A method for assessing hydrogen embrittlement risk of high-strength steel
Through thermal desorption and electrochemical hydrogen charging methods, the hydrogen concentration and hydrogen permeability rate of high-strength steel are measured, which solves the problem of inability to monitor hydrogen infiltration and escape in the prior art, and provides accurate evaluation of the risk of hydrogen embrittlement of high-strength steel and composition design guide.
Patent Information
- Application Number
- CN202110598125.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-05-31
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2041-05-31
AI Technical Summary
The prior art is difficult to monitor and evaluate the infiltration and escape rate of hydrogen in high-strength steel in real time, and it is impossible to accurately evaluate the risk of hydrogen embrittlement, which affects the production and use of materials.
The thermal desorption and electrochemical hydrogen charging methods are used to calculate the reversible hydrogen trap density by measuring the saturated hydrogen concentration, hydrogen permeation rate and hydrogen eluting rate, and provide a risk assessment of hydrogen embrittlement in high-strength steel.
Accurately obtain the concentration and number of traps in high-strength steel, guide the design and use environment selection of components, and reduce the risk of hydrogen embrittlement.
Smart Images

Figure QLYQS_1 
Figure BDA0003091946880000041 
Figure BDA0003091946880000063
Abstract
Description
Technical Field
[0001] The invention relates to the field of metal material analysis, and in particular to a method for assessing the risk of hydrogen embrittlement of high-strength steel. Background Art
[0002] Diffusible hydrogen is the core factor causing hydrogen embrittlement in high-strength steel. Hydrogen is inevitably introduced into high-strength steel during the production stages such as smelting, pickling, electroplating, welding, and subsequent processing and use by users. Hydrogen exists in steel in two states, one is in the form of non-diffusible hydrogen, and the other is in the form of diffusible hydrogen. Among them, diffusible hydrogen can diffuse in steel and accumulate in defects, grain boundaries, etc. The interaction between diffusible hydrogen and stress is the main cause of hydrogen embrittlement and delayed fracture in ultra-high-strength steel. It can be seen that the source of hydrogen in high-strength steel is very wide, and the introduction of hydrogen can be said to run through the entire life cycle of high-strength steel, and The content of diffusible hydrogen in high-strength steel is not constant during the production process and the user's processing and use, and the risk of hydrogen embrittlement also exists in the whole process; the diffusible hydrogen in the high-strength steel matrix is mainly distributed in the hydrogen traps of the matrix. Different high-strength steels have different numbers of hydrogen traps due to different structures, which ultimately leads to different diffusible hydrogen contents, and ultimately manifests in different risks of hydrogen embrittlement; therefore, obtaining the content of diffusible hydrogen in high-strength steel is of great practical significance for evaluating the risk of hydrogen embrittlement of high-strength steel. Accurately obtaining the hydrogen content in high-strength steel is an important prerequisite for studying the risk of hydrogen embrittlement of high-strength steel. At present, the analytical measurement methods of hydrogen concentration in high-strength steel are mainly divided into the following types:
[0003] 1) Infrared absorption thermal conductivity method: Infrared absorption thermal conductivity method is currently the most widely used method for determining the hydrogen content of steel materials. This method uses a pulse electrode to quickly dissolve the steel material in a graphite crucible. During the measurement, the hydrogen element is converted into hydrogen gas, and then the thermal conductivity method is used to determine the hydrogen content under the condition of argon as the carrier gas. The contents of the three elements of hydrogen are calculated separately;
[0004] 2) Mass spectrometry: Mass spectrometry is a hot research direction in the industry. This method is different from other determination methods. Mass spectrometry is to first melt the steel material at high temperature and then determine the hydrogen content of the liquid steel material.
[0005] 3) Thermal analysis spectrometer: The release rate of hydrogen at a given temperature is measured using a quadrupole mass spectrometer, and the concentration of hydrogen released at different temperatures can be obtained after integration;
[0006] 4) Thermal desorption method: This method uses the relative thermal conductivity of the measured gas to determine the hydrogen content in the gas. Based on this physical property, the concentration of the measured gas can be known by simply detecting the thermal conductivity of the measured gas. Nitrogen is used as the protective gas. When using it, the test sample is heated to a certain temperature to release the diffused hydrogen, and the hydrogen concentration is calculated using the change in thermal conductivity.
[0007] 5) Hydrogen permeation method: using a double electrolytic cell experimental device, there are different electrolytic cells on both sides of the sample, a certain positive potential is applied to the anode, and the anode surface of the sample needs to be plated with Ni or Pt in advance. Under the action of the anode potential, the hydrogen released from the sample is oxidized to form an anode current curve, and the total amount of hydrogen released can be obtained by integrating the curve;
[0008] 6) Oil-discharge method: add a valve to the top of the graduated burette, partially melt the bottom to form a wide flat mouth for placing the sample; fill the glass tube with silicone oil that is higher than the valve, cover it with a flat glass, put a flat container filled with silicone oil downward, and close the valve. Wipe the surface of the sample dry and place it on a flat glass, cover it with a glass tube, and hydrogen will diffuse out from the inside of the sample and reconstitute into hydrogen gas, moving upward along the glass tube, while discharging the silicone oil, creating a space composed of hydrogen below the valve, the volume of which is the total amount of hydrogen in the sample.
[0009] The current hydrogen measurement methods mainly obtain the amount of diffusible hydrogen in high-strength steel, but cannot obtain the number of hydrogen traps in the high-strength steel structure. High-strength steel goes through multiple processes from production, processing, use to service, and faces a variety of environments. Each process and environment has an impact on the entry and escape of hydrogen in high-strength steel, and different high-strength steels are affected differently. In actual practice, real-time monitoring is impossible.
[0010] In view of this, it is urgent to develop a new high-strength steel hydrogen embrittlement risk assessment method that can judge the hydrogen embrittlement risk of high-strength steel by the hydrogen penetration and escape rates, thereby guiding users to reasonably select materials and store them according to the use environment. Summary of the invention
[0011] In view of the defects existing in the prior art, the purpose of the present invention is to provide a method for assessing the hydrogen embrittlement risk of high-strength steel. By thermal desorption of hydrogen and electrochemical hydrogen charging, the saturated hydrogen concentration of high-strength steel is accurately obtained, providing an important basis for the hydrogen embrittlement risk assessment and composition design of high-strength steel; then, through diffusion hydrogen desorption test, the hydrogen permeation rate and hydrogen escape rate are calculated to provide guidance for the hydrogen embrittlement risk in the future production and storage process of high-strength steel; finally, the reversible hydrogen trap density of high-strength steel is further derived. This indicator has a strong correlation with the organization and composition of high-strength steel, and can be used to guide the improvement of the composition organization design of high-strength steel, providing theoretical support for the research and development of high-strength steel.
[0012] In order to achieve the above object, the present invention adopts the following technical solution:
[0013] The present invention provides a method for assessing hydrogen embrittlement risk of high-strength steel, comprising the following steps:
[0014] (1) preparing a sample of high-strength steel and removing free hydrogen in the sample by heating;
[0015] (2) Removal of hydrogen by thermal desorption: using thermal desorption to remove diffusible hydrogen in the sample;
[0016] (3) Electrochemical hydrogenation: The sample after the dehydrogenation treatment is charged with hydrogen for 0.5-10 hours by electrochemical method;
[0017] (4) Determining the saturated hydrogen concentration: measuring the hydrogen concentration of the sample one by one according to the hydrogen filling time, determining the saturated hydrogen concentration of the sample at each hydrogen filling time by comparison, and recording the hydrogen filling time at which the saturated hydrogen concentration is reached;
[0018] (5) The hydrogen permeation rate, hydrogen escape rate and reversible hydrogen trap density of the sample are calculated according to the saturated hydrogen concentration of the sample to evaluate the hydrogen embrittlement risk of the high-strength steel.
[0019] Preferably, in the step (1), after the high-strength steel is made into a sample, it is subjected to surface treatment by ultrasonic treatment with acetone; and / or
[0020] During the heating process, a heating furnace is used to heat the sample; and / or
[0021] During the heating process, the heating temperature is 150-170° C. and the heating time is 0.5-2 h; and / or
[0022] After the heat treatment, the free hydrogen concentration in the sample is reduced to 0.02 ppm or less.
[0023] Preferably, in step (2), during the thermal desorption process for removing hydrogen, the sample is heated to 400° C. and maintained for 20-60 min; and / or
[0024] During the thermal desorption process of removing hydrogen, a hydrogen analyzer is used to measure the content of diffusible hydrogen.
[0025] Preferably, in step (3), during the electrochemical hydrogen charging process, the hydrogen charging solution is 0.5 mol / L H2SO4 + 0.3 g / L thiourea solution, and the hydrogen charging current is 10 mA / cm 2 of constant current.
[0026] Preferably, in the step (4), during the process of determining the saturated hydrogen concentration, the comparative determination method is: comparing the difference between the hydrogen concentrations of samples with different hydrogen charging time, and when the difference is less than 0.1 ppm, the hydrogen concentration is the saturated hydrogen concentration of the sample.
[0027] Preferably, in step (5), the hydrogen permeation rate of the sample is obtained by the following formula:
[0028] V 渗 =C H饱和 / T 充氢 ;
[0029] Where V 渗is the hydrogen permeation rate of the sample, in ppm / min;
[0030] C H饱和 is the saturated hydrogen concentration of the sample, in ppm;
[0031] T 充氢 It is the hydrogen charging time for the sample to reach saturated hydrogen concentration, in minutes.
[0032] Preferably, in step (5), the hydrogen escape rate of the sample is obtained by the steps of:
[0033] preparing a hydrogen-filled saturated sample according to the saturated hydrogen concentration of the sample;
[0034] The hydrogen-saturated sample was placed in an environment with a temperature of 20-25°C and a humidity of 60-90%, and was placed for 4-72 hours for different lengths of hydrogen release treatment. The hydrogen concentration was then measured until the hydrogen concentration dropped below 0.1 ppm. The different hydrogen release times and corresponding hydrogen concentrations were recorded, and the hydrogen escape rate of the sample was calculated.
[0035] Preferably, in step (5), the reversible hydrogen trap density of the sample is obtained by the following formula:
[0036]
[0037] In the formula, ρ H陷阱 is the reversible hydrogen trap density of the sample, in / cm 3 ;
[0038] P 钢 is the density of high-strength steel, in g / cm 3 ;
[0039] C H饱和 is the saturated hydrogen concentration of the sample, in ppm;
[0040] m H is the molar mass of hydrogen in g / mol;
[0041] N A is Avogadro's constant, 6.02×10 23 .
[0042] The high-strength steel hydrogen embrittlement risk assessment method of the present invention can accurately obtain the saturated hydrogen concentration in the high-strength steel, and use it to characterize the number of reversible hydrogen traps in the high-strength steel, and clarify the influence of different organizations on the hydrogen embrittlement traps and hydrogen concentration of the high-strength steel in combination with the microstructure of the high-strength steel, and theoretically study the relationship between the microstructure of the high-strength steel and hydrogen embrittlement, providing effective support for the research and development of high-strength steel. At the same time, the hydrogen permeation rate and hydrogen escape rate are calculated based on the saturated hydrogen concentration, and different high-strength steels are compared to analyze their hydrogen embrittlement sensitivity, which is used to guide users to make reasonable material selection and warehousing, and also provide suggestions for hydrogen embrittlement of high-strength steel at the production site;
[0043] The high-strength steel hydrogen embrittlement risk assessment method of the present invention has the following beneficial effects:
[0044] 1. The high-strength steel hydrogen embrittlement risk assessment method of the present invention accurately obtains the saturated hydrogen concentration of high-strength steel through thermal desorption and electrochemical hydrogen charging, providing an important basis for the hydrogen embrittlement risk assessment between high-strength steels;
[0045] 2. The high-strength steel hydrogen embrittlement risk assessment method of the present invention calculates the hydrogen permeation rate and hydrogen escape rate through thermal desorption hydrogen removal, electrochemical hydrogen charging and diffusion hydrogen release tests, and provides guidance for the hydrogen embrittlement risk in the future production and storage process of high-strength steel;
[0046] 3. The high-strength steel hydrogen embrittlement risk assessment method of the present invention further derives the reversible hydrogen trap density of high-strength steel. This index has a strong correlation with the structure and composition of high-strength steel, and can be used to guide the improvement of the composition and structure design of high-strength steel, providing theoretical support for the research and development of high-strength steel. DETAILED DESCRIPTION
[0047] The present invention will be described in detail below in conjunction with specific embodiments. The following embodiments will help those skilled in the art to further understand the present invention, but are not intended to limit the present invention in any form.
[0048] The method for assessing hydrogen embrittlement risk of high-strength steel provided by the present invention comprises the following steps:
[0049] (1) preparing a sample of high-strength steel and removing free hydrogen in the sample by heating;
[0050] The specific process is as follows: the high-strength steel is sheared into 100mm*20mm specimens, 10 of each sample are prepared, and then the specimens are degreased by acetone ultrasound to ensure that the surface is clean and free of impurities; the high-strength steel is then heated in a heating furnace to remove free hydrogen in the specimens, the heating temperature is controlled at 150-170℃, and the heating time is 0.5-2h, and finally the concentration of free hydrogen in the specimens is reduced to below 0.02ppm;
[0051] (2) Removal of hydrogen by thermal desorption: using thermal desorption to remove diffusible hydrogen in the sample;
[0052] The specific process is: using thermal desorption method to heat the sample to 400°C, maintaining it for 20-60 minutes to remove the diffuse hydrogen in the sample, and using a hydrogen analyzer to obtain the diffuse hydrogen concentration of the sample during the dehydrogenation process. In a specific embodiment, a German Bruker hydrogen analyzer can be used.
[0053] (3) Electrochemical hydrogenation: The sample after the dehydrogenation treatment is charged with hydrogen for 0.5-10 hours by electrochemical method;
[0054] The specific process is as follows: first, prepare the hydrogen charging solution: prepare 0.5mol / L H2SO4+0.3g / L thiourea solution as the hydrogen charging solution, and store it at room temperature for 24h; then use the electrochemical constant current mode with a hydrogen charging current of 10mA / cm 2 , placing the sample in a hydrogen charging solution and performing hydrogen charging for different time periods of 0.5-10h, wherein the hydrogen charging time can be 0.5h / 1h / 2h / 6h / 10h; then placing the hydrogenated sample in liquid nitrogen for storage;
[0055] (4) Determining the saturated hydrogen concentration: measuring the hydrogen concentration of the sample one by one according to the hydrogen charging time, determining the saturated hydrogen concentration of the sample by comparison, and recording the hydrogen charging time to reach the saturated hydrogen concentration;
[0056] The specific process is: measure the hydrogen (hydrogen concentration) of the hydrogen-filled samples one by one according to the hydrogen filling time, compare the difference between the hydrogen concentrations of the samples under different hydrogen filling times, and when the difference is less than 0.1ppm, the hydrogen concentration is the saturated hydrogen concentration of the sample, and record the hydrogen filling time to reach the saturated hydrogen concentration;
[0057] (5) The hydrogen permeation rate, hydrogen escape rate and reversible hydrogen trap density of the sample are calculated based on the saturated hydrogen concentration of the sample to evaluate the hydrogen embrittlement risk of high-strength steel.
[0058] The specific process is:
[0059] (5.1) Calculation of hydrogen permeation rate: Calculated by the saturated hydrogen concentration of the sample and the hydrogen charging time to reach the saturated hydrogen concentration. The formula is as follows:
[0060] V 渗 =C H饱和 / T 充氢 ;
[0061] Where V 渗 is the hydrogen permeation rate of the sample, in ppm / min;
[0062] C H饱和 is the saturated hydrogen concentration of the sample, in ppm;
[0063] T 充氢 It is the hydrogen charging time for the sample to reach saturated hydrogen concentration, in minutes.
[0064] (5.2) Calculation of hydrogen escape velocity:
[0065] Five hydrogen-filled saturated samples were prepared according to the saturated hydrogen concentration of the samples;
[0066] The hydrogen-saturated samples were placed in an environment with a temperature of 20-25°C and a humidity of 60-90%, and placed for 4-72 hours for different lengths of hydrogen release treatment (for example, the placement time was 4h / 12h / 24h / 48h / 72h), and then the hydrogen concentration was measured until the hydrogen concentration dropped below 0.1ppm. The different hydrogen release times and corresponding hydrogen concentrations were recorded, and the hydrogen escape rate of the sample was calculated based on the difference in hydrogen concentration and the corresponding hydrogen release time.
[0067] (5.3) Calculation of reversible hydrogen trap density: When the hydrogen concentration reaches saturation, it is considered that the reversible hydrogen traps are fully occupied. The saturated hydrogen concentration C H饱和 , high strength steel density ρ 钢 And the chemical properties of hydrogen are used for calculation. The specific calculation method is as follows:
[0068] Saturated hydrogen concentration: Among them C H饱和 In step (4), m 钢 is the quality of high-strength steel, m H is the mass of hydrogen;
[0069] High strength steel density: Where m 钢 is the sample mass, V 钢 is the sample volume, ρ 钢 It is the density of high-strength steel, which is generally 7.85g / cm 3 ;
[0070] Reversible hydrogen trap density:
[0071]
[0072] In the formula, ρ H陷阱 is the reversible hydrogen trap density of the sample, in / cm 3 ;
[0073] ρ 钢 is the density of high-strength steel, in g / cm 3 , generally 7.85g / cm 3
[0074] C H饱和 is the saturated hydrogen concentration of the sample, in ppm;
[0075] M H is the molar mass of hydrogen in g / mol;
[0076] N A is Avogadro's constant, which is 6.02×10 23 ;
[0077] The high-strength steel hydrogen embrittlement risk assessment method of the present invention is further described below with reference to specific examples;
[0078] Example 1
[0079] In this embodiment, DP1180 cold-rolled finished plate is selected from the production site as the test object, and the specific hydrogen embrittlement risk assessment method is:
[0080] (1) The DP1180 cold-rolled finished plate was sheared into 100 mm*20 mm samples, and 10 samples were prepared for standby use. The samples were then degreased using acetone ultrasound to ensure that the surface was clean and free of impurities. The high-strength steel was then heated in a heating furnace to remove free hydrogen in the samples. The heating temperature was controlled to be 170°C and the heating time was 1 h. Finally, the concentration of free hydrogen in the samples was reduced to below 0.02 ppm.
[0081] (2) Hydrogen removal by thermal desorption: The sample was heated to 400 °C and kept for 30 min to remove the diffusible hydrogen in the sample. During the dehydrogenation process, the diffusible hydrogen concentration of the sample was obtained using a hydrogen analyzer from Bruker, Germany.
[0082] (3) Electrochemical hydrogenation: 1 L of 0.5 mol / L H2SO4 + 0.3 g / L thiourea solution was prepared as the hydrogenation solution and stored at room temperature for 24 h. Then, the electrochemical constant current mode was used with a hydrogenation current of 10 mA / cm 2 , placing the sample in a hydrogen charging solution and performing hydrogen charging for different lengths of time, wherein the hydrogen charging time is 1h / 2h / 6h / 10h; then placing the hydrogenated sample in liquid nitrogen for storage;
[0083] (4) Determine the saturated hydrogen concentration: measure the hydrogen (hydrogen concentration) of the hydrogen-filled samples one by one according to the hydrogen filling time, until the difference between the hydrogen concentrations of the samples is less than 0.1 ppm. The hydrogen concentration at this time is the saturated hydrogen concentration of the sample, and the hydrogen filling time to reach the saturated hydrogen concentration is recorded at the same time;
[0084] (5) The hydrogen permeation rate, hydrogen escape rate and reversible hydrogen trap density of the sample were calculated according to the saturated hydrogen concentration of the sample (see Table 1 for the results) to evaluate the hydrogen embrittlement risk of high-strength steel.
[0085] (5.1) Hydrogen permeation rate V 渗 =C H饱和 / T 充氢 ;
[0086] (5.2) Calculation of hydrogen escape velocity:
[0087] Prepare 5 hydrogen-filled saturated samples according to the saturated hydrogen concentration of the samples; place the hydrogen-filled saturated samples in an environment with a temperature of 20-25°C and a humidity of 60-90% for 4h / 12h / 24h / 48h / 72h, respectively, and then measure the hydrogen concentrations until the hydrogen concentration drops below 0.1ppm, record different hydrogen release times and corresponding hydrogen concentrations, and calculate the hydrogen escape rate of the samples according to the difference in hydrogen concentration and the corresponding hydrogen release time;
[0088] (5.3) Reversible hydrogen trap density
[0089] Example 2
[0090] In this example, QP1180 cold-rolled finished plate is selected as the test object, and the specific hydrogen embrittlement risk assessment method is as follows:
[0091] (1) The QP1180 cold-rolled finished plate was sheared into 100 mm*20 mm samples, and 10 samples were prepared for standby use. The samples were then degreased using acetone ultrasound to ensure that the surface was clean and free of impurities. The high-strength steel was then heated in a heating furnace to remove free hydrogen in the samples. The heating temperature was controlled to be 170°C and the heating time was 1.5 h. Finally, the concentration of free hydrogen in the samples was reduced to below 0.02 ppm.
[0092] (2) Hydrogen removal by thermal desorption: The sample was heated to 400 °C and kept for 30 min to remove the diffusible hydrogen in the sample. During the dehydrogenation process, the diffusible hydrogen concentration of the sample was obtained using a hydrogen analyzer from Bruker, Germany.
[0093] (3) Electrochemical hydrogenation: 1 L of 0.5 mol / L H2SO4 + 0.3 g / L thiourea solution was prepared as the hydrogenation solution and stored at room temperature for 24 h. Then, the electrochemical constant current mode was used with a hydrogenation current of 10 mA / cm 2 , placing the sample in a hydrogen charging solution and performing hydrogen charging for different lengths of time, wherein the hydrogen charging time is 1h / 2h / 6h; then placing the hydrogenated sample in liquid nitrogen for storage;
[0094] (4) Determine the saturated hydrogen concentration: measure the hydrogen (hydrogen concentration) of the hydrogen-filled samples one by one according to the hydrogen filling time, until the difference between the hydrogen concentrations of the samples is less than 0.1 ppm. The hydrogen concentration at this time is the saturated hydrogen concentration of the sample, and the hydrogen filling time to reach the saturated hydrogen concentration is recorded at the same time;
[0095] (5) The hydrogen permeation rate, hydrogen escape rate and reversible hydrogen trap density of the sample were calculated according to the saturated hydrogen concentration of the sample (see Table 1 for the results) to evaluate the hydrogen embrittlement risk of high-strength steel.
[0096] Among them, the hydrogen escape rate is calculated as follows: 5 hydrogen-saturated samples are prepared according to the saturated hydrogen concentration of the sample; the hydrogen-saturated samples are placed in an environment with a temperature of 20-25°C and a humidity of 60-90% for 4h / 12h / 24h / 48h / 72h respectively, and then the hydrogen concentration is measured respectively until the hydrogen concentration drops below 0.1ppm, and the different hydrogen release times and corresponding hydrogen concentrations are recorded, and the hydrogen escape rate of the sample is calculated according to the difference in hydrogen concentration and the corresponding hydrogen release time.
[0097] Example 3
[0098] In this embodiment, MS1180 cold-rolled finished plate is selected as the test object, and the specific hydrogen embrittlement risk assessment method is as follows:
[0099] (1) The MS1180 cold-rolled finished plate was sheared into 100 mm*20 mm specimens, and 10 specimens were prepared for standby use. The specimens were then degreased using acetone ultrasound to ensure that the surface was clean and free of impurities. The high-strength steel was then heated in a heating furnace to remove free hydrogen in the specimens. The heating temperature was controlled to be 170°C and the heating time was 2 h. Finally, the concentration of free hydrogen in the specimens was reduced to below 0.02 ppm.
[0100] (2) Hydrogen removal by thermal desorption: The sample was heated to 400 °C and kept for 30 min to remove the diffusible hydrogen in the sample. During the dehydrogenation process, the diffusible hydrogen concentration of the sample was obtained using a hydrogen analyzer from Bruker, Germany.
[0101] (3) Electrochemical hydrogenation: 1 L of 0.5 mol / L H2SO4 + 0.3 g / L thiourea solution was prepared as the hydrogenation solution and stored at room temperature for 24 h. Then, the electrochemical constant current mode was used with a hydrogenation current of 10 mA / cm 2 , placing the sample in a hydrogen charging solution and performing hydrogen charging for different lengths of time, wherein the hydrogen charging time is 0.5h / 1h / 2h / 6h / 8h; then placing the hydrogenated sample in liquid nitrogen for storage;
[0102] (4) Determine the saturated hydrogen concentration: measure the hydrogen (hydrogen concentration) of the hydrogen-filled samples one by one according to the hydrogen filling time, until the difference between the hydrogen concentrations of the samples is less than 0.1 ppm. The hydrogen concentration at this time is the saturated hydrogen concentration of the sample, and the hydrogen filling time to reach the saturated hydrogen concentration is recorded at the same time;
[0103] (5) The hydrogen permeation rate, hydrogen escape rate and reversible hydrogen trap density of the sample were calculated according to the saturated hydrogen concentration of the sample (see Table 1 for the results) to evaluate the hydrogen embrittlement risk of high-strength steel.
[0104] Among them, calculation of hydrogen escape rate: prepare 5 hydrogen-saturated samples according to the saturated hydrogen concentration of the samples; place the hydrogen-saturated samples in an environment with a temperature of 20-25°C and a humidity of 60-90% for 4h / 12h / 24h / 48h / 72h respectively, and then measure the hydrogen concentration respectively until the hydrogen concentration drops below 0.1ppm, record different hydrogen release times and corresponding hydrogen concentrations, and calculate the hydrogen escape rate of the samples according to the difference in hydrogen concentration and the corresponding hydrogen release time;
[0105] Table 1 Hydrogen embrittlement risk assessment indicators
[0106]
[0107]
[0108] It can be seen from Table 1 that the hydrogen escape rate and reversible hydrogen trap density of steel grades DP1180 and QP1180 are relatively large, and the hydrogen permeation rate is relatively slow. It can be seen that steel grades DP1180 and QP1180 are relatively less affected by the environment, and the risk of hydrogen embrittlement is relatively small, and they are not sensitive to the environment; while the hydrogen escape rate and reversible hydrogen trap density of steel grade MS1180 are relatively small, and the hydrogen permeation rate is relatively fast. It can be seen that steel grade MS1180 is relatively greatly affected by the external environment, and the risk of hydrogen embrittlement is relatively large. During storage and processing, special attention should be paid to keeping the environment dry to avoid cracking caused by hydrogen permeation.
[0109] In summary, the high-strength steel hydrogen embrittlement risk assessment method of the present invention accurately obtains the saturated hydrogen concentration of high-strength steel through thermal desorption hydrogen removal and electrochemical hydrogen charging, providing an important basis for the hydrogen embrittlement risk assessment between high-strength steels; the high-strength steel hydrogen embrittlement risk assessment method calculates the hydrogen permeation rate and hydrogen escape rate through thermal desorption hydrogen removal, electrochemical hydrogen charging and diffusion hydrogen release tests, providing guidance for the hydrogen embrittlement risk in the future production and storage process of high-strength steel; the high-strength steel hydrogen embrittlement risk assessment method further derives the reversible hydrogen trap density of high-strength steel, which has a strong correlation with the organization and composition of high-strength steel, and can be used to guide the improvement of the composition organization design of high-strength steel, providing theoretical support for the research and development of high-strength steel.
[0110] In summary, the above embodiments are only used to illustrate the technical solutions of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solutions of the present invention can be modified or replaced by equivalents without departing from the purpose and scope of the technical solutions of the present invention, which should be included in the scope of the claims of the present invention.
Claims
1. A method for assessing hydrogen embrittlement risk of high-strength steel, characterized in that: The following steps are involved: (1) forming a sample of high-strength steel and removing free hydrogen in the sample by heating; (2) Removal of hydrogen by thermal desorption: The diffusible hydrogen in the sample is removed by thermal desorption; (3) Electrochemical hydrogenation: The sample after the dehydrogenation treatment is charged with hydrogen by electrochemical method for 0.5-10 hours; (4) Determining the saturated hydrogen concentration: measuring the hydrogen concentration of the sample one by one according to the hydrogen filling time, determining the saturated hydrogen concentration of the sample at each hydrogen filling time by comparison, and recording the hydrogen filling time at which the saturated hydrogen concentration is reached; In the process of determining the saturated hydrogen concentration, the comparison determination method is: comparing the difference between the hydrogen concentrations of the samples with different hydrogen charging time, and when the difference is less than 0.1ppm, the hydrogen concentration is the saturated hydrogen concentration of the sample; (5) calculating the hydrogen permeation rate, hydrogen escape rate and reversible hydrogen trap density of the sample according to the saturated hydrogen concentration of the sample to evaluate the hydrogen embrittlement risk of the high-strength steel, The hydrogen permeation rate of the sample is obtained by the following formula: V 渗 =C H饱和 / T 充氢 ; Where V 渗 is the hydrogen permeation rate of the sample, in ppm / min; C H饱和 is the saturated hydrogen concentration of the sample, in ppm; T 充氢 It is the hydrogen charging time for the sample to reach saturated hydrogen concentration, in min; The hydrogen escape rate of the sample is obtained by the following steps: preparing a hydrogen-filled saturated sample according to the saturated hydrogen concentration of the sample; The hydrogen-saturated sample is placed in an environment with a temperature of 20-25° C. and a humidity of 60-90%, and is placed for 4-72 hours for different lengths of hydrogen release treatment, and then the hydrogen concentration is measured until the hydrogen concentration drops below 0.1 ppm, and the different hydrogen release times and the corresponding hydrogen concentrations are recorded, and the hydrogen escape rate of the sample is calculated according to the hydrogen concentration difference and the corresponding hydrogen release time; The reversible hydrogen trap density of the sample is obtained by the following formula: ; In the formula, ρ H陷阱 is the reversible hydrogen trap density of the sample, in / cm 3 ; P 钢 is the density of high-strength steel, in g / cm 3 ; C H饱和 is the saturated hydrogen concentration of the sample, in ppm; m H is the molar mass of hydrogen in g / mol; N A is Avogadro's constant, 6.02╳10 23 .
2. The high-strength steel hydrogen embrittlement risk assessment method according to claim 1, characterized in that: In the step (1), after the high-strength steel is made into a sample, the surface is treated by ultrasonic treatment with acetone; and / or During the heating process, a heating furnace is used to heat the sample; and / or During the heating process, the heating temperature is 150-170° C. and the heating time is 0.5-2 h; and / or After the heat treatment, the free hydrogen concentration in the sample is reduced to 0.02 ppm or less.
3. The high-strength steel hydrogen embrittlement risk assessment method according to claim 1, characterized in that: In the step (2), during the thermal desorption process for removing hydrogen, the sample is heated to 400° C. and maintained for 20-60 min; and / or During the thermal desorption process of removing hydrogen, a hydrogen analyzer is used to measure the content of diffusible hydrogen.
4. The high-strength steel hydrogen embrittlement risk assessment method according to claim 1, characterized in that: In the step (3), during the electrochemical hydrogen charging process, the hydrogen charging solution is 0.5 mol / L H2SO4+0.3 g / L thiourea solution, and the hydrogen charging current is 10 mA / cm 2 of constant current.