A preparation method of graded magnetic porous carbonized wood composite phase change material
By preparing a graded magnetic porous carbonized wood composite phase change material, the problems of low thermal energy storage efficiency and insufficient multi-energy response capacity of phase change materials in the prior art are solved, and efficient thermal energy conversion and stability improvement of multiple energy sources are achieved.
Patent Information
- Application Number
- CN202211161968.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-09-23
- Publication Date
- 2024-11-01
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing phase change materials have problems of leakage, low thermal conductivity and low energy conversion capabilities in thermal energy storage, which limits their practical application and is difficult to convert thermal energy in response to multiple energy sources at the same time.
The preparation method of graded magnetic porous carbonized wood composite phase change material is adopted. By delectin treatment on the wood block, immersing it in ferric nitrate solution and carbonizing it, combining stearic acid to form magnetic carbonized wood, and decorating Fe3O4 magnetic nanoparticles to improve thermal conductivity and Magnetic, realizes multi-energy driven composite PCM.
It realizes the thermal energy conversion of various energy sources for solar energy, electrical energy and magnetic energy, with good morphological stability, excellent thermal performance, cycle stability and high latent heat, meeting various application needs.
Smart Images

Figure CN115505375B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a method for preparing a phase change material, in particular to a method for preparing a graded magnetic porous carbonized wood composite phase change material. Background Art
[0002] The shortage of non-renewable energy and the increasing impact of greenhouse gas emissions on the environment have hindered the healthy development of society and the satisfaction of people's needs. Developing renewable energy sources, such as solar energy, electrical energy, and magnetic energy, is one of the most promising options to solve these problems. Thermal energy storage (TES) has become one of the most effective ways to utilize existing energy. Phase change materials (PCMs) have attracted attention in thermal energy storage due to their excellent thermal stability and high energy storage density. However, disadvantages such as leakage during phase change, low thermal conductivity, and low energy conversion capacity limit their practical applications. Considering the above disadvantages of PCMs, combining PCMs with functional supporting matrices that can respond to different energy sources and convert them into thermal energy is a method to improve the thermal energy conversion efficiency as well as improve shape stability and thermal conductivity. Therefore, it is necessary to combine environmentally friendly natural materials with functional nanomaterials to prepare multi-energy-driven composite phase change materials in order to improve the performance and application of phase change materials. Summary of the invention
[0003] The technical problem to be solved by the present invention is to provide a method for preparing a graded magnetic porous carbonized wood composite phase change material, which can simultaneously respond to multiple energy sources such as solar energy, electrical energy and magnetic energy for thermal energy conversion, and has good morphological stability, excellent thermal performance, excellent cycle stability and high latent heat.
[0004] The technical solution adopted by the present invention to solve the above technical problems is to provide a method for preparing a graded magnetic porous carbonized wood composite phase change material, comprising the following steps: S1) delignifying a wood block; S2) immersing the treated wood block in an iron nitrate solution to obtain iron nitrate / delignification, and then carbonizing to obtain a magnetic carbonized wood; S3) immersing the magnetic carbonized wood in molten stearic acid to obtain a magnetic porous carbonized wood composite phase change material.
[0005] Further, the step S1 comprises: S11) first, immersing the wood block in a solution containing NaOH and Na2SO3 and boiling it to remove most of the lignin, and then repeatedly immersing the wood block in clear boiling water to remove NaOH and Na2SO3; S12) secondly, placing the wood block in a H2O2 solution and boiling it until it turns white to further remove the lignin; S13) finally, obtaining the wood block from which the lignin is removed and storing it in deionized water for later use.
[0006] Furthermore, the wood block in step S1 is a poplar wood block, and the poplar wood block has a length of 30 mm, a width of 20 mm, and a thickness of 5 mm.
[0007] Furthermore, in step S1, the concentration of NaOH solution is 2.5 mol / L, the concentration of Na2SO3 solution is 0.4 mol / L, the concentration of H2O2 solution is 2.5 mol / L, and the boiling time is 3 h.
[0008] Further, the step S2 comprises: S21) first dissolving Fe(NO3)3∙9H2O in deionized water and stirring; S22) then immersing the wood blocks from which the lignin has been removed into the solution until they turn brown; S23) then, taking the wood blocks out of the solution and placing them in a freeze dryer for freeze drying to obtain iron nitrate / delignification; S24) finally, carbonizing the iron nitrate / delignification to obtain magnetic carbonized wood.
[0009] Furthermore, the weight ratio of Fe(NO3)3∙9H2O and stearic acid is 1-3:2.
[0010] Furthermore, in step S2, the amount of Fe(NO3)3∙9H2O used is 1-3 g, the amount of deionized water used is 25 mL, the stirring time is 1 hour, and the freeze-drying time is 12 hours.
[0011] Furthermore, the carbonization process in step S2 is as follows: first, in a nitrogen atmosphere, the temperature is increased to 300° C. at a rate of 2.0° C. / min and maintained for 1 hour, and then the temperature is increased to 500° C. at a rate of 5.0° C. / min and maintained for 1 hour.
[0012] Furthermore, the step S3 comprises: completely melting stearic acid; immersing the magnetic carbonized wood in the melted stearic acid under vacuum conditions; and removing residual liquid on the surface of the composite material using filter paper.
[0013] Furthermore, in step S3, the melting point of stearic acid is 80°C, and the vacuuming time is 2 hours.
[0014] Compared with the prior art, the present invention has the following beneficial effects: the preparation method of the graded magnetic porous carbonized wood composite phase change material provided by the present invention prepares a multi-energy driven composite PCM by decorating Fe3O4 magnetic nanoparticles as the main matrix on the de-woodened wood block and using stearic acid as the thermal energy guest. The specific advantages are as follows:
[0015] 1) The SA / MCW composite material of the present invention can simultaneously respond to multiple energy sources, including solar energy, electrical energy and magnetic energy, to perform thermal energy conversion.
[0016] 2) SA / MCW composites have good morphological stability, excellent thermal properties, excellent cycling stability, high latent heat, and high thermal / electrical conductivity of pure PCM.
[0017] 3) The multi-energy SA / MCW composite phase change material of the present invention can meet the thermal energy storage requirements in various applications.
[0018] 4) The raw materials used in the present invention are cheap and readily available, and the preparation and use processes are simple. BRIEF DESCRIPTION OF THE DRAWINGS
[0019] Figure 1 A schematic diagram of the solar thermal conversion curve of SA / MCW-4 prepared in an embodiment of the present invention when simulated exposed to different solar radiation intensities;
[0020] Figure 2 It is a schematic diagram of the electrothermal conversion curve of SA / MCW-4 prepared in an embodiment of the present invention after applying different potentials;
[0021] Figure 3 In the figure, a is the hysteresis loop of SA / MCWs composite materials with different Fe3O4 concentrations, b shows a schematic diagram of the magnetothermal conversion process in an alternating magnetic field, c is a schematic diagram of the temperature-time curve of the SA / MCW-4 sample of the present invention in the process of absorbing heat energy, and d is a schematic diagram of the temperature-time curve of the SA / MCW-4 sample of the present invention in the process of releasing heat energy. DETAILED DESCRIPTION
[0022] The present invention will be further described below in conjunction with the accompanying drawings and embodiments.
[0023] The method for preparing the graded magnetic porous carbonized wood composite phase change material provided by the present invention comprises the following steps:
[0024] S1) Delignification of poplar wood blocks; poplar wood has high absorption capacity and good mechanical properties after lignin removal and carbonization, which is beneficial for maintaining thermal storage capacity; while other woods, such as balsa and basswood, show relatively poor performance. Removal of lignin can expand the porosity and eliminate the barriers related to mass and energy transfer in wood through highly oriented cellulose microfibrils and nanofibers with high absorption capacity. Therefore, it is advantageous to use delignified wood blocks (DW) as support materials for shape-stable composite phase change materials. Compared with natural wood, these support materials have lower density, larger surface area and higher porosity, paralleling other routes based on cellulose cryogels and aerogels.
[0025] S2) The treated poplar wood block is immersed in an iron nitrate solution to obtain iron nitrate / delignification, and then carbonized to obtain magnetic carbonized wood; due to the excellent magnetic properties of Fe(NO3)3∙9H2O, its introduction not only further improves the thermal conductivity, but also achieves excellent microwave absorption performance by achieving a balance between impedance matching and high loss characteristics. Compared with the results of some related reports on wood-based magnetic material PCM composite systems, the magnetic properties and energy conversion efficiency of the composite material of the present invention are very outstanding. The present invention combines Fe(NO3)3∙9H2O with wood and PCM as an example, and the resulting composite material has ultra-high thermal energy capacity, enhanced thermal conductivity, excellent microwave absorption performance, and efficient sunlight and magnetothermal conversion performance.
[0026] S3) Immersing the magnetic carbonized wood in molten stearic acid to obtain a magnetic porous carbonized wood composite phase change material.
[0027] The present invention prepares multi-energy driven composite PCM by decorating Fe3O4 magnetic nanoparticles on delignified wood as the main matrix and stearic acid as the thermal energy guest. Magnetic carbonized wood (MCW) can improve the thermal conductivity and electrical conductivity of the obtained SA / MCW composite PCM, which is beneficial to reduce the time of heat storage and release process. At the same time, the introduction of Fe3O4 nanoparticles gives the composite PCM magnetic properties. More importantly, the prepared SA / MCW composite PCM can capture energy from solar energy, electrical energy and magnetic energy, so they can be effectively used for solar-thermal energy, electrical-thermal energy and magnetic-thermal energy conversion at the same time. In addition, the multi-energy driven phase change materials have good morphological stability, high latent heat, excellent thermal properties and excellent cycle stability.
[0028] Preferably, the weight ratio of Fe(NO3)3∙9H2O to stearic acid is 1-3:2; increasing the amount of SA to more than 2 parts may cause leakage of the prepared composite material, while reducing the amount of SA may reduce the performance of PCM and Fe3O4 particles in the composite material. Example
[0029] First, the poplar wood blocks were immersed in a solution containing NaOH (2.5 mol / L) and Na2SO3 (0.4 mol / L) and boiled for 12 h to remove most of the lignin. The wood blocks were then repeatedly immersed in clear boiling water to remove NaOH and Na2SO3. Second, to further remove lignin, the wood blocks were boiled in H2O2 solution (2.5 mol / L) for about 3 h until they turned white. The treated wood was then taken out and washed with deionized water. Finally, the delignified wood chips were obtained and stored in deionized water for later use.
[0030] MCW is through Fe 3+@DW was prepared by carbonization of Fe3O4 nanoparticles and in situ formation. Fe(NO3)3∙9H2O was first dissolved in 25 mL of deionized water and stirred for 1 h. The delignified wood samples were then immersed in the solution until they turned brown. Afterwards, the samples were taken out of the solution and placed in a freeze dryer for 12 h for freeze drying to obtain ferric nitrate / delignified (Fe 3+ @DW). Finally, Fe 3+ @DW was heated to 300 °C at a rate of 2.0 °C / min and kept for 1 h in a nitrogen atmosphere, and then heated to 500 °C at a rate of 5.0 °C / min and kept for 1 h to obtain magnetic carbonized wood (MCW).
[0031] The SA / MCW composite PCM was prepared by vacuum impregnation process. Initially, stearic acid (SA) was completely melted at 80 °C. Then, MCW was immersed in the molten SA under vacuum for 2 h. The MCW / PCM composite was finally obtained after the liquid SA remaining on the surface of MCW was removed by filter paper. The obtained composite sample was called SA / MCW-n, corresponding to different MCW samples from MCW-1 to MCW-4. Accordingly, the SA / MCW composite PCM prepared under different concentrations of Fe(NO3)3∙9H2O was named MCW-n. The samples prepared in the present invention were named SA / MCW-1, SA / MCW-2, SA / MCW-3 and SA / MCW-4, and all samples had the same DW and SA contents, but different Fe(NO3)3∙9H2O concentrations. The amount of SA corresponding to the SA / MCW-1, SA / MCW-2, SA / MCW-3 and SA / MCW-4 prepared by the present invention is 2g, and the amount of Fe(NO3)3·9H2O is 1g, 1.5g, 2g and 3g respectively. Increasing the amount of Fe(NO3)3·9H2O to more than 3g may reduce the performance of the PCM in the composite material, while reducing the amount of Fe(NO3)3·9H2O to less than 1g may cause leakage of the prepared composite material. Compared with other samples, SA / MCW3 exhibits better energy storage magnetic properties.
[0032] The SA / MCW-4 samples of the present invention were subjected to various energy fields, including solar radiation, electric field, and magnetic field, to verify their responsiveness to multiple energy sources. The solar thermal conversion behavior of SA / MCW-4 was studied by exposing the samples to simulated solar radiation (AM 1.5) with intensities of 1 sun (curve ①), 1.5 sun (curve ②), and 2 sun (curve ③). Figure 1As shown. Thermocouples are used to record the temperature changes inside the sample and transmit the data to the display in real time. The temperature of SA / MCW-4 rises rapidly under simulated solar radiation, and the heating rate increases with the increase of SA / MCW-4 radiation intensity, as shown in curve ①. As the radiation time increases, the inflection point of the SA / MCW-4 temperature curve appears between 71.1 ℃ and 80.3 ℃. This shows that the phase change of SA / MCW-4 occurs in response to solar radiation, and the absorbed light energy is converted into heat energy and then stored in the PCM. After turning off the incident light, the temperature of SA / MCW-4 drops rapidly, and a freezing platform appears between 70.2 ℃ and 63.6 ℃, indicating that SA / MCW-4 releases a large amount of heat energy through freezing.
[0033] Due to their excellent electrical conductivity, the present invention can directly apply an electric potential on the SA / MCWs composite material to trigger the electrothermal conversion performance. The SA / MCW-4 sample was subjected to an electric field of different voltages, and the sample temperature was recorded and displayed in Figure 2 At input voltages of 1.3, 1.9, and 2.5 V, the temperature of SA / MCW-4 can reach around 86 °C, 92 °C, and 100 °C, respectively, showing an effective electrical response. The inflection point occurs between 71 °C and 72 °C, which corresponds to the phase transition temperature of SA / MCW-4. When the applied voltage is removed, the sample temperature drops rapidly due to the high thermal conductivity, and other inflection points during the cooling process appear. These findings suggest that the electric potential can produce a phase transition in the SA / MCW composite and release the thermal energy stored during the cooling process.
[0034] The magnetic properties of SA / MCWs composites with different concentrations of Fe3O4 were tested under magnetic field at room temperature. The corresponding hysteresis loops are shown in Figure 2. Figure 3 As shown in (a). It can be seen that all SA / MCWs composites exhibit typical superparamagnetism. The saturation magnetization (Ms) of SA / MCW-1, SA / MCW-2, SA / MCW-3 and SA / MCW-4 are 0.54, 2.69, 6.36 and 14.68 emu g-1, respectively. This indicates that a higher Fe3O4 particle concentration in the composites leads to excellent magnetic properties. Figure 3Figure b shows a schematic diagram of the magnetothermal conversion process in an alternating magnetic field. The magnetothermal effect is related to the sample concentration and the alternating magnetic field. During this process, the SA / MCW-4 sample was placed in a 5 mL induction coil and exposed to an alternating magnetic field (1.36 MHz and 550 A m-1), and a fiber optic thermometer was used to record the temperature change of the sample. The obtained sample temperature-time curves are shown in Figure 3c and d. The temperature of SA / MCW-4 rose rapidly to 71 °C and then slowly increased between 94 s and 103 s, as shown in Figure 3c and d. Figure 3 As shown in Figure c, it shows that the phase change process absorbs some heat energy. After that, once the temperature reaches about 74 °C, the heating rate of the composite material increases until it reaches 125 °C. The temperature curve of the SA / MCW-4 sample immediately drops to the phase change range after the alternating magnetic field is terminated, and heat energy is released, as shown in Figure 4. Figure 3 These findings indicate that the SA / MCW-4 composite has good magnetothermal conversion and storage capabilities when exposed to an alternating magnetic field, which expands the application range of composite PCMs.
[0035] Although the present invention has been disclosed as above with preferred embodiments, it is not intended to limit the present invention. Any person skilled in the art may make some modifications and improvements without departing from the spirit and scope of the present invention. Therefore, the scope of protection of the present invention shall be based on the definition of the claims.
Claims
1. A method for preparing a graded magnetic porous carbonized wood composite phase change material, characterized in that: The steps include: S1) Delignification treatment of wood blocks; S2) immersing the treated wood block in an iron nitrate solution to obtain iron nitrate / delignification, and then carbonizing to obtain magnetic carbonized wood; S3) immersing the magnetic carbonized wood in molten stearic acid to obtain a magnetic porous carbonized wood composite phase change material; The step S1 comprises: S11) First, the wood block is immersed in a solution containing NaOH and Na2SO3 and boiled to remove most of the lignin, and then the wood block is repeatedly immersed in clear boiling water to remove NaOH and Na2SO3; S12) Secondly, the wood pieces are boiled in H2O2 solution until they turn white to further remove lignin; S13) Finally, the lignin-free wood blocks were obtained and stored in deionized water for later use; The carbonization process in step S2 is as follows: first, in a nitrogen atmosphere, the temperature is raised to 300° C. at a rate of 2.0° C. / min and maintained for 1 hour, and then the temperature is raised to 500° C. at a rate of 5.0° C. / min and maintained for 1 hour.
2. The method for preparing the graded magnetic porous carbonized wood composite phase change material according to claim 1, characterized in that: The wood block in step S1 is a poplar wood block, and the length of the poplar wood block is 30 mm, the width is 20 mm, and the thickness is 5 mm.
3. The method for preparing the graded magnetic porous carbonized wood composite phase change material according to claim 1, characterized in that: In step S1, the concentration of NaOH solution is 2.5 mol / L, the concentration of Na2SO3 solution is 0.4 mol / L, the concentration of H2O2 solution is 2.5 mol / L, and the boiling time is 3 h.
4. The method for preparing the graded magnetic porous carbonized wood composite phase change material according to claim 1, characterized in that: The step S2 comprises: S21) First, Fe(NO3)3·9H2O was dissolved in deionized water and stirred; S22) The delignined wood pieces are then immersed in the solution until they turn brown; S23) Next, the wood block is taken out from the solution and placed in a freeze dryer for freeze drying to obtain iron nitrate / delignification; S24) Finally, the iron nitrate / delignification is carbonized to obtain magnetic carbonized wood.
5. The method for preparing the graded magnetic porous carbonized wood composite phase change material according to claim 4, characterized in that: The weight ratio of the Fe(NO3)3·9H2O to stearic acid is 1-3:
2.
6. The method for preparing the graded magnetic porous carbonized wood composite phase change material according to claim 5, characterized in that: In step S2, the amount of Fe(NO3)3·9H2O used is 1-3 g, the amount of deionized water used is 25 mL, the stirring time is 1 hour, and the freeze-drying time is 12 hours.
7. The method for preparing the graded magnetic porous carbonized wood composite phase change material according to claim 1, characterized in that: The step S3 comprises: completely melting stearic acid; immersing the magnetic carbonized wood in the melted stearic acid under vacuum conditions; and removing residual liquid on the surface of the composite material with filter paper to obtain the composite material.
8. The method for preparing the graded magnetic porous carbonized wood composite phase change material according to claim 7, characterized in that; In step S3, the melting point of stearic acid is 80° C., and the vacuuming time is 2 hours.