A method for preparing a MEMS probe for wafer-level testing

By using molten material to fill molds and micro-nano processing technology in the preparation of MEMS probes, the problems of low efficiency and crosstalk noise in the existing technology are solved, and the preparation of probes with high precision and strong anti-interference ability is achieved, which is suitable for high-frequency testing. .

CN115508594BActive Publication Date: 2024-11-15XI AN JIAOTONG UNIV +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211213693.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-09-30
Publication Date
2024-11-15
Estimated Expiration
2042-09-30

AI Technical Summary

Technical Problem

The existing MEMS probe preparation methods for wafer-level testing are inefficient, and the crosstalk noise between probes during high-frequency testing leads to a decrease in signal integrity, especially the radial size of non-linear-shaped probes increases significantly.

Method used

The insulating isolation layer and shielding metal layer are prepared by directly filling the molten probe material into the mold prepared by MEMS technology, and the insulating isolation layer and shielding metal layer are prepared by combining magnetron sputtering and micro-nano processing technology. The accuracy and anti-interference ability of the probe are improved through micro-nano processing.

Benefits of technology

It realizes high efficiency and high accuracy probe preparation, reduces the increase in the radial size of the probe, enhances the anti-interference ability of the probe, and is suitable for testing occasions in different frequency bands.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115508594B_ABST
    Figure CN115508594B_ABST
Patent Text Reader

Abstract

The present invention discloses a method for preparing a MEMS probe for wafer-level testing, wherein a probe body is prepared by a micro-casting process, an insulating isolation layer is deposited on the surface of the probe body, and a shielding metal layer is prepared on the surface of the insulating isolation layer to complete the preparation of the probe. Due to the good micro-machining capability of MEMS technology, the present technical solution can be used to prepare a probe with good consistency, high precision, and strong anti-interference ability, which is suitable for high-needle parallel testing.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of wafer-level test probes, and in particular relates to a method for preparing a MEMS probe for wafer-level test. Background Art

[0002] Chips are known as "modern industrial food" and are the cornerstone of the new generation of information industry. The quality assurance of chip processing and the optimization of processing technology are completed through multiple testing procedures during the chip processing process. Among them, wafer-level testing is the dividing point between the early preparation of chips and the later packaging, and plays an important role in chip quality and processing cost control. With the rapid development of the semiconductor industry, the process accuracy requirements of chips are getting higher and higher, the line width on the chip is getting smaller and smaller, the size of the pad is getting smaller and smaller, and the arrangement density is getting higher and higher. For this reason, wafer-level testing requires the use of probes with higher accuracy and smaller size. In addition, with the increase in the speed of the processor chip core and memory chip, the speed of the test interface has also increased. The crosstalk noise between the probes during the test causes the test signal integrity to decrease, which has become a major problem facing wafer testing.

[0003] Patent CN111812366A discloses a method for manufacturing a wafer test microprobe based on microelectromechanical system (MEMS) technology. This solution adopts multiple photolithography and electroplating methods to improve the accuracy of the probe; Patent CN113391101A discloses a method for preparing a shell-core microprobe. By electroplating a highly conductive metal layer on the surface of the probe core prepared by LIGA or quasi-LIGA technology, the electrical performance of the probe is improved; Patent CN201721629633.4 discloses a high-frequency test probe and its preparation method. It completes the preparation of the high-frequency test probe by placing an ordinary probe in a cylindrical insulating sleeve, and placing a cylindrical ultra-fine copper tube outside the insulating sleeve. High-temperature resistant resin is filled between the ordinary probe and the insulating sleeve, and between the insulating sleeve and the ultra-fine copper tube for sealing and fixing.

[0004] The above patents respectively solve the problems of probe preparation accuracy, performance and crosstalk between probes when used for high-frequency testing, and promote the advancement of wafer-level test probe technology. However, patents CN111812366A and CN113391101A have low preparation efficiency, and the electroplating of probes with a cross-sectional size of about 50μm often takes several hours. The method for preparing high-frequency probes disclosed in patent CN201721629633.4 will greatly increase the radial size of the probe, especially when the shape of the probe is non-linear, the increase in radial size is more obvious. Summary of the invention

[0005] The invention provides a method for preparing a MEMS probe for wafer-level testing, and aims to provide a method for preparing the probe for wafer-level testing with high efficiency and high precision.

[0006] To achieve the above object, the present invention provides a method for preparing a MEMS probe for wafer-level testing, comprising the following steps:

[0007] Step 1, etching the polished surface of the first single crystal silicon wafer to obtain a mold cavity, the etching shape is the shape of the probe or the probe group, the etching depth is greater than or equal to the thickness of the probe, and the mold cavity includes a probe mold cavity and a probe interconnection area mold cavity;

[0008] Step 2, etching a feed inlet and an exhaust hole on a second single crystal silicon wafer, wherein the distance between the feed inlet and the exhaust hole is the length of the probe;

[0009] Step 3, removing the remaining photoresist on the first and second single crystal silicon wafers, contacting and pressing the polished surfaces of the first and second single crystal silicon wafers together, aligning the feed port with the mold cavity of the probe interconnection area, and aligning the exhaust hole with the other end of the probe mold cavity away from the mold cavity of the interconnection area;

[0010] Step 4: injecting the completely melted probe body material into the mold cavity through the feed port, and performing a degassing treatment to remove bubbles in the probe body material;

[0011] Step 5: After the probe body material is solidified, separate the first single crystal silicon wafer and the second single crystal silicon wafer, remove the single crystal silicon around the probe body material, release the probe or probe group, and obtain the probe body;

[0012] Step 6: depositing metal oxide / non-metal oxide as an insulating isolation layer on the surface of the probe body by magnetron sputtering, or preparing an organic polymer insulating isolation layer on the surface of the probe body by a Czochralski method;

[0013] Step 7, depositing a shielding metal film on the surface of the insulating isolation layer, and then electroplating a shielding layer made of the same material as the shielding metal film to obtain a shielding metal layer;

[0014] Step 8: Grind both ends of the probe body to expose the metal material of the probe body to obtain the probe.

[0015] Furthermore, in step 1 and step 2, dry etching is used when etching the two single crystal silicon wafers.

[0016] Furthermore, before executing step 3, the feed port is etched into a funnel shape.

[0017] Furthermore, in step 3, after the two single crystal silicon wafers are pressed together, the cavities of the probe molds are independent of each other except for the interconnection area.

[0018] Furthermore, in step 5, wet etching is used to remove the single crystal silicon around the probe body material.

[0019] Furthermore, after step 5 is completed, the surface of the probe body is polished.

[0020] Furthermore, electrochemical polishing is performed.

[0021] Furthermore, in step 6, the prepared insulating isolation layer completely insulates the probe body from the shielding metal layer, and the melting point of the material of the insulating isolation layer is greater than the highest temperature on the probe body when the probe is working.

[0022] Furthermore, in step 7, the material of the shielding metal layer is Cu or Ag.

[0023] Furthermore, in step 7, the thickness of the shielding metal layer is greater than the skin depth of the interfering electromagnetic wave in the shielding metal layer.

[0024] Compared with the prior art, the present invention has at least the following beneficial technical effects:

[0025] The method of the present invention is more efficient than the MEMS probe preparation method based on LIGA or quasi-LIGA technology (photolithography + electroplating) by directly filling the molten probe material into the mold prepared using MEMS technology. The existing electroplating method is to prepare the probe by reducing and continuously depositing the metal ions in the electroplating solution at the cathode under the action of the electric field. The deposition rate is often only tens of nanometers to hundreds of nanometers per minute. The present invention uses a method of directly filling the mold with molten material, which has a fast filling speed and can complete the filling of probe materials with a cross-sectional size of tens of microns within a few minutes.

[0026] When this technical solution is used to prepare a MEMS probe for wafer-level testing, the insulating isolation layer and the shielding metal layer are both prepared using micro-nano processing methods. The thickness of the insulating isolation layer can be as small as tens of nanometers, and the thickness of the shielding metal layer can be adjusted in the range of tens of nanometers to tens of micrometers to prepare probes for testing occasions in different frequency bands. Due to the high-precision processing characteristics of micro-nano processing technology, the dimensional accuracy of the probe is easier to control, and the increase in the radial size of the probe based on the size of the probe body can be controlled to a minimum of sub-micron level.

[0027] Furthermore, the present invention prepares a complete shielding layer outside the insulating isolation layer. The shielding layer can reduce the noise caused by coupling, mutual inductance or mutual capacitance between probes. The better the sealing of the shielding layer, the stronger the shielding effect. Setting a complete shielding layer helps to improve the anti-interference ability of high-frequency probes.

[0028] Furthermore, after obtaining the probe body, the surface of the probe body is polished so that the insulating isolation layer is more evenly attached to the probe surface, while reducing probe surface defects and stress concentration when the probe is working, thereby increasing the fatigue life of the probe. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] Figure 1 Prepare a flow chart for MEMS probes for wafer-level testing;

[0030] Figure 2 This is a schematic diagram of the first single crystal silicon wafer after etching;

[0031] Figure 3 This is a schematic diagram of the second single crystal silicon wafer after etching;

[0032] Figure 4 This is a schematic diagram of two single crystal silicon wafers pressed together;

[0033] Figure 5 The figure is a schematic diagram of the structure of a linear high-frequency probe prepared by the method of the present invention.

[0034] In the attached drawings: 1. the first single crystal silicon wafer; 2. the second single crystal silicon wafer; 11. the probe mold cavity; 12. the probe interconnection area mold cavity; 21. the feed port; 22. the exhaust hole; 3. the probe body; 4. the insulating isolation layer; 5. the shielding metal layer. DETAILED DESCRIPTION

[0035] In order to make the purpose and technical solution of the present invention clearer and easier to understand, the present invention is further described in detail below in conjunction with the accompanying drawings and embodiments. The specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.

[0036] In the description of the present invention, it should be understood that the terms "center", "longitudinal", "lateral", "up", "down", "front", "back", "left", "right", "vertical", "horizontal", "top", "bottom", "inside", "outside" and the like indicate positions or positional relationships based on the positions or positional relationships shown in the accompanying drawings, and are only for the convenience of describing the present invention and simplifying the description, rather than indicating or implying that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as limiting the present invention. In addition, the terms "first" and "second" are used only for descriptive purposes, and cannot be understood as indicating or implying relative importance or implicitly indicating the number of technical features indicated. Thus, the features defined as "first" and "second" may explicitly or implicitly include one or more of the features. In the description of the present invention, unless otherwise specified, "multiple" means two or more. In the description of the present invention, it should be noted that, unless otherwise clearly specified and limited, the terms "installed", "connected", and "connected" should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection, or it can be indirectly connected through an intermediate medium, or it can be the internal communication of two components. For ordinary technicians in this field, the specific meanings of the above terms in the present invention can be understood according to specific circumstances.

[0037] Example 1

[0038] Reference Figure 1 , a method for preparing a MEMS probe for wafer-level testing, comprising the following steps:

[0039] Step 1, spin-coating a 30 μm thick photoresist on the polished side of the first single crystal silicon wafer, limiting the pattern on the mask to the shape of the probe group, the probe is linear, 40 μm wide, 7000 μm long, 15 probes form a probe group, and transferring the pattern of the probe group to the photoresist through exposure and development to expose the single crystal silicon in the probe group pattern area; after the first single crystal silicon wafer is exposed and developed, the shape of the exposed single crystal silicon area is the same as the shape of the probe group;

[0040] Step 2, the single crystal silicon in the probe group pattern area exposed on the first single crystal silicon wafer is dry-etched with good anisotropy to a depth of 50 μm to form a mold cavity for MEMS micro casting, the mold cavity including a probe mold cavity 11 and a probe interconnection area mold cavity 12; the schematic diagram of the first single crystal silicon wafer after etching is shown in FIG. Figure 2 As shown;

[0041] Step 3, spin-coating a 30 μm thick photoresist on the polished side of the second single crystal silicon wafer, defining the pattern on the mask as the shape of the MEMS micro casting feed port and the exhaust hole, transferring the shape of the feed port and the exhaust hole to the photoresist through exposure and development, exposing the single crystal silicon in the feed port and the exhaust hole pattern area; after the second single crystal silicon wafer is exposed and developed, the shape of the exposed single crystal silicon area is the same as the shape of the feed port and the exhaust hole;

[0042] Step 4: Perform dry etching with good anisotropy on the exposed single crystal silicon area on the second single crystal silicon wafer, and completely etch through the area to form the feed port 21 and exhaust hole 22 of the mold cavity. The schematic diagram of the second single crystal silicon wafer after etching is shown in FIG. Figure 3 As shown;

[0043] Step 5, photolithography and etching are performed on the feed port 21 again to etch the feed port 21 into a funnel shape;

[0044] Step 6, removing the remaining photoresist on the two single crystal silicon wafers, and washing the two etched single crystal silicon wafers with HCl solution, NaOH solution, acetone, ethanol, and deionized water in sequence;

[0045] Step 7, the polished surfaces of the two cleaned single crystal silicon wafers are contacted and pressed together, the second single crystal silicon wafer is located above the first single crystal silicon wafer, the feed port on the second single crystal silicon wafer is aligned with the mold cavity of the probe interconnection area, and the exhaust hole is aligned with the other end of the mold cavity of the probe mold cavity away from the interconnection area. The schematic diagram of the two single crystal silicon wafers pressed together is as shown in Figure 4 As shown;

[0046] Step 8, filling the completely melted probe body material containing Cu and Pd into the mold cavity through the feed port, with the filling thickness equal to the probe thickness of 40 μm, and then performing ultrasonic degassing for 10 minutes to remove bubbles that may exist in the probe body material;

[0047] Step 9: After the probe body material is completely solidified and cooled, separate the two single crystal silicon wafers, and use a wet etching method to remove the single crystal silicon around the probe body material to release the probe group;

[0048] Step 10: polish the probe surface using an electrochemical polishing process so that the insulating isolation layer can be more evenly attached to the probe surface, while reducing probe surface defects, reducing stress concentration when the probe is working, and improving the fatigue life of the probe;

[0049] Step 11, using magnetron sputtering to deposit 1 μm thick Al2O3 as an insulating isolation layer on the other surfaces of the probe body except the two end faces in the length direction; the probe length direction refers to the direction of the largest external dimension of the probe; the insulating isolation layer completely insulates the probe body from the shielding metal layer, and the melting point of Al2O3 is greater than the highest temperature on the probe body when the probe is working;

[0050] Step 12, firstly depositing a 200nm shielding metal film on the surface of the insulating isolation layer by magnetron sputtering, and then depositing a 4μm thick metal Cu as a shielding layer on the surface of the shielding metal film by electroplating, the shielding metal film and the shielding layer constitute a shielding metal layer; the thickness of the shielding metal layer is greater than the skin depth of the interfering electromagnetic wave in the shielding metal layer;

[0051] Step 13: Grind the surface covered with the insulating isolation layer and the shielding metal layer within 200 μm from the two end faces in the length direction of the probe, remove the shielding metal layer and the insulating isolation layer in this part, and expose the metal material in this part of the probe body, so as to obtain Figure 5 The probes shown are used to form stable electrical connections with the signal lines on the probe card and the pads on the chip.

[0052] Example 2

[0053] Reference Figure 1 , a method for preparing a MEMS probe for wafer-level testing is as follows:

[0054] Step 1, spin-coating a 30 μm thick photoresist on the polished side of the first single crystal silicon wafer, limiting the pattern on the mask to the shape of the probe group, the probe is linear, 45 μm wide, 5000 μm long, 15 probes form a probe group, and transferring the pattern of the probe group to the photoresist through exposure and development to expose the single crystal silicon in the probe group pattern area; after the first single crystal silicon wafer is exposed and developed, the shape of the exposed single crystal silicon area is the same as the shape of the probe group;

[0055] Step 2, dry-etching the single crystal silicon in the probe group pattern area exposed on the first single crystal silicon wafer, with an etching depth of 50 μm, to form a mold cavity for MEMS micro-casting, the mold cavity including a probe mold cavity 11 and a probe interconnection area mold cavity 12; the schematic diagram of the first single crystal silicon wafer after etching is shown in FIG. Figure 2 As shown;

[0056] Step 3, spin-coating a 35 μm thick photoresist on the polished side of the second single crystal silicon wafer, defining the pattern of the mask to be the shape of the MEMS micro casting feed port and the exhaust hole, and transferring the shape of the feed port and the exhaust hole to the photoresist through exposure and development, exposing the single crystal silicon in the feed port and the exhaust hole pattern area; after the second single crystal silicon wafer is exposed and developed, the shape of the exposed single crystal silicon area is the same as the shape of the feed port and the exhaust hole;

[0057] Step 4, dry-etching the exposed single crystal silicon area on the second single crystal silicon wafer, and completely etching through the area to form a feed inlet and exhaust hole of the mold chamber. The schematic diagram of the second single crystal silicon wafer after etching is shown in FIG3 ;

[0058] Step 5, photolithography and etching are performed on the feed port again to etch the feed port into a funnel shape;

[0059] Step 6, removing the remaining photoresist on the two single crystal silicon wafers, and washing the two etched single crystal silicon wafers with HCl solution, NaOH solution, acetone, ethanol, and deionized water in sequence;

[0060] Step 7, the polished surfaces of the two cleaned single crystal silicon wafers are contacted and pressed together, the second single crystal silicon wafer is located above the first single crystal silicon wafer, the feed port on the second single crystal silicon wafer is aligned with the mold cavity of the probe interconnection area, and the exhaust hole is aligned with the other end of the mold cavity of the probe mold cavity away from the interconnection area. The schematic diagram of the two single crystal silicon wafers pressed together is as shown in Figure 4 As shown;

[0061] Step 8: Fill the completely melted probe body material containing Cu, Pd and Au into the mold cavity through the feed port, with a filling thickness of 45 μm for the probe thickness, and then perform ultrasonic degassing for 10 minutes to remove bubbles that may exist in the probe body material;

[0062] Step 9: After the probe body material is completely solidified and cooled, separate the two single crystal silicon wafers, and use wet etching to remove the single crystal silicon around the probe body material to release the probe group;

[0063] Step 10: polish the probe surface using an electrochemical polishing process so that the insulating isolation layer can be more evenly attached to the probe surface, while reducing probe surface defects, reducing stress concentration when the probe is working, and improving the fatigue life of the probe;

[0064] Step 11, using the Czochralski method to deposit a 2 μm thick polyurethane (PU) film as an insulating isolation layer on the other surfaces of the probe body except the two end faces in the length direction; the probe length direction refers to the direction of the largest external dimension of the probe; the insulating isolation layer completely insulates the probe body from the shielding metal layer, and the melting point of PU is greater than the highest temperature on the needle body when the probe is working;

[0065] Step 12, after the PU film is completely cured, a 300nm shielding metal film is first deposited on the surface of the insulating isolation layer by magnetron sputtering, and then a 5μm thick metal Ag is deposited on the surface of the shielding metal film by electroplating as a shielding layer, and the shielding metal film and the shielding layer constitute a shielding metal layer; the thickness of the shielding metal layer is greater than the skin depth of the interfering electromagnetic wave in the shielding metal layer;

[0066] Step 13: Grind the surfaces covered with the insulating isolation layer and the shielding metal layer within 300 μm from the two end faces in the length direction of the probe to remove the shielding metal layer and the insulating isolation layer at this position; expose the metal material at this position of the probe body, and obtain Figure 5 The probes shown are used to form stable electrical connections with the signal lines on the probe card and the pads on the chip.

[0067] The present invention provides a method for preparing a MEMS probe for wafer-level testing. The micro-nano manufacturing method is used to prepare an insulating isolation layer and a shielding metal layer on the surface of the prepared probe body. The thickness of the insulating isolation layer can be as small as tens of nanometers and as high as micrometers. The thickness of the shielding metal layer can be from tens of nanometers to tens of micrometers. Probes for testing occasions in different frequency bands can be prepared. The technical solution can be used to prepare probes with good consistency, high precision, and strong anti-interference ability, which are suitable for parallel testing of high needle counts.

[0068] According to the contents of the present invention, by utilizing the general knowledge and techniques in the art, without departing from the concept of the above scheme of the present invention, the present invention can make various modifications such as changing the probe shape, size, material, thickness of the insulating isolation layer or the shielding metal layer, and all other embodiments obtained without making any creative work shall fall within the scope of protection of the present invention.

Claims

1. A method for preparing a MEMS probe for wafer-level testing, characterized in that: The following steps are involved: Step 1, etching the polished surface of the first single crystal silicon wafer to obtain a mold cavity, the etching shape is the shape of the probe or the probe group, the etching depth is greater than or equal to the thickness of the probe, and the mold cavity includes a probe mold cavity and a probe interconnection area mold cavity; Step 2, etching a feed inlet and an exhaust hole on a second single crystal silicon wafer, wherein the distance between the feed inlet and the exhaust hole is the length of the probe; Step 3, removing the remaining photoresist on the first and second single crystal silicon wafers, contacting and pressing the polished surfaces of the first and second single crystal silicon wafers together, aligning the feed port with the mold cavity of the probe interconnection area, and aligning the exhaust hole with the other end of the probe mold cavity away from the mold cavity of the interconnection area; Step 4: injecting the completely melted probe body material into the mold cavity through the feed port, and performing a degassing treatment to remove bubbles in the probe body material; Step 5: After the probe body material is solidified, separate the first single crystal silicon wafer and the second single crystal silicon wafer, remove the single crystal silicon around the probe body material, release the probe or probe group, and obtain the probe body; Step 6: depositing metal oxide / non-metal oxide as an insulating isolation layer on the surface of the probe body by magnetron sputtering, or preparing an organic polymer insulating isolation layer on the surface of the probe body by a Czochralski method; Step 7, depositing a shielding metal film on the surface of the insulating isolation layer, and then electroplating a shielding layer made of the same material as the shielding metal film to obtain a shielding metal layer; Step 8: Grind both ends of the probe body to expose the metal material of the probe body to obtain the probe.

2. The method for preparing a MEMS probe for wafer-level testing according to claim 1, characterized in that: In the step 1 and the step 2, dry etching is used when etching the two single crystal silicon wafers.

3. The method for preparing a MEMS probe for wafer-level testing according to claim 1, characterized in that: Before executing step 3, the feed port is etched into a funnel shape.

4. The method for preparing a MEMS probe for wafer-level testing according to claim 1, characterized in that: In the step 3, after the two single crystal silicon wafers are pressed together, the cavities of the probe molds are independent of each other except for the interconnection area.

5. The method for preparing a MEMS probe for wafer-level testing according to claim 1, characterized in that: In the step 5, wet etching is used to remove the single crystal silicon around the probe body material.

6. The method for preparing a MEMS probe for wafer-level testing according to claim 1, characterized in that: After step 5 is completed, the surface of the probe body is polished.

7. The method for preparing a MEMS probe for wafer-level testing according to claim 6, characterized in that: Polishing is performed by electrochemical method.

8. The method for preparing a MEMS probe for wafer-level testing according to claim 1, characterized in that: In step 6, the prepared insulating isolation layer completely insulates the probe body from the shielding metal layer, and the melting point of the material of the insulating isolation layer is greater than the highest temperature on the probe body when the probe is working.

9. The method for preparing a MEMS probe for wafer-level testing according to claim 1, characterized in that: In step 7, the material of the shielding metal layer is Cu or Ag.

10. The method for preparing a MEMS probe for wafer-level testing according to claim 1, characterized in that: In step 7, the thickness of the shielding metal layer is greater than the skin depth of the interfering electromagnetic wave in the shielding metal layer.