Ceramic slurries, battery separators and lithium-ion batteries

By using ceramic slurry with specific ceramic particles and binders, the problem of curling lithium-ion battery separators in dry environments is solved, the curling resistance of the separators and the rate performance of the lithium-ion battery are improved, and the rate performance of the lithium-ion battery is avoided. Issues of diaphragm breathability and preparation complexity.

CN115473003BActive Publication Date: 2024-11-22LUCKY FILM CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211198973.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-09-29
Publication Date
2024-11-22
Estimated Expiration
2042-09-29

AI Technical Summary

Technical Problem

The existing lithium-ion battery separators are prone to be curled due to water loss in a dry environment due to ceramic coating, which affects the production efficiency and yield of the battery cell. The improved solution leads to an increase in the permeability of the separator or the preparation process is complicated and operation is difficult.

Method used

Use ceramic slurry with HR value of 1.50-1.90, LBD of 0.55-0.75g/cm3 and TBD of 0.90-1.25g/cm3, combined with an appropriate amount of adhesive and surfactant to prepare ceramic coatings to reduce The drying loss and shrinkage of the ceramic coating reduces the tensile stress on the base film.

Benefits of technology

It effectively reduces the shrinkage caused by drying and water loss of ceramic coating, reduces the curling of the membrane, improves the curling resistance of the membrane and the rate performance of the lithium-ion battery, while maintaining good breathability and preparation ease.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115473003B_ABST
    Figure CN115473003B_ABST
Patent Text Reader

Abstract

The present invention discloses a ceramic slurry, a battery separator and a lithium ion battery. The ceramic slurry comprises ceramic particles and a binder, the HR value of the ceramic particles is 1.50-1.90, wherein HR=TBD / LBD, LBD is the bulk density of the ceramic particles, and the value is 0.55-0.75 g / cm 3 , TBD is the tapped bulk density of ceramic particles, which is 0.90-1.25 g / cm 3 The ceramic coating prepared by the ceramic slurry has a high packing density, small gaps between particles, and low drying water loss, which effectively reduces the shrinkage of the ceramic coating due to drying water loss, thereby reducing the tensile stress of the ceramic coating on the base membrane due to water loss shrinkage, and making the diaphragm curling smaller.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of lithium ion battery separators, and in particular relates to a ceramic slurry, a battery separator and a lithium ion battery. Background Art

[0002] Lithium-ion battery separators have the function of blocking electrons from conducting lithium ions in lithium-ion batteries. Currently, polyolefin microporous membranes are more commonly used. Due to the disadvantages of single polyolefin microporous membranes such as poor thermal stability and poor electrolyte wettability, a ceramic coating needs to be applied on the base membrane. Since the ceramic coating contains hydrophilic groups such as hydroxyl groups, it is easy to absorb or lose water in a humid or dry environment. During the assembly process of lithium-ion batteries, the dry environment will cause the ceramic coating to lose water, and produce tensile stress on the base membrane, causing the separator to curl in the direction of the coating, thereby affecting the efficiency and yield of battery cell production.

[0003] In order to improve the curling resistance of the diaphragm, Kyoritsu Chemical Industry Co., Ltd.'s patent CN105027328B proposes adding an elastic particle to the ceramic coating liquid to reduce the tensile stress on the base film by improving the softness of the coating and alleviating the curling of the ceramic coated lithium-ion battery diaphragm; Shanghai Enjie New Materials Technology Co., Ltd.'s patent CN112563663A proposes adding a core-shell structure adhesive to the ceramic coating slurry to reduce the shrinkage caused by the collapse of the adhesive particles through the protection of the hard shell; Xingyuan Materials CN110571394A proposes reducing the specific surface area of ​​ceramic particles, increasing the molecular weight of CMC, reducing the amount of CMC, and reducing the proportion of hydrophilic monomers in the adhesive to reduce the water content and reduce the curling of the diaphragm. However, the above technical solutions result in increased air permeability of the diaphragm or complex preparation processes and low operability. Summary of the invention

[0004] The present invention aims to solve one of the technical problems in the related art at least to a certain extent. To this end, one object of the present invention is to provide a ceramic slurry, a battery separator and a lithium ion battery. The ceramic coating prepared by the ceramic slurry has a high packing density, small gaps between particles, and low drying water loss, which effectively reduces the shrinkage of the ceramic coating due to drying water loss, thereby reducing the tensile stress of the ceramic coating on the base film due to water loss shrinkage, and making the separator curl less.

[0005] In one aspect of the present invention, the present invention provides a ceramic slurry. According to an embodiment of the present invention, the ceramic slurry comprises: ceramic particles and a binder, wherein the HR value of the ceramic particles is 1.50-1.90, wherein HR=TBD / LBD, and LBD is the bulk density of the ceramic particles, which is 0.55-0.75 g / cm 3 , TBD is the tapped bulk density of the ceramic particles, ranging from 0.90 to 1.25 g / cm 3 .

[0006] The inventors found that if LBD < 0.55 g / cm 3 When LBD>0.75g / cm 3 When the ceramic coating particles are too densely packed, the membrane permeability increases, the lithium ion migration rate decreases, and the rate performance of the lithium ion battery is reduced. At the same time, the tapped bulk density (TBD) value of the above ceramic particles is 0.90-1.25g / cm 3 , HR=TBD / LBD, and the HR value is 1.50-1.90. The inventors found that the smaller the HR value of the ceramic particles, the better the particle fluidity and the better the particle morphology regularity. However, when HR<1.50, the D 50 The particle size is relatively large, the particles are loosely packed, and the ceramic coating is easy to curl; if HR>1.90, the ceramic particles have poor fluidity, irregular particle shape, low sphericity, large specific surface area and high water loss rate. Therefore, the LBD value of this application is 0.55-0.75g / cm 3 , TBD value is 0.90-1.25g / cm 3 The ceramic coating prepared by the ceramic slurry of ceramic particles with HR value of 1.50-1.90 and adhesive has high packing density, small gaps between particles, and low drying water loss, which effectively reduces the shrinkage of the ceramic coating due to drying water loss, thereby reducing the tensile stress of the ceramic coating on the base membrane due to water loss shrinkage, making the diaphragm curling smaller.

[0007] In addition, the ceramic slurry according to the above embodiment of the present invention may also have the following technical features:

[0008] In some embodiments of the present invention, based on 100 parts by weight of the ceramic particles, the binder is 2-10 parts by weight. Thus, the tensile stress of the ceramic coating on the base film due to water loss shrinkage can be reduced, so that the curling of the diaphragm is reduced.

[0009] In some embodiments of the present invention, the specific surface area of ​​the ceramic particles is 4.0-8.0 m 2 / g. As a result, the ceramic particles can have regular morphology, low water loss rate and dense packing.

[0010] In some embodiments of the present invention, the water loss rate of the ceramic particles is not greater than 1500 ppm, thereby reducing the tensile stress of the ceramic coating on the base film due to water loss shrinkage, and reducing the curling of the diaphragm.

[0011] In some embodiments of the present invention, the D of the ceramic particles 50 The diameter of the ceramic coating is 0.42-0.85 μm. This can reduce the tensile stress of the ceramic coating on the base film due to water loss shrinkage, making the diaphragm curling smaller.

[0012] In some embodiments of the present invention, the ceramic particles include at least one of alumina, boehmite, magnesia, and silica.

[0013] In some embodiments of the present invention, the shape of the ceramic particles is spherical or quasi-spherical. Thereby, the tensile stress of the ceramic coating on the base film due to water loss shrinkage can be reduced, and the diaphragm curling is small.

[0014] In some embodiments of the present invention, the elastic modulus of the adhesive film after film formation of the adhesive is 0.05 MPa - 0.50 MPa, and the glass transition temperature of the adhesive film is -45°C < Tg < 0°C. Thereby, the thermal shrinkage performance of the ceramic coating can be improved, and the diaphragm curling is small.

[0015] In some embodiments of the present invention, the adhesive includes a soft monomer and a hard monomer. The soft monomer includes acrylate, and the hard monomer includes at least one of (meth)acrylonitrile, styrene, and (meth)acrylate. The molar ratio of the soft monomer to the hard monomer is 1.2 - 7.3. Thereby, the thermal shrinkage performance of the ceramic coating can be improved, and the diaphragm curling is small.

[0016] In some embodiments of the present invention, the ceramic slurry further includes a dispersant, a surfactant, and water. Thereby, the stability and coatability of the ceramic slurry can be improved.

[0017] In some embodiments of the present invention, based on 100 parts by weight of the ceramic particles, the adhesive is 2 - 10 parts by weight, the dispersant is 0.1 - 0.5 parts by weight, the surfactant is 0.01 - 0.3 parts by weight, and the water is 120 - 220 parts by weight. Thereby, the stability and coatability of the ceramic slurry can be improved, and the diaphragm curling is small.

[0018] In some embodiments of the present invention, the dispersant includes at least one of sodium polyacrylate, lithium polyacrylate, potassium polyacrylate, and ammonium polyacrylate.

[0019] In some embodiments of the present invention, the surfactant includes at least one of silicone surfactants, fluorosilicone surfactants, fluorosilicone-modified surfactants, and silicone-modified surfactants.

[0020] In still another aspect of the present invention, the present invention provides a battery separator. According to an embodiment of the present invention, the battery separator includes: a base film and a ceramic coating, the ceramic coating being formed on at least one surface of the base film, wherein the ceramic coating includes the above-mentioned ceramic slurry. Thereby, the ceramic coating prepared on the base film using the above-mentioned ceramic slurry has a uniform density, can keep the diaphragm surface flat in the dry environment of battery production, and reduce the dry curling in the width direction of the diaphragm.

[0021] In addition, the battery separator according to the above embodiment of the present invention may also have the following technical features:

[0022] In some embodiments of the present invention, the thickness of the ceramic coating on one side is 1.0-5.0 μm, thereby reducing the drying curling of the separator.

[0023] In some embodiments of the present invention, the coating density ρ of the ceramic coating satisfies: 1.5 g / (m 2 *μm)≤ρ≤2.0g / (m 2 *μm). This can reduce the drying curling of the separator.

[0024] In a third aspect of the present invention, the present invention provides a lithium-ion battery. According to an embodiment of the present invention, the lithium-ion battery comprises the battery separator. Thus, wrinkles and folds are not likely to occur during the assembly of the lithium-ion battery, so that the lithium-ion battery has a high assembly yield and efficiency.

[0025] Additional aspects and advantages of the present invention will be given in part in the following description and in part will be obvious from the following description, or will be learned through practice of the present invention. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] The above and / or additional aspects and advantages of the present invention will become apparent and easily understood from the description of the embodiments in conjunction with the following drawings, in which:

[0027] Figure 1 is a scanning electron microscope image of the ceramic coating of Example 1 of the present invention;

[0028] Figure 2 is a scanning electron microscope image of the ceramic coating of Comparative Example 1 of the present invention;

[0029] Figure 3 It is a schematic cross-sectional diagram of a diaphragm curling test according to an embodiment of the present invention. DETAILED DESCRIPTION

[0030] The embodiments of the present invention are described in detail below, which are intended to explain the present invention but should not be construed as limiting the present invention.

[0031] In one aspect of the present invention, the present invention provides a ceramic slurry. According to an embodiment of the present invention, the ceramic slurry includes: ceramic particles and a binder.

[0032] According to an embodiment of the present invention, the HR value of the ceramic particles is 1.50-1.90, wherein HR=TBD / LBD, LBD is the bulk density of the ceramic particles, and the value is 0.55-0.75 g / cm 3 , TBD is the tapped bulk density of ceramic particles, ranging from 0.90 to 1.25 g / cm3 The inventors found that if LBD is less than 0.55 g / cm 3 When LBD is greater than 0.75g / cm, the ceramic coating particles are loosely stacked, making the ceramic coating prone to water loss and drying, resulting in membrane curling. 3 When the ceramic coating particles are too densely packed, the membrane permeability increases, the lithium ion migration rate decreases, and the rate performance of the lithium ion battery is reduced. At the same time, the tapped bulk density (TBD) value of the above ceramic particles is 0.90-1.25g / cm 3 , HR=TBD / LBD, and the HR value is 1.50-1.90. The inventors found that the smaller the HR value of the ceramic particles, the better the particle fluidity and the better the regularity of the particle morphology. However, when the HR is less than 1.50, the D 50 The particle size is relatively large, the particles are loosely packed, and the ceramic coating is easy to curl; if the HR is greater than 1.90, the ceramic particles have poor fluidity, irregular particle shape, low sphericity, large specific surface area and high water loss rate. Therefore, the LBD value of this application is 0.55-0.75g / cm 3 , TBD value is 0.90-1.25g / cm 3 The ceramic coating prepared by the ceramic slurry of ceramic particles with HR value of 1.50-1.90 and adhesive has high packing density, small gaps between particles, and low drying water loss, which effectively reduces the shrinkage of the ceramic coating due to drying water loss, thereby reducing the tensile stress of the ceramic coating on the base membrane due to water loss shrinkage, making the diaphragm curling smaller.

[0033] It should be noted that the tapped bulk density TBD and loose density LBD of the above-mentioned ceramic particles can be achieved by adjusting the particle size and particle size distribution of the ceramic particles, and the tapped bulk density TBD test method is carried out in accordance with GB / T 5162-2021 standard, and the loose density LBD is carried out in accordance with GB / T 1479.1-2011.

[0034] According to an embodiment of the present invention, the specific surface area of ​​the ceramic particles is 4.0-8.0 m 2 / g. The inventors found that if the specific surface area of ​​ceramic particles is greater than 8m 2 / g, the ceramic particles have irregular morphology and high water loss rate; if the specific surface area of ​​the ceramic particles is less than 4m 2 / g, the ceramic particles are too large, resulting in loose particles. Therefore, the surface area of ​​this application is 4.0-8.0m 2 / g of ceramic particles can make the ceramic particles regular in shape, low in water loss rate and compact in stacking.

[0035] According to an embodiment of the present invention, the water loss rate of the ceramic particles is not greater than 1500 ppm. The inventors have found that a lower water loss rate of the ceramic particles can result in less water loss of the ceramic coating when the ceramic slurry is coated on the base film and transferred from the normal temperature environment to the drying room. Thus, by using the ceramic particles with a water loss rate not greater than 1500 ppm in this application, the tensile stress on the base film caused by the water loss shrinkage of the ceramic coating can be reduced, and the diaphragm curling can be minimized. It should be noted that the specific test method for the water loss rate of the above ceramic particles is as follows: Measure the water content ω1 of the ceramic particles in an environment of 25 ± 2 °C and a humidity of 45%, and then measure the water content ω2 of the ceramic particles in a drying room with a water content of 10 - 20 ppm. The water loss rate of the ceramic particles = ω1 - ω2.

[0036] According to an embodiment of the present invention, in order to increase the packing density of the ceramic particles, reduce the tensile stress on the base film caused by the water loss shrinkage of the ceramic coating, and minimize the diaphragm curling, the D of the ceramic particles used in this application 50 is 0.42 - 0.85 μm. Further, the shape of the ceramic particles is spherical or quasi-spherical. Thus, the tensile stress on the base film caused by the water loss shrinkage of the ceramic coating can be reduced, and the diaphragm curling can be minimized. It should be noted that ceramic particles are conventional materials in the art, and those skilled in the art can select the specific type of ceramic particles according to the actual situation. For example, the ceramic particles include, but are not limited to, at least one of alumina, boehmite, magnesium oxide, and silicon dioxide.

[0037] According to an embodiment of the present invention, the elastic modulus of the adhesive film after the adhesive forms a film is 0.05 MPa - 0.50 MPa, and the glass transition temperature of the adhesive film is -45 °C < Tg < 0 °C. The inventors have found that if the elastic modulus of the adhesive film after the adhesive forms a film is greater than 0.50 MPa, the ceramic coating is relatively hard, and the tensile stress generated on the base film during water loss deformation is large, resulting in severe diaphragm curling; if the elastic modulus of the adhesive film after the adhesive forms a film is less than 0.05 MPa, the ceramic coating is relatively soft, and the thermal shrinkage performance is poor. At the same time, when the glass transition temperature of the adhesive film < -45 °C, the content of soft monomers is relatively high, and the heat resistance and mechanical properties of the soft diaphragm are poor; when the glass transition temperature of the adhesive film > 0 °C, the content of hard monomers is relatively high, the ceramic coating is hard, the diaphragm has poor curl resistance and low peel strength. Thus, by using the adhesive with an elastic modulus of 0.05 MPa - 0.50 MPa and a glass transition temperature of -45 °C < Tg < 0 °C after film formation in this application, the thermal shrinkage performance of the ceramic coating can be improved and it has good flexibility, effectively reducing the tensile stress on the base film caused by the water loss shrinkage of the ceramic coating, and minimizing the diaphragm curling.

[0038] It should be noted that the method of forming a film from the adhesive is a conventional method in the art, and those skilled in the art can select according to the actual situation. For example, the adhesive is poured onto a polytetrafluoroethylene plate and then dried to form a film. At the same time, on the premise that the elastic modulus of the adhesive film after film formation is 0.05 - 0.50 MPa and the glass transition temperature of the adhesive film is -45°C < Tg < 0°C, those skilled in the art can select the specific type of the adhesive according to the actual situation. For example, the adhesive used in this application includes a soft monomer and a hard monomer. The soft monomer includes acrylate esters, and the hard monomer includes at least one of (meth)acrylonitrile, styrene, and (meth)acrylate esters, and the molar ratio of the soft monomer to the hard monomer is 1.2 - 7.3. Preferably, the adhesive includes butyl acrylate, isooctyl acrylate, acrylonitrile, styrene, and methyl methacrylate.

[0039] According to an embodiment of the present invention, based on 100 parts by weight of the above-mentioned ceramic particles, the above-mentioned adhesive is 2 - 10 parts by weight. The inventors have found that if the amount of the adhesive is too much, the proportion of the ceramic material in the coating slurry will decrease accordingly, resulting in poor air permeability, heat resistance, and curl resistance of the separator; if the amount of the adhesive is too little, the peel strength of the separator will be low. Therefore, using the ceramic slurry with 2 - 10 parts by weight of the adhesive based on 100 parts by weight of the ceramic particles in this application can make the air permeability, heat resistance, curl resistance, and peel strength of the separator good.

[0040] According to an embodiment of the present invention, in order to improve the stability and coatability of the coating slurry, the ceramic slurry further includes a dispersant, a surfactant, and water. Those skilled in the art can understand that the above-mentioned dispersant and surfactant are both conventional materials in the art, and those skilled in the art can select according to the actual situation. For example, the dispersant includes but is not limited to at least one of sodium polyacrylate, lithium polyacrylate, potassium polyacrylate, and ammonium polyacrylate; the surfactant includes but is not limited to at least one of silicone surfactants, fluorosurfactants, fluorine-modified surfactants, and silicone-modified surfactants; the water is preferably deionized water. Further, based on 100 parts by weight of the ceramic particles, the adhesive is 2 - 10 parts by weight, the dispersant is 0.1 - 0.5 parts by weight, the surfactant is 0.01 - 0.3 parts by weight, and the water is 120 - 220 parts by weight. The inventors have found that when each component is within the above weight range, the slurry has good dispersibility and uniform particles, and the peel strength, heat resistance, and curl resistance of the separator are good, and the coatability during on-line coating is good.

[0041] In another aspect of the present invention, the present invention provides a lithium-ion battery separator. According to an embodiment of the present invention, the battery separator comprises: a base film and a ceramic coating, wherein the ceramic coating is formed on at least one side of the base film, wherein the ceramic coating comprises the above-mentioned ceramic slurry. Thus, the ceramic coating prepared on the base film using the above-mentioned ceramic slurry has a uniform density, can keep the separator surface flat in a dry environment for battery manufacturing, and reduce drying curling in the width direction of the separator.

[0042] It should be noted that the present application mainly solves the problem of drying and curling of unilateral ceramic coating diaphragms. Those skilled in the art can understand that, for ceramic coatings on both sides of the base membrane, if the ceramic coatings on both sides of the base membrane are the same, the tensile stress of the base membrane due to water loss shrinkage of the ceramic coatings on both sides is the same, and the tensile stresses on both sides of the base membrane can offset each other, so the present application mainly solves the problem of drying and curling of unilateral ceramic coating diaphragms. For the specific type of base membrane, the coating method of the ceramic coating and the drying method of the ceramic coating, those skilled in the art can make selections according to actual conditions. For example, the base membrane is a polyolefin microporous membrane, preferably PE and PP materials; a closed scraper coating method is used to form a ceramic coating on the base membrane; the drying method of the ceramic coating includes air drying, vacuum drying and radiation drying, preferably air drying, and the drying temperature is 35°C-65°C. It should be noted that the above-mentioned features and advantages described for the ceramic slurry are also applicable to the battery diaphragm and will not be repeated here.

[0043] In some embodiments of the present invention, the thickness of the single-sided ceramic coating is 1.0-5.0 μm. The inventors have found that if the thickness of the single-sided ceramic coating is less than 1.0 μm, the ceramic coating is too thin, the coating in contact with the base film loses water quickly, the diaphragm curls severely, and the puncture resistance mechanical properties and heat resistance of the diaphragm deteriorate; if the thickness of the single-sided ceramic coating is greater than 5.0 μm, the energy density of the lithium-ion battery is reduced, the distance of lithium ion shuttle increases, the lithium ion conductivity is reduced, and the cost of the diaphragm is increased. Therefore, the use of a ceramic coating with a single-sided thickness of 1.0-5.0 μm in the present application can reduce the drying curling of the diaphragm. Specifically, the thermal shrinkage of the obtained diaphragm after 1 hour at 130°C is less than 3.0%, the air permeability of the diaphragm is 100-280s / 100ml, the dry curling of the diaphragm is less than 7.0%, and the coating density ρ of the ceramic coating satisfies: 1.5g / (m 2 *μm)≤ρ≤2.0g / (m 2 *μm).

[0044] In the third aspect of the present invention, the present invention provides a lithium-ion battery. According to an embodiment of the present invention, the lithium-ion battery includes the above-mentioned battery separator. As a result, wrinkles and folds are not easy to appear during the assembly of the lithium-ion battery, so that the lithium-ion battery has a high assembly yield and efficiency. It should be noted that the other components of the lithium-ion battery except the separator are conventional components in the field, and those skilled in the art can choose according to actual conditions. At the same time, the features and advantages described for the above-mentioned ceramic slurry and lithium-ion battery separator are also applicable to the lithium-ion battery, which will not be repeated here.

[0045] The present invention is described below with reference to specific embodiments. It should be noted that these embodiments are merely illustrative and do not limit the present invention in any way.

[0046] Example 1

[0047] Preparation method of ceramic slurry:

[0048] (1) 100 parts by weight of ceramic particles and 0.3 parts by weight of sodium polyacrylate are stirred and dispersed in 150 parts by weight of deionized water to form a ceramic particle suspension;

[0049] (2) The ceramic particle suspension is ground with a sand mill to prepare a ceramic particle dispersion, and then 5 parts by weight of a binder and 0.05 parts by weight of an organic fluorine-modified polysiloxane are added to the ceramic particle dispersion to prepare a ceramic slurry.

[0050] Diaphragm preparation method:

[0051] A PE polyethylene film (thickness: 12 μm) manufactured by a wet process was used as a substrate, and the ceramic slurry was coated on one side of the substrate by gravure coating to form a ceramic coating, which was then dried at 55° C. for 30 seconds to form a diaphragm with a ceramic coating.

[0052] The specific parameters of ceramic slurry are as follows:

[0053] The ceramic particles are alumina powder (LBD = 0.62 g / cm 3 , HR=1.64,D 50 =0.68μm, water loss rate 1100ppm, specific surface area SA = 6.5m 2 / g); the soft monomers of the adhesive are butyl acrylate and isooctyl acrylate, the hard monomers are acrylonitrile monomer and methyl methacrylate monomer, and the molar ratio of the soft and hard monomers is 7.3, the elastic modulus of the adhesive film after film formation is 0.05MPa, Tg=-45℃; the thickness of the ceramic coating formed on the diaphragm is 4μm on one side. The tap density TBD test method is carried out in accordance with GB / T5162-2021 standard, and the bulk density LBD test method is carried out in accordance with GB / T 1479.1-2011 standard.

[0054] Ceramic coating thickness test: Use a Mahr thickness gauge to directly test the thickness of the manufactured diaphragm product at multiple points and take the average value.

[0055] Example 2

[0056] The preparation method of the ceramic slurry and the preparation method of the diaphragm in Example 2 are the same as those in Example 1.

[0057] The specific parameters of ceramic slurry are as follows:

[0058] The ceramic particles are alumina powder (LBD = 0.62 g / cm 3 , HR=1.64,D 50 =0.68μm, water loss rate 1100ppm, specific surface area SA = 6.5m 2 / g); the soft monomers of the adhesive are butyl acrylate and isooctyl acrylate, the hard monomers are methyl methacrylate monomer and styrene monomer, and the molar ratio of the soft and hard monomers is 4.1. The elastic modulus of the adhesive film after film formation is 0.35MPa, Tg=-21°C; the thickness of the ceramic coating is 4μm.

[0059] The testing methods for tap density TBD, bulk density LBD and ceramic coating thickness are the same as those in Example 1.

[0060] Example 3

[0061] The preparation method of the ceramic slurry and the preparation method of the diaphragm in Example 3 are the same as those in Example 1.

[0062] The ceramic particles are alumina powder (LBD = 0.62 g / cm 3 , HR=1.64,D 50 =0.68μm, water loss rate 1100ppm, specific surface area SA = 6.5m 2 / g); the soft monomers of the adhesive are butyl acrylate and isooctyl acrylate, the hard monomers are acrylonitrile monomer and styrene monomer, and the molar ratio of the soft and hard monomers is 1.2. The elastic modulus of the adhesive film after film formation is 0.50MPa, Tg = -1.8°C; the thickness of the ceramic coating is 4μm.

[0063] The testing methods for tap density TBD, bulk density LBD and ceramic coating thickness are the same as those in Example 1.

[0064] Example 4

[0065] The preparation method of the ceramic slurry and the preparation method of the diaphragm in Example 4 are the same as those in Example 1.

[0066] The ceramic particles are alumina powder (LBD = 0.55 g / cm 3, HR = 1.64, D50 = 0.85 μm, water loss rate 980 ppm, specific surface area SA = 4.5 m 2 / g); the soft monomers of the adhesive are butyl acrylate and isooctyl acrylate, the hard monomers are acrylonitrile monomer and styrene monomer, and the molar ratio of the soft and hard monomers is 1.2. The elastic modulus of the adhesive film after film formation is 0.50MPa, Tg = -1.8°C; the thickness of the ceramic coating is 4μm.

[0067] The testing methods for tap density TBD, bulk density LBD and ceramic coating thickness are the same as those in Example 1.

[0068] Example 5

[0069] The preparation method of the ceramic slurry and the preparation method of the diaphragm in Example 5 are the same as those in Example 1.

[0070] The ceramic particles are alumina powder (LBD = 0.75 g / cm 3 , HR = 1.66, D50 = 0.42 μm, water loss rate 1300 ppm, specific surface area SA = 7.5 m 2 / g); the soft monomers of the adhesive are butyl acrylate and isooctyl acrylate, the hard monomers are acrylonitrile monomer and styrene monomer, and the molar ratio of the soft and hard monomers is 1.2. The elastic modulus of the adhesive film after film formation is 0.50MPa, Tg = -1.8°C; the thickness of the ceramic coating is 4μm.

[0071] The testing methods for tap density TBD, bulk density LBD and ceramic coating thickness are the same as those in Example 1.

[0072] Example 6

[0073] The preparation method of the ceramic slurry and the preparation method of the diaphragm in Example 6 are the same as those in Example 1.

[0074] The ceramic particles are boehmite particles (LBD = 0.55 g / cm 3 , HR = 1.85, D50 = 0.50 μm, water loss rate 1500 ppm, specific surface area SA = 7.9 m 2 / g); the soft monomers of the adhesive are butyl acrylate and isooctyl acrylate, the hard monomers are acrylonitrile monomer and styrene monomer, and the molar ratio of the soft and hard monomers is 1.2. The elastic modulus of the adhesive film after film formation is 0.50MPa, Tg = -1.8°C; the thickness of the ceramic coating is 4μm.

[0075] The testing methods for tap density TBD, bulk density LBD and ceramic coating thickness are the same as those in Example 1.

[0076] Example 7

[0077] Except that the thickness of the ceramic coating is 2 μm, other parameters and methods are the same as those in Example 5.

[0078] Example 8

[0079] Except that the amount of the binder is 8 parts by weight, other parameters and methods are the same as those in Example 1.

[0080] Example 9

[0081] Except that the amount of the binder is 10 parts by weight, other parameters and methods are the same as those in Example 1.

[0082] Example 10

[0083] Except that the amount of the binder is 2 parts by weight, other parameters and methods are the same as those in Example 1.

[0084] Comparative Example 1

[0085] The preparation method of the ceramic slurry and the preparation method of the diaphragm in Comparative Example 1 are the same as those in Example 1.

[0086] The ceramic particles are alumina powder (LBD = 0.53 g / cm 3 , HR=1.50,D 50 =0.88μm, water loss rate 780ppm, specific surface area SA = 4.2m 2 / g); the soft monomer of the adhesive is isooctyl acrylate, the hard monomer is styrene monomer, and the molar ratio of the soft and hard monomers is 7.5. The elastic modulus of the adhesive film after film formation is 0.03MPa, Tg = -48°C; the thickness of the ceramic coating is 4μm.

[0087] The testing methods for tap density TBD, bulk density LBD and ceramic coating thickness are the same as those in Example 1.

[0088] Comparative Example 2

[0089] The preparation method of the ceramic slurry and the preparation method of the diaphragm in Comparative Example 2 are the same as those in Example 1.

[0090] The ceramic particles are alumina powder (LBD = 0.79 g / cm 3 , HR=1.81,D 50 =0.40μm, water loss rate 2100ppm, specific surface area SA = 8.3m 2 / g); the soft monomer of the adhesive is butyl acrylate, the hard monomer is acrylonitrile monomer, and the molar ratio of the soft and hard monomers is 1.0. The elastic modulus of the adhesive film after film formation is 0.85MPa, Tg=3.0℃; the thickness of the ceramic coating is 4μm.

[0091] The testing methods for tap density TBD, bulk density LBD and ceramic coating thickness are the same as those in Example 1.

[0092] The ceramic coatings of Example 1 and Comparative Example 1 were subjected to electron microscope scanning.

[0093] The scanning electron microscope image of the ceramic coating of Example 1 is as follows Figure 1 As shown, the scanning electron microscope image of the ceramic coating of Comparative Example 1 is as follows Figure 2 As shown, from Figure 1 and Figure 2 It can be seen that the coated ceramic particles of Example 1 are small and more densely packed, and have better curling resistance. The performance of the diaphragms obtained in Examples 1-10 and Comparative Examples 1-2 was tested, and the specific test method is as follows:

[0094] (1) Air permeability test

[0095] Test according to the Gurley method in GB / T 458-2008 “Determination of air permeability of paper and paperboard” and record the time required for 100 ml of air to pass through.

[0096] (2) Heat shrinkage test

[0097] First, cut a 120mm×120mm ceramic diaphragm of regular shape, and measure the length L of the diaphragm in the horizontal and vertical directions of the diaphragm with a steel ruler or projector with an accuracy of at least 0.1mm. TD0 , L MD0 (generally about 10mm), put the sample into two A4 papers, and then put them into a 130℃ oven for 1h. Take them out immediately after baking and leave them for half an hour. Measure the horizontal and vertical lengths of the diaphragm and record the data L TD , L MD . Then use formulas ① and ② to calculate the transverse and longitudinal thermal shrinkage:

[0098] η TD =(L TD0 -L TD ) / L TD0 ×100%①

[0099] η MD =(L MD0 -L MD ) / L MD0 ×100%②

[0100] Among them, η TD is the transverse thermal shrinkage of the diaphragm after baking, η MD The diaphragm shrinks longitudinally after baking.

[0101] (3) Dry curl test

[0102] In order to make the curling difference more obvious, the test was carried out in a drying room with a moisture content of 10-20ppm. First, a square ceramic diaphragm with a horizontal length of 200mm and a vertical length of 200mm was cut, and the diaphragm was flattened under the action of external force, and the horizontal length L of the diaphragm was tested. TD1 Then remove the external force and test the length L of the projection of the two longitudinal edges of the curled diaphragm on the table. TD2 The test diagram is as follows: Figure 3 As shown, the curl degree of the diaphragm in the transverse direction is calculated using formula ③:

[0103] Curl = (L TD1 -L TD2 ) / L TD1 *100%③

[0104] (4) Coating density ρ test: Cut 100mm*100mm PE base film and the diaphragm coated with ceramic slurry and weigh the mass m0 and m1 respectively. Test the base film and diaphragm thickness h0 and h1, ρ = (m1-m0) / [(h1-h0)*(0.1*0.1)]

[0105] The test results of the diaphragm performance of Examples 1-10 and Comparative Examples 1-2 are shown in Table 1.

[0106] Table 1

[0107]

[0108]

[0109] It can be seen from the data in Table 1 that, from Example 1 to Example 3, as the elastic modulus of the film increases, the dry curl of the diaphragm also gradually increases. Comparison of the results of Example 3 and Example 5 shows that as the packing density of the ceramic particles gradually increases, the thermal shrinkage decreases, and the dry curl of the diaphragm decreases. Comparison of the results of Example 6 with Example 4 shows that as the HR value of the ceramic particles increases and the specific surface area increases, the dry curl of the diaphragm increases. Comparison of the results of Example 7 with Example 5 shows that as the thickness of the ceramic coating decreases, the ceramic coating loses water faster, so the dry curl of the diaphragm increases. It can be seen from the results of Example 1 with Examples 8-10 that as the amount of adhesive increases, the air permeability of the diaphragm increases, the thermal shrinkage becomes larger, and the curl does not change much within the appropriate range of the adhesive. Comparison of the results of Example 5 with Comparative Example 1 shows that when the packing density of the ceramic particles is too small, the stacking is too loose, and the flexibility of the adhesive film is too high, the dry curl and thermal shrinkage of the diaphragm are very large. From the comparison of the results of Example 1 and Comparative Example 2, it can be seen that when the ceramic particle packing density is too large, the packing is too dense, and the rigidity of the adhesive film is too large, the air permeability and dry curl of the diaphragm are very large. The above data show that the HR value and LBD value of the ceramic particles and the elastic modulus value of the adhesive film after film formation have a great influence on the properties of the diaphragm, especially the curl of the diaphragm. Therefore, the use of the ceramic slurry of the present application to prepare the diaphragm can significantly reduce the dry curl of the diaphragm.

[0110] In the description of this specification, the description with reference to the terms "one embodiment", "some embodiments", "example", "specific example", or "some examples" etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representations of the above terms do not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described may be combined in any one or more embodiments or examples in a suitable manner. In addition, those skilled in the art may combine and combine the different embodiments or examples described in this specification and the features of the different embodiments or examples, without contradiction.

[0111] Although the embodiments of the present invention have been shown and described above, it is to be understood that the above embodiments are exemplary and are not to be construed as limitations of the present invention. A person skilled in the art may change, modify, replace and vary the above embodiments within the scope of the present invention.

Claims

1. A ceramic slurry, It is characterized in that include: Ceramic particles and a binder, wherein the HR value of the ceramic particles is 1.50-1.90, wherein HR=TBD / LBD, LBD is the bulk density of the ceramic particles, and the value is 0.55-0.75 g / cm 3 , TBD is the tapped bulk density of the ceramic particles, ranging from 0.90 to 1.25 g / cm 3 , the elastic modulus of the adhesive film after film formation is 0.05MPa-0.50MPa; Based on 100 parts by weight of the ceramic particles, the binder is 2-10 parts by weight; The specific surface area of ​​the ceramic particles is 4.0-8.0 m2 / g; The water loss rate of the ceramic particles is no more than 1500 ppm; The D50 of the ceramic particles is 0.42-0.85 μm; The ceramic particles include at least one of alumina, boehmite, magnesium oxide and silicon dioxide; The ceramic particles are spherical or quasi-spherical in shape; The adhesive comprises a soft monomer and a hard monomer, wherein the soft monomer comprises acrylates, and the hard monomer comprises at least one of (meth)acrylonitrile, styrene, and (meth)acrylates, and the molar ratio of the soft monomer to the hard monomer is 1.2-7.

3.

2. The ceramic slurry according to claim 1, It is characterized in that The glass transition temperature of the film is -45℃ <Tg<0℃。 3. The ceramic slurry according to claim 1, It is characterized in that Also included are dispersants, surfactants and water.

4. The ceramic slurry according to claim 3, It is characterized in that Based on 100 parts by weight of the ceramic particles, The binder is 2-10 parts by weight, the dispersant is 0.1-0.5 parts by weight, the surfactant is 0.01-0.3 parts by weight and the water is 120-220 parts by weight; The dispersant includes at least one of sodium polyacrylate, lithium polyacrylate, potassium polyacrylate and ammonium polyacrylate; The surfactant includes at least one of an organic silicon surfactant, an organic fluorine surfactant, an organic fluorine-modified surfactant, and an organic silicon-modified surfactant.

5. A battery separator, It is characterized in that include: A base film and a ceramic coating, wherein the ceramic coating is formed on at least one surface of the base film, wherein the ceramic coating comprises the ceramic slurry according to any one of claims 1-4.

6. The battery separator according to claim 5, It is characterized in that The thickness of the ceramic coating on one side is 1.0-5.0 μm; The coating density ρ of the ceramic coating satisfies: 1.5g / (m 2 *μm)≤ρ≤2.0g / (m 2 *μm); The base film is a polyolefin microporous film.

7. A lithium ion battery, It is characterized in that The battery separator comprises the battery separator according to claim 5 or 6.