artificial stone product.
2. The method for preparing artificial stone according to claim 1, characterized in that: In step (1), the natural ore is natural granite mining crushed stone.
3. The method for preparing artificial stone according to claim 1, characterized in that: In step (3), the resin is an unsaturated resin.
4. The method for preparing artificial stone according to claim 1, characterized in that: In step (3), the ultrasonic mixing process is as follows: ultrasonic mixing treatment is performed for 60 to 120 minutes at an ultrasonic power of 150 to 300 W.
5. The method for preparing artificial stone according to claim 1, characterized in that: In step (3), the microwave baking process is: microwave heating at 80-90° C. for 20-30 minutes.
6. The method for preparing artificial stone according to claim 1, characterized in that: In step (4), the microwave drying process is: microwave heating at 50-60° C. for 60-90 min.
7. An artificial stone prepared by the preparation method according to any one of claims 1 to 6, characterized in that: The artificial stone is in the shape of a rectangular plate as a whole, and is provided with a plurality of parallel and spaced channels with circular cross sections along the length direction.