Molded body made of opaque quartz glass and its preparation method

By adding SiO2 nanoparticles and optimizing the process during wet milling, the problems of density inhomogeneity and high cost of opaque quartz glass molds in semiconductor manufacturing have been solved, and molds with high uniform reflectivity have been prepared, which are suitable for high-quality components in semiconductor manufacturing.

CN115521062BActive Publication Date: 2026-11-17HERAEUS QUARZGLAS GMBH & CO KG
View PDF 13 Cites 0 Cited by

Patent Information

Application Number
CN202210676915.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2021-06-24
Filing Date
2022-06-15
Publication Date
2026-11-17
Estimated Expiration
2042-06-15

AI Technical Summary

Technical Problem

Existing opaque quartz glass molds cannot meet the requirements of high uniform reflectivity and cost-effective fabrication in semiconductor manufacturing, and traditional methods suffer from density inhomogeneity and difficulty in reproducing.

Method used

By adding SiO2 nanoparticles during the wet milling process, controlling the solid content of the slurry and the wet milling time, a uniform density distribution and a stable solid distribution are ensured. Using synthetic quartz glass materials and an optimized sintering process, a molded body with uniformity and density is prepared.

Benefits of technology

It achieves molded bodies with high uniform reflectivity, reduces density differences, improves the reproducibility and cost-effectiveness of fabrication, and is suitable for high-quality components in semiconductor manufacturing.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115521062B_ABST
    Figure CN115521062B_ABST
Patent Text Reader

Abstract

This application relates to a molded body made of opaque quartz glass and a method for preparing the same. The present invention provides a known method for preparing a molded body made of opaque quartz glass, the method comprising the following steps: (a) providing SiO2 grains obtained by pulverizing quartz glass having a purity of at least 99.9% by weight of SiO2; (b) forming a slurry comprising a suspension and the SiO2 grains and having a total solids content; (c) wet milling the SiO2 grains in the slurry to form milled SiO2 grain particles; (d) forming a porous green body from the slurry; and (e) sintering the porous green body to form the molded body. In order to provide a molded body made of opaque quartz glass produced by this method, which can be used to prepare components for semiconductor manufacturing with uniform reflectivity at low cost, it is proposed that the wet milling of the SiO2 grains is carried out at least temporarily in the presence of SiO2 nanoparticles in the total solids content of the slurry in the range of 0.1 wt% to 10 wt%, and that the slurry has a solids content in the range of 76 wt% to 80 wt% after the addition of the SiO2 nanoparticles and after the wet milling.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to a molded body made of porous opaque quartz glass, said opaque quartz glass having closed porosity, a chemical purity of at least 99.9% by weight of SiO2, and a density of 2.14 g / cm³. 3 Up to 2.19 g / cm 3 Density within the range.

[0002] Furthermore, the present invention relates to a method for preparing a molded body made of opaque quartz glass, the method comprising the following steps:

[0003] (a) Providing SiO2 grains obtained by crushing quartz glass having a purity of at least 99.9% by weight of SiO2.

[0004] (b) Forming a slurry comprising the suspension and the SiO2 grains and having a total solids content.

[0005] (c) Wet milling the SiO2 grains in the slurry to form milled SiO2 grain particles.

[0006] (d) Forming a porous green body from the slurry, and

[0007] (e) Sintering the porous green body to form the molded body.

[0008] Such molded bodies made of opaque quartz glass are used, for example, in the engineering of chemical processes or in semiconductor manufacturing for processing wafers to prepare quartz glass components and to optimize thermal management in processing chambers. Quartz glass components are, for example, simple quartz glass parts such as tubes, rods, plates, flanges, rings, or blocks. Alternatively, they are complex components, such as reactors or equipment, such as transport racks, bell jars, crucibles, protective screens, process tubes, etc. Further processing of the molded body to obtain components made of opaque quartz glass may include machining such as cutting, milling, grinding, polishing, and / or thermal processing such as welding, reshaping, and flame polishing. Background Technology

[0009] Prior Art 1

[0010] To prepare this type of molded body from opaque quartz glass, a known method is to first prepare quartz glass grains by crushing transparent quartz glass, and then further process these in a liquid to obtain a slurry. In the following text, the term "slurry" may also be used interchangeably with the terms slurry, suspension, or dispersion.

[0011] Therefore, for example, DE 43 38 807 C1 (equivalent publication: US 5,674,792 A) describes molded bodies made of opaque, closed-cell quartz glass. The quartz glass is characterized by a chemical purity of at least 99.9% by weight of SiO2, a hydroxyl group content of 30 to 600 ppm by weight, and a minimum concentration of 2.15 g / cm³. 3 Density within a certain range. At least 80% of the pores have a pore size of less than 20 μm. To prepare the molded body, naturally occurring crystalline quartz raw material is purified, electrofused to obtain quartz glass, and then the quartz glass is ground to obtain fine SiO2 grains with a purity exceeding 99.9% by weight. The ground SiO2 grains are further pulverized by wet grinding in deionized water using grinding balls to obtain "ground SiO2 grain particles". After wet grinding, the particle size of the ground SiO2 grain particles is in the range of 0.45 μm to 50 μm, of which approximately 60% of the SiO2 particles have a size in the range of 1 μm to 10 μm. The resulting slurry has a solids content of approximately 78%, and is poured into a plaster mold, dried to form a green body, and compacted by sintering in temperature intervals between 1350°C and 1450°C to form a closed-cell molded body made of opaque quartz glass with a hydroxyl group content of 100 ppm by weight to 500 ppm by weight.

[0012] Molded bodies prepared in this manner from opaque quartz glass exhibit low spectral transmittance in the wavelength range of 190 nm to 2650 nm and have an irradiation layer thickness of 1 mm at a practically constant level of less than 10%. Therefore, it is suitable for fabricating components where thermal insulation or heat dissipation is critical at high temperatures. Furthermore, opaque quartz glass exhibits properties that are otherwise characteristic and advantageous to quartz glass, such as a low coefficient of thermal expansion, high-temperature stability, and good chemical resistance to many processing media.

[0013] DE 44 40 104 A1 (equivalent publication: US 5,736,206 A) describes the development of a molded body from DE 43 38 807 C1. This molded body has transparent surface regions, which are produced by localized heating of the surface, for example, by means of a heated burner, a plasma torch, or a CO2 laser.

[0014] EP 3 205 630 A1 proposes that, in order to prepare a diffuser material made of opaque quartz glass with particularly high purity requirements, synthetically prepared transparent quartz glass grains with a hydroxyl group content of at least 200 ppm by weight are used as the starting material instead of naturally occurring quartz glass grains. The starting material is pulverized, and the pulverized grains are further wet-milled in a slurry to obtain a particle size with an average of less than 10 μm. The slurry is poured into a mold to form a green body, which is dried at a temperature below 1400°C and then sintered to achieve a density of 2.145 g / cm³. 3 The diffuse material forms a molded body. Considering impurities of 0.4 ppm by weight of Li, Na, K, Mg, Ca, Fe, Cu, Cr, Mn, Ti, Al, Zr, Ni, Mo and W, its purity exceeds 99.99% SiO2.

[0015] EP 1 516 864 A2 (equivalent publications: DE 103 44 189 A; JP 2005097103 A) describes a method for preparing casting parts made of a glassy composite material by casting a highly filled slurry with a solids content of at least 80% by weight. First, a homogeneous base slurry is prepared by grinding high-purity synthetic amorphous quartz glass in deionized water. The base slurry may contain up to 5% by weight of SiO2 nanoparticles. A composite slurry is produced from the base slurry by mixing it with additional quartz glass grains with a particle size greater than 10 μm. The composite slurry is further homogenized and then poured into an impermeable mold. A frozen blue preform is formed, which is subsequently dried and sintered. Furthermore, a pipe made of an opaque glassy composite material is described, having a homogeneous matrix of quartz glass in which quartz glass grains with a grain size greater than 10 μm are embedded. The average density of the composite material is, for example, 2.15 g / cm³. 3 .

[0016] In the method known from EP 1 516 864 A2, the highly filled slurry solidifies in volume rather than starting from the surface through contact with the liquid-absorbing mold. The high solids content stabilizes the slurry and counteracts rapid settling. However, freeze-drying blue green bodies is a lengthy, energy-intensive, and difficult-to-reproduce process. This is because the green body may be lost if the liquid is not removed quickly enough during thawing. This is particularly problematic in the case of thick-walled green bodies. Furthermore, highly filled slurries with a solids content greater than 80% exhibit unfavorable flow behavior with high viscosity at both low and high shear rates. Therefore, on the one hand, casting structures (visual inhomogeneities) can easily form during mold filling. On the other hand, closed air bubbles cannot escape and result in cavities in the sintered molded body.

[0017] Opaque quartz glass is also suitable for coating formation. Slurry-based preparation methods for this purpose are described in EP2 069 244 B1 (equivalent application: US 8,209,998 B2) and EP 2 878 584 A1 (equivalent application: US 9,680,360B2). To adjust the flow properties of the slurry or optimize the coating function, SiO2 nanoparticles are added to the slurry. Summary of the Invention

[0018] Technical goals

[0019] In principle, increased productivity in semiconductor manufacturing is accompanied by increased demands on the quality of materials used in the process, particularly regarding chemical purity. As semiconductor structures become increasingly miniaturized, public attention is also focused on other material properties that are prerequisites for the large-area uniform processing of semiconductor components, such as the high and uniform reflectivity of the components used. Molded bodies or components made of opaque quartz glass to date have not adequately met these requirements.

[0020] Therefore, the present invention aims to provide a molded body made of opaque quartz glass, which can be used to prepare high-quality components for semiconductor manufacturing, particularly components with uniform reflectivity.

[0021] The present invention is also based on the aim of specifying a cost-effective and reproducible method for preparing such molded bodies made of opaque quartz glass. Detailed Implementation

[0022] Regarding this method, the objective is achieved according to the invention starting with a method of the type mentioned at the beginning, which involves wet milling of SiO2 grains according to method step (c) at least temporarily in the presence of SiO2 nanoparticles, the proportion of which in the total solids content of the slurry is in the range of 0.1% by weight to 10% by weight, and is characterized in that, after the addition of SiO2 nanoparticles and after wet milling, the slurry has a solids content in the range of 76% by weight to 80% by weight.

[0023] A prerequisite for uniform reflectivity in molded bodies is uniform density and solids distribution. In the case of slurry casting methods, density differences can occur during the molding of green bodies from the slurry via settling and / or separation (segregation). This is especially true when the slurry contains a mixture of different mobile solid particles, which can lead to the enrichment of specific particle types and size fractions in different volumetric regions of the green body. When molding green bodies from the slurry, gravity and the direction of liquid absorption (dehydration direction) are decisive influencing variables in forming different volumetric regions with distinct characteristics. In a suspension, solid particles settle to the bottom under the influence of gravity. The settling rate is proportional to the square of the particle size (at least for low settling rates). This leads to particle size segregation. Furthermore, particles of different sizes aggregate to varying degrees. In this way, settling results in a density difference from top to bottom. The present invention aims to reduce the influence of these and other influencing variables that can lead to non-uniform density and solids distribution in the green body.

[0024] The solid component of the slurry required by this method is SiO2 grains (hereinafter also referred to as "quartz glass grains") obtained by crushing quartz glass. Other solid components of the slurry required by this method are SiO2 nanoparticles. These are prepared, for example, from organosilicon compounds converted to SiO2 through polymerization, condensation, oxidation, pyrolysis, or precipitation. In this method, fine synthetic SiO2 dust particles with a size less than 1 μm, preferably less than 500 nm, are precipitated as intermediates, final products, or byproducts; these are referred to herein as "SiO2 nanoparticles".

[0025] During wet milling, the quartz glass grains are further pulverized. The intensity of the pulverization process can be enhanced by adding a grinding media, preferably composed of synthetically prepared quartz glass. In the method according to the invention, wet milling is carried out at least temporarily or throughout the entire milling duration in a slurry containing SiO2 nanoparticles in addition to the quartz glass grains.

[0026] The particle size of SiO2 nanoparticles is typically in the range of approximately 100 nm ± 50 nm. They possess a large surface area and create contact points in the green body, promoting hard sintering of the molded body. For this reason, SiO2 nanoparticles are often added to the slurry, especially after the wet milling process is completed; this is sometimes referred to as “pulverization.” In contrast, the presence of SiO2 nanoparticles has been found to have a favorable effect on some properties of the molded body obtained as a processed product, even during the wet milling of quartz glass grains. In particular, a particularly uniform density distribution, referred to below as “uniformity,” has been observed within the volume of the molded body. This is not bound by this explanation but is attributed to the fact that the wet milling process on the quartz glass grains continuously generates new fracture surfaces, which form fresh and relatively reactive surfaces with which the SiO2 nanoparticles can interact. This interaction can lead to the formation of weak bonds due to intermolecular forces and hinder the flowability of both SiO2 nanoparticles and milled SiO2 grains, resulting in a stable solid distribution within the slurry volume even with a relatively low solid content of less than 80% by weight, preferably less than 79.5% by weight. In this way, for example, sedimentation or segregation of different solid components can be counteracted, especially if the molding of the porous green body involves pouring the slurry into a liquid-absorbing mold.

[0027] Compared to the density distribution achievable during wet milling without the addition of SiO2 nanoparticles, the molded bodies prepared in this manner exhibit a measurably more uniform density distribution. No visually discernible inhomogeneities were observed in the sintered molded body volume, such as the translucent regions observed after wet milling without the addition of SiO2 nanoparticles or with delayed addition. The molded bodies have a visually uniform appearance.

[0028] The degree of interaction depends on the concentration of SiO2 nanoparticles in the slurry. To achieve a significant effect on uniformity, the proportion of SiO2 nanoparticles in the total solids content of the slurry is in the range of 0.1 wt% to 10 wt%, preferably in the range of 1 wt% to 2 wt%, and most preferably at most 5 wt%. At very high proportions of SiO2 nanoparticles (greater than 10 wt%), the viscosity of the slurry increases, making casting more difficult. Furthermore, this results in a lower density of the green body, making hard sintering more difficult.

[0029] The degree of interaction also depends on the duration of the wet milling process in the presence of SiO2 nanoparticles. This essentially involves the pulverization process. Therefore, it has been shown that it is effective to wet mill SiO2 grains in the presence of SiO2 nanoparticles for at least 1 hour, preferably at least 10 hours, and particularly preferably at least 120 hours, according to method step (c). Wet milling processes lasting longer than 240 hours result in a relatively further gain in uniformity, although particularly high uniformity requirements may justify the long process duration.

[0030] The total solids content of the slurry is obtained at the end of the wet milling process. This is set as a target value from the beginning or from the initial solids content by adding additional solids during the wet milling process. Some deviation from the target value may occur due to abrasion from any grinding media. The initial solids content comprises quartz glass grains, and it may also comprise at least some SiO2 nanoparticles. The formation of the slurry according to step (b) involves mixing a suspension with the initial solids content / total solids content, which may be absorbed in a separate dispersion. The wet milling process begins when the slurry (with or without additional grinding media) is moved sufficiently strongly by stirring, rotating, applying ultrasound, or some other means to pulverize the quartz glass grains.

[0031] At the end of the wet milling process and during the molding of the porous green body, the solids content of the slurry is set to be in the range of 76% to 80% by weight, preferably in the range of 77% to 79.5% by weight. This makes it possible to prepare molded bodies particularly cost-effectively by introducing the slurry into a mold that absorbs a portion of the suspension (e.g., by pouring). Furthermore, at solids contents less than 76% or less than 77% by weight, the process can cause rapid settling, and thus particle size segregation, and consequently, non-uniform green bodies and molded bodies. At solids contents greater than 80% or greater than 89.5% by weight, the process can hinder the homogenization of the slurry and create casting structures in the molded body.

[0032] The slurry contains SiO2 nanoparticles from the outset, or the SiO2 nanoparticles are added to the slurry before or during the wet milling process. This addition is advantageously carried out by adding them to a dispersion, by means of which the nanoparticles are in colloidal form at a concentration of at least 20 μL. 2 At least a portion of the SiO2 nanoparticles in the slurry have a specific surface area (BET) of / g.

[0033] Adding SiO2 nanoparticles to the dispersion simplifies its processing.

[0034] To ensure a more uniform distribution of the solids contained therein, homogenization is performed by moving the slurry or dispersion.

[0035] In a particularly advantageous variation of the method, after wet milling, the slurry is cooled in continuous motion for at least 1 hour, preferably at least 10 hours, and particularly preferably at least 30 hours.

[0036] Some of the kinetic energy used during the grinding process is converted into heat. This causes the slurry to heat up during wet grinding. After the wet grinding process is complete, the temperature of the slurry is typically in the range of 30°C to 60°C. It has been found that molding green bodies from heated slurry can lead to inhomogeneities in the green bodies and molded bodies. Therefore, in this preferred variation of the method, a gradual cooling of the slurry is provided without grinding media and with continuous movement. The gradual cooling of the slurry is, for example, controlled, regulated, or (preferably) free cooling to ambient temperature, such as to room temperature.

[0037] It has been confirmed that if the slurry contains SiO2 particles after wet milling, and these SiO2 particles have a D-size of less than 50 μm, it will be effective. 90 and D less than 15μm 50 A value-limited granularity distribution is advantageous.

[0038] In this case, wet milling is preferably performed in a drum mill lined with plastic and using abrasive media made of synthetic quartz glass, until D is obtained. 90 Particle size distribution with values ​​less than 50 μm. This particle size distribution refers to milled SiO2 grains prepared by wet milling. SiO2 nanoparticles have a particle size distribution outside the range detectable by measurement methods.

[0039] It has been shown that it is particularly beneficial if the pH of the slurry is in the range of 3 to 5 and the solids content is in the range of 77% to 79.5% by weight after the wet milling process is completed.

[0040] The pH range and solids content range mentioned above characterize the corresponding values ​​at the end of the wet milling process.

[0041] Depending on the height and volume of the molded body to be prepared, the molding time (pouring time) can range from several hours to several days. Therefore, it is advantageous if the slurry exhibits settling behavior, characterized by the formation of sediment less than 20 mm in height after a 24-hour settling period in a 145 mm slurry column. Whether the slurry possesses this property can be determined using experiments described according to the "Definitions and Measurement Methods".

[0042] SiO2 grains are preferably obtained by crushing synthetically prepared transparent quartz glass, wherein the crushing includes electric and / or electro-hydraulic crushing of the quartz glass.

[0043] In electro-hydraulic crushing, ultrashort high-voltage pulses are applied to SiO2 grains in a liquid (such as water). When the voltage rise time is less than 500 ns, the high-voltage pulse preferably penetrates the solid particles. This is because the dielectric strength of the liquid (water) is higher than that of the solid when the voltage rise time is short. Conversely, spark discharge occurs during electro-hydraulic crushing of liquid carrier media (e.g., water). In both cases, electrical breakdown results in pressure fluctuations (shock waves), which ensures largely contamination-free pulverization of the quartz glass grains.

[0044] The green body is preferably obtained by pouring the slurry into a mold. However, other processing methods of the slurry are also suitable, such as drawing it into a mold, dipping, spraying, painting, thin coating, removal, coating, scraping, etc.

[0045] In the preferred procedure, the green body is dried before sintering, and the drying is preferably carried out at a high temperature and includes a drying duration of at least 24 hours.

[0046] For economic reasons, the drying time should be as short as possible. During the process, drying may take several days, such as 7 days or less, depending on the molded body or the drying temperature. The drying temperature should advantageously not exceed 120°C to avoid sudden escape of water vapor.

[0047] Furthermore, it has been shown that it is advantageous to remove the surface area of ​​the green blank by machining, particularly by sand milling, prior to sintering, with the preferred use of machining tools having a machined surface made of plastic-bonded grains.

[0048] The green body typically already has a shape close to the final outline of the molded body to be prepared. This is, for example, a solid monolith or a hollow body. Machining produces a shape close to the final outline or achieves surface smoothing or structuring. In addition, surface areas that may contain impurities are removed. These impurities may have been formed on the surface, for example, through previous process steps, and may cause undesirable surface devitrification in subsequent sintering steps.

[0049] Compared to metal or ceramic adhesives, the wear of plastic adhesives for cutting, grinding, or polishing can be burned off, and therefore does not result in the significant introduction of impurities into the green body.

[0050] When quartz glass grains are crushed according to step (a) of method, as in the case of wet milling in step (b), fracture surfaces and fragments are produced, which are typically not spherical but rather have non-spherical, cracked, or split morphologies. In the green body, these SiO2 particles interlock with each other. This increases strength, reduces the tendency to fracture, and thus facilitates the handling of the green body.

[0051] The green body is dried and sintered to form an airtight, mechanically stable molded body. The intensity of the sintering process is selected to achieve the highest possible closed porosity of the molded body. The appropriate sintering parameters (sintering temperature, sintering time, atmosphere) are determined based on simple experiments.

[0052] In an advantageous procedure, sintering according to method step (d) is carried out at a sintering temperature in the range of 1325°C to 1600°C, particularly at a sintering temperature below 1500°C and more preferably below 1450°C, preferably in air.

[0053] Regarding the molded body made of opaque quartz glass, the above-mentioned technical objective is achieved according to the invention starting with a molded body having the characteristics mentioned at the beginning, wherein the quartz glass has uniformity defined by the fact that the molded body has a first volume region of maximum density and a second volume region of minimum density, wherein the density difference between the maximum and minimum density is less than 0.025 g / cm³. 3 .

[0054] Obviously, the molded body volume ideally has no density difference at all. However, in practice, the difference between the maximum and minimum density exists within the range of measurement accuracy. These density differences arise due to gravity, settling, and / or stratification (segregation) when the green body is formed from a slurry of a mixture of different movable solid particles, as explained above in more detail with reference to the method according to the invention.

[0055] Less than 0.026 g / cm³ 3 Preferably less than 0.018 g / cm³ 3 The density difference between the maximum and minimum density is reflected by a visually uniform opaque appearance, such as the absence of translucent or transparent volume areas at the edges of the molded body.

[0056] The molded body according to the invention is preferably prepared by the above-described slurry casting method using a casting mold with a liquid-absorbing wall. It is preferably composed of synthetically prepared quartz glass. The synthetic quartz glass is characterized by high purity. The synthetic quartz glass is prepared using a synthetically prepared starting material containing organosilicon. It is highly pure in the sense that the main component is SiO2, and unwanted impurities are present at most in the sub-ppm range. The opaque quartz glass preferably has a total impurity content of Li, Na, K, Mg, Ca, Fe, Cu, Cr, Mn, Ti, Al, Zr, Ni, Mo, and W not exceeding 0.5 ppm by weight. The opacity of the molded body is determined by the number, size, and shape of the pores. These serve as optical interference points in the quartz glass matrix and make the molded body opaque (translucent or opaque), depending on the layer thickness. The pores are as small as possible and uniformly distributed in the quartz glass molded body. At least 80% of the pores have a pore size of less than 20 μm, preferably less than 15 μm, and particularly preferably less than 10 μm. The 80% pore ratio refers only to pores with a diameter greater than 1 μm.

[0057] Molded bodies are hermetically tight and therefore lack open porosity. This makes them suitable for applications where high thermal and chemical stability, as well as high resistance to corrosive gases and liquids, are important. The open porosity of a workpiece reflects its absorbency, which is detectable based on a dye penetration test. Molded bodies with a porosity less than 3% are referred to herein as "hermetically tight," which can also be detected by the lack of absorbency in a dye penetration test. The porosity of molded bodies typically ranges from 0.5% to 3% by weight.

[0058] Molded bodies can be used as diffuse reflective components in heating devices. The high uniformity of molded bodies also contributes to more uniform reflectivity, particularly in the infrared wavelength range. This, in turn, enables reduced heat loss and energy savings in heating, and allows for optimization of thermal conditions within the heating device. For example, the usable furnace area can be increased, and process fluctuations can be reduced.

[0059] Molded bodies typically possess one or more of the following properties:

[0060] ·In 4×10 10 dPa·s up to 7×10 10 Viscosity at 1350℃ in the range of dPa·s

[0061] • Elastic modulus of at least 68 GPa

[0062] • Shear modulus of at least 29 GPa

[0063] • Flexural strength of at least 100 MPa

[0064] • Dielectric strength of at least 30 kV / mm

[0065] At least 10 16 Specific resistance of Ωm

[0066] • Relative permittivity of up to 3.8.

[0067] Definitions and measurement methods

[0068] The terms described above are defined as follows. These definitions form part of this specification. In the event of any conflict between one of the following definitions and the rest of the description, the statements in the remainder of this specification shall prevail.

[0069] If no measurement method is specified for a parameter, a standard measurement method shall be used for that parameter, and in particular, the measurement method specified in the relevant ISO specification whose publication date is closest to the publication date of this application. If no measurement conditions are specified, the following conditions shall apply as standard conditions (SATP conditions): temperature: 298.15 K (25 °C, 77 °F) and absolute pressure: 100 kPa (14.504 psi, 0.986 atm).

[0070] Opaque quartz glass

[0071] Opaque quartz glass contains small air bubbles, which cause light scattering and give the glass a translucent to whitish appearance. There is a fluid transition between opacity and translucency. Translucency refers to the partial transmission of light, based on a lower degree of light absorption than on light scattering. Opacity is the reciprocal of translucency. In this respect, opacity is a measure of the light impermeability of quartz glass.

[0072] Synthetic preparation of quartz glass

[0073] Synthetic transparent quartz glass can be obtained, for example, through flame hydrolysis or oxidation of synthesized organosilicon compounds, through polycondensation of organosilicon compounds according to the so-called sol-gel method, or through hydrolysis and precipitation of inorganic silicon compounds in a liquid. In the industrial production of synthetic quartz glass, primary particles rich in SiO2 are also precipitated as so-called dust or filter dust. After pre-compacting by granulation, this dust can also be sintered or melted to obtain synthetic transparent quartz glass.

[0074] slurry

[0075] The term "slurry" is used to refer to a suspension or dispersion of liquid and SiO2 solid particles. The liquid used may be water, which is purified by distillation or deionization to minimize impurities. The term "slurry" is also commonly used instead of "slurry."

[0076] Particle size and particle size distribution

[0077] Use D 10 Or D 50 Or D 90 The values ​​characterize particle size and particle size distribution. These values ​​are taken from particle size distribution curves that show the cumulative volume of SiO2 particles as a function of particle size. In this case, D 10 The value represents the particle size that does not reach 10% of the cumulative volume of SiO2 particles, and therefore, D 90 The value represents the particle size that does not reach 90% of the cumulative volume of SiO2 particles. Particle size distribution was determined using a Mastersizer 3000 particle analyzer from Malvern Panalytical GmbH by scattered light and laser diffraction spectroscopy according to ISO 13320.

[0078] Measuring Settlement Behavior

[0079] Add sufficient slurry to the graduated cylinder until a column height of 145 mm is achieved. After predetermined time intervals, measure the height of the supernatant (above the precipitate). The height of the precipitate is thus determined. The graduated cylinder is not moved during the process.

[0080] Measure the maximum density difference

[0081] Since the molded body according to the invention does not have open porosity, simple density measurement of the sample is possible according to Archimedes' principle.

[0082] Density distribution was determined by taking at least three uniformly distributed density measurement samples at a measurement distance of 1 cm and having a distance of approximately 1 cm above the height of the cylindrical sample body. 3 The density is determined by the sample volume. The density measurement sample includes a volume region arranged at the bottom during the molding (casting) of the green body and a volume region arranged at the top along the longitudinal axis of the cylinder of the sample body during the molding of the green body. The sample body is 5 cm high, such that, for example, the center-to-center distance of the three density measurement samples is 1.5 cm and the distance from the end face is 0.5 cm.

[0083] The maximum and minimum densities are determined from the density measurement samples.

[0084] Pore ​​diameter / pore volume (porosity) ) / Aperture Distribution

[0085] The pore size is the maximum distance between two opposing pore walls. The "pore volume" of a porous material represents the free volume occupied by cavities within the material. Pore volume is determined based on density measurements.

[0086] Considering the specific density of transparent quartz glass, the porosity was determined based on density measurements; it is approximately 2.2 g / cm³. 3 .

[0087] Aperture distribution represents the frequency of the measured apertures. Apertures are determined using scanning electron micrographs of polished sample portions. In the case of circular apertures, it is expressed as the measured diameter, and in the case of non-circular apertures, it is expressed as the average diameter, which is calculated from the area of ​​the inner circle of an ellipse that is as large as possible and surrounds only the aperture surface, with the diameter of the ellipse perpendicular to the aperture surface at the same center point.

[0088] sintering

[0089] "Sintering" refers to the process of treating a molded body at a high temperature above 1100°C and hot-compacting it during the process. Sintering can be carried out in air, under an inert gas, or under a vacuum. Vacuum should be understood to mean an absolute gas pressure of less than 2 mbar. Attached Figure Description

[0090] The invention will now be explained in more detail using exemplary embodiments and accompanying drawings. Detailed Description:

[0091] Figure 1 This is a flowchart explaining the production of an embodiment of the molded body according to the present invention.

[0092] Figure 2 It is a photograph of a cross-section parallel to the longitudinal axis of a cylindrical reference sample produced according to existing technology.

[0093] Figure 3 It is a diagram showing the sedimentation process of different slurries.

[0094] Figure 4 It is a bar chart showing the flowability of different slurries.

[0095] Figure 5 This is a bar graph showing the aperture distribution of the molded body according to the present invention.

[0096] Figure 6 It is a graph showing the particle size distribution in the slurry after the wet milling process is completed, and

[0097] Figure 7 It is a bar graph showing the density of quartz glass plates prepared from different slurries. Detailed Implementation

[0099] based on Figure 1 The following examples illustrate the method according to the invention using a preparation example of a plate-shaped molded body made of opaque quartz glass for use in a heating apparatus for semiconductor manufacturing.

[0100] Crushed quartz glass crystals 1

[0101] Typically, transparent synthetic quartz glass cylinders are prepared by flame hydrolysis of a starting material containing organosilicon. The quartz glass cylinders are sawn into segments, and these segments are crushed by electric or electro-hydraulic crushing to form SiO2 grains 1. These grains made from synthetically prepared SiO2 represent one of the starting materials for the slurry.

[0102] SiO2 nanoparticles prepared by pyrolysis

[0103] The SiO2 nanoparticles prepared by the pyrolysis method used in this paper are commercially available as a white, loose powder under the name "ZANDOSIL". This powder has a particle size of approximately 30 μm. 2 The SiO2 nanoparticles have a BET surface area of ​​approximately 200 g / L and a bulk density of approximately 200 g / L. They exist as aggregates or agglomerates of primary SiO2 particles and typically exhibit a wide particle size distribution ranging from approximately 5 nm to approximately 200 nm, with a typical size of approximately 100 nm ± 50 nm. SiO2 nanoparticles readily adhere to each other and form large clusters, making it difficult to measure the size of individual particles. A simple and relatively accurate method for particle size determination is using microscopy.

[0104] Suspension 3

[0105] For a batch of 10 kg slurry 1 (SiO2 water slurry), 8.2 kg of amorphous synthetic quartz glass crystals 1 and 1.8 kg of deionized water 3 with a conductivity of less than 1 μS are mixed in a drum mill lined with polyurethane and having a volume capacity of about 20 liters.

[0106] Dispersion 4

[0107] SiO2 nanoparticles 2 were absorbed in deionized water with a conductivity of less than 1 μS in colloidal form at a weight ratio of 50:50, and the dispersion 4 was homogenized by using a stirrer and stored in a rolling manner until use.

[0108] Basic slurry 5

[0109] The suspension 3 and dispersion 4 are combined to form a base slurry 5. In this case, the proportion of dispersion 4 is adjusted such that the added SiO2 nanoparticles account for 1%, 2%, 5%, or 10% of the solid content of the base slurry 5. Thus, the solid content consists of amorphous synthetic quartz glass grains and SiO2 nanoparticles, and at the end of the wet milling process, the solid content is in the range of 76% to 80% by weight, particularly preferably in the range of 77% to 79.5% by weight. In this case, it is considered that the solid content slightly increases due to the wear of the grinding media during the wet milling process.

[0110] A grinding media made of synthetic quartz glass is added to the base slurry 5 and ground on a roller at 20 rpm. During wet grinding, the pH decreases to approximately 4. Simultaneously, the quartz glass grains 1 are further pulverized, thereby continuously generating new fracture surfaces and forming new and relatively reactive surfaces. SiO2 nanoparticles 2 can interact with these surfaces, which can reduce the migration rate of both the SiO2 nanoparticles and the ground SiO2 grains. Therefore, the solid distribution within the slurry volume can be stabilized, and the separation of different solid components can be reduced.

[0111] During wet milling, the aforementioned quartz glass grains 1 are ground to obtain fine SiO2 powder particles. The wet milling process continues until a particle size distribution is established, wherein the particle size distribution of the powder particles reaches a D of less than 50 μm. 90 Value. In one exemplary embodiment, after an 11-day wet milling duration, a D value with 42.5 μm was obtained. 90 Value, 12.7μm D 50 Value and 2.18μm D 10 Granularity distribution of values. Figure 6 The graph shows the corresponding particle size distribution. In this case, the proportional particle volume V (in %) is plotted on the y-axis, and the particle size d (in μm) is plotted on the x-axis. Fine fractions with particle sizes smaller than 1 μm cannot be resolved using the selected measurement method, i.e., SiO2 nanoparticles cannot be resolved. However, larger particles produce more accurate results, which determine the termination of the wet milling process.

[0112] Stabilization of slurry 6a

[0113] The result of the wet milling process is a homogenized slurry 6a of water, milled SiO2 grains and SiO2 nanoparticles, which also contains low, undetermined SiO2 fractions from abrasion by the quartz glass grinding media.

[0114] Following the wet milling process, the homogenized slurry 6a has a temperature of approximately 40°C and is characterized by a uniform solids distribution. The milling media are removed, and the slurry 6a is allowed to reach ambient temperature by being stored on rollers and allowed to cool freely under motion. Cooling the slurry 6a to ambient temperature (25°C) under rotation takes several hours, for example, 30 to 200 hours; in an exemplary embodiment, it is 48 hours. This process stabilizes the previously generated uniform solids distribution. A homogenized and stable slurry 6b is obtained, consisting of a suspension, milled SiO2 powder particles, SiO2 nanoparticles, and a proportion of SiO2 abraded from the milling media.

[0115] Preparation of green body and SiO2 molded body

[0116] Under pressure, a homogenized stabilized slurry 6b is poured into a plastic mold having a liquid-tight cylindrical jacket and a porous substrate made of plastic. The substrate is adjacent to a drainage system, on which additional negative pressure can be applied to accelerate dehydration. Within the plastic mold, the homogenized stabilized slurry 6b is dehydrated to form a porous cylindrical green body 7 with an outer diameter of 100 mm. Several green bodies 7 with cylindrical heights ranging from 50 mm to 100 mm were produced experimentally.

[0117] To remove the bound water, the green blank 7 was dried in a ventilated oven at approximately 60°C for two days, and after cooling, the contaminated surface areas of the still porous green blank 7 were ground away. When using a grinding disc, the grinding media was fixed in a plastic holder. The amount of material removed was approximately 0.5 mm at the cylindrical jacket surface and approximately 5 mm at the end faces.

[0118] To sinter the green body 7, the green body is heated in a sintering furnace to a heating temperature of 1375°C (or 1400°C in the case of a measurement sample) in air at a heating rate of 2°C / min and held at that temperature for 4.5 hours. It is then cooled to a furnace temperature of 1000°C at a cooling rate of 2°C / min, and then left unadjusted with the furnace closed. A quartz glass cylinder 8 with a diameter of 90 mm is obtained. Depending on the initial height of the green body 7, the cylinder height ranges from approximately 45 mm to 90 mm.

[0119] Table 1 summarizes the composition of the measured samples A to G and the comparative samples H and J, the solid content in the slurry when poured into the casting mold, the time of addition of SiO2 nanoparticles, and the optional sintering temperature.

[0120] Table 1

[0121]

[0122]

[0123] Here:

[0124] The BEFORE in column 2 means that the indicated proportion of SiO2 nanoparticles are added to the slurry before the wet milling process begins.

[0125] The AFTER in column 3 means that SiO2 nanoparticles in the indicated proportions are added to the slurry after the wet milling process is completed.

[0126] The resulting quartz glass cylinder 8 (molded body) is composed of non-porous synthetic quartz glass with a purity of at least 99.99% by weight of SiO2 and a density of 2.15 g / cm³. 3 The total porosity of the molded body is approximately 2.5%. The pores have a maximum size of less than 20 μm; typically (median), the maximum size is approximately 3 μm.

[0127] The quartz glass exhibited a total impurity content of 0.2 ppm by weight for Li, Na, K, Mg, Ca, Fe, Cu, Cr, Mn, Ti, Al, Zr, and Ni. These impurities were determined by ICP-OES or ICP-MS.

[0128] Molded quartz glass includes:

[0129] ·6×10 10 Viscosity at 1350℃ (dPa·s)

[0130] • Elastic modulus of 70 GPa

[0131] • Shear modulus of 30 GPa

[0132] • 120MPa bending strength

[0133] • Dielectric strength of 32kV / mm

[0134] ·5×10 16 Specific resistance of Ωm

[0135] · Relative permittivity of 3.8.

[0136] The green bodies obtained from comparative sample H exhibited visual separation of solid particles with a higher proportion of coarse grains in the lower region of the green body. The green bodies obtained from comparative sample J exhibited casting banding and a filling structure. This effect was particularly pronounced in the sintered molded body. Then, in sample H, a large density difference existed between the top and bottom because the finer fractions were more sinteringly active than the coarser particles. The upper portion of the molded body became very dense and visually translucent, while the density in the lower portion was relatively low and the molded body appeared opaque (white). The casting structure of sample J also became apparent, especially in the sintered molded body, particularly when cut into sheets several millimeters thick. For the measured samples A to G in Table 1, density and porosity distributions were determined, and settling behavior and runoff time were measured on the relevant slurries of the measured samples.

[0137] Measurement of density distribution

[0138] Figure 7 The bar chart shows the density values ​​d (in g / cm³) of the measured samples A to G. 3 (in units), maximum density (d) max (right column), minimum density (d) min (left column) and average density (d av (middle column). The density measurement sample originates from the central longitudinal axis of the corresponding measurement sample, i.e., from the upper volume region, the central volume region, and the lower volume region (based on the orientation of the green body after casting slurry 6b).

[0139] Here, it can be seen that the quartz glass plates A to E, prepared through a wet milling process in the presence of SiO2 nanoparticles, exhibit a relatively small span between their minimum and maximum densities. The maximum span here is approximately 0.21 g / cm³. 3 (For sample D), and the minimum span is 0.11 g / cm. 3 (For samples A and E). This is an indication of the high uniformity of the molded bodies prepared in this manner. However, quartz glass cylinders D and E, with a SiO2 nanoparticle ratio of 10% by weight during wet milling, exhibited relatively lower densities than samples A (1% SiO2 nanoparticles during wet milling) and C (5% SiO2 nanoparticles).

[0140] Quartz glass plate F was prepared without the addition of SiO2 nanoparticles and used as a reference sample. For quartz glass plate G, 1% by weight of SiO2 nanoparticles were added to the homogenizing slurry only after the wet milling process was completed. Quartz glass plates F and G exhibited a large range in density values ​​and therefore low uniformity.

[0141] Figure 2A cross-section along the longitudinal cylindrical axis of the reference sample F is shown. Visually, the surface appears white and matte in the areas at the center 22 and on the lower side 23 of the plate. In contrast, the quartz glass in the area on the top side 21 of the plate is darker, indicating higher density and initial transparency. Reference numeral 24 indicates a cut workpiece not relevant here.

[0142] Measurement of sedimentation trend of slurry

[0143] To this end, 100 ml of slurry 6b was placed in each graduated cylinder, forming a column with a height of 145 mm. After predetermined time intervals, the height of the supernatant above the precipitate was measured using a measuring tape. The height of the precipitate was then calculated.

[0144] Figure 3 The figure shows the results of sedimentation experiments with slurries of different compositions. Sediment height h S Plot the time t (in mm) on the y-axis, and plot it after the start of the experiment. S (In units of h) Plotted on the x-axis.

[0145] This shows that the slurries wet-milled in the presence of SiO2 nanoparticles (samples A, C, and D) exhibit a lower settling tendency than the slurry without added SiO2 nanoparticles (sample F) or the slurry subsequently incorporating the nanoparticles (sample G). This effect becomes particularly significant when the measurement duration is less than three days. Table 2 lists the settling heights 24 hours after the start of the experiment.

[0146] Table 2

[0147]

[0148] This indicates that wet milling in the presence of SiO2 nanoparticles achieves a more stable slurry with a lower settling tendency.

[0149] First, a low settling trend is also important because it depends on the filling level of the casting mold. When casting slurry, the casting time can be several hours, for example, in the range of 24 hours to 60 hours.

[0150] Measurement of slurry viscosity

[0151] To qualitatively measure the viscosity of the slurry, a runoff test was performed. In this case, a stable, homogeneous slurry 6b was placed in the end of a disposable Eppendorf pipette (165 mm), and the time required for 10 ml of slurry to be exhausted was measured electronically through a light barrier. The measurement was performed three times, and the average value was calculated.

[0152] Figure 4The bar chart shows the results of these runoff experiments with different slurry compositions. The runoff time t... A (In seconds) Plotted on the y-axis.

[0153] This shows that the wet-milled slurries (samples A, C, and D) in the presence of SiO2 nanoparticles have a longer runoff time and a correspondingly higher viscosity than the slurry (sample F) without added SiO2 nanoparticles.

[0154] Measurement of pore size distribution

[0155] Figure 5 The bar chart shows the measurement results of the pore sizes / pore diameters distribution in sample A (with 1 wt% SiO2 nanoparticles added during wet milling). The digital H (frequency) is displayed on the y-axis, and the pore diameter d... P Displayed (in μm) on the x-axis, rounded to full micrometers. Maximum distribution is used for pore sizes between 1 μm and 2 μm. Pores with a diameter of 7 μm or larger are not represented.

Claims

1. A method for preparing a molded body made of opaque quartz glass, the method comprising the following steps: (a) Providing SiO2 grains obtained by crushing quartz glass having a purity of at least 99.9% by weight of SiO2. (b) Forming a slurry comprising the suspension and the SiO2 grains and having a total solids content. (c) Wet milling the SiO2 grains in the slurry to form milled SiO2 grain particles. (d) Forming a porous green body from the slurry, comprising the process step of pouring the slurry into a dewatering mold, and (e) Sintering the porous green body to form the molded body of opaque quartz glass. characterized in that The wet milling of the SiO2 grains according to method step (c) is carried out in the presence of SiO2 nanoparticles, at least for a portion of the wet milling step or throughout the entire wet milling step, wherein the proportion of the SiO2 nanoparticles in the total solids content of the slurry is in the range of 0.1 wt% to 10 wt%, and is characterized in that, after the addition of the SiO2 nanoparticles and after the wet milling, the slurry has a solids content in the range of 76 wt% to 79.5 wt%, and wherein at least a portion of the SiO2 nanoparticles in the slurry is added in colloidal form to a specific surface area BET of at least 20 m². 2 The dispersion is in a concentration of / g, and the molded body has a concentration of less than 0.026 g / cm³. 3 The uniformity is defined by the density difference between the maximum and minimum densities.

2. The method of claim 1, wherein, The proportion of SiO2 nanoparticles in the total solids content is in the range of 1% to 2% by weight.

3. The method according to claim 2, characterized in that, The proportion of SiO2 nanoparticles in the total solids content is at most 5% by weight.

4. The method according to any one of claims 1 to 3, characterized in that, The wet milling of the SiO2 grains according to method step (c) is carried out in the presence of SiO2 nanoparticles for at least 1 hour.

5. The method according to any one of claims 1 to 3, characterized in that, The wet milling of the SiO2 grains according to method step (c) is carried out in the presence of SiO2 nanoparticles for at least 10 hours.

6. The method according to any one of claims 1 to 3, characterized in that, The wet milling of the SiO2 grains according to method step (c) is carried out in the presence of SiO2 nanoparticles for at least 120 hours.

7. The method according to any one of claims 1 to 3, characterized in that, After the wet milling, the slurry is cooled under moving conditions for at least 1 hour.

8. The method according to any one of claims 1 to 3, characterized in that, After the wet milling, the slurry is cooled under moving conditions for at least 10 hours.

9. The method according to any one of claims 1 to 3, characterized in that, After the wet milling, the slurry is cooled under moving conditions for at least 30 hours.

10. The method according to any one of claims 1 to 3, characterized in that, After the wet milling, the slurry has Si02 particles having a particle size distribution defined by a D 90 value of less than 15 µm. 50 value of less than 15 µm.

11. The method according to any one of claims 1 to 3, characterized in that, After the addition of the SiO2 nanoparticles and after wet milling, the slurry has a pH in the range of 3 to 5 and a solids content in the range of 77% to 79.5% by weight.

12. The method according to any one of claims 1 to 3, characterized in that, The slurry exhibits sedimentation behavior, characterized in that a column of the slurry with a height of 145 mm forms a precipitate with a height of less than 20 mm after a 24-hour settling time.

13. The method according to any one of claims 1 to 3, characterized in that, The SiO2 grains are obtained by crushing the synthesized transparent quartz glass, wherein the crushing includes electric and / or electro-hydraulic crushing of the transparent quartz glass.

14. The method according to any one of claims 1 to 3, characterized in that, The green blank is dried before sintering, wherein the drying is carried out at a high temperature and includes a drying duration of at least 24 hours.

15. The method according to any one of claims 1 to 3, characterized in that, The surface area of ​​the green blank is removed by machining before sintering, wherein a machining tool with a machining surface made of grains bonded by plastic is used.

16. The method according to claim 15, characterized in that, The surface area of ​​the green blank is removed by sand milling before sintering.

17. The method according to any one of claims 1 to 3, characterized in that, The sintering according to method step (e) is carried out at a sintering temperature in the range of 1325°C to 1600°C.

18. The method according to any one of claims 1 to 3, characterized in that, The sintering according to step (e) is carried out at 1500°C.

19. The method according to any one of claims 1 to 3, characterized in that, The sintering according to step (e) is carried out at 1450°C.

20. A molded body made of opaque porous quartz glass by the method according to any one of claims 1 to 19, wherein the quartz glass has a closed porosity, a chemical purity of at least 99.9% by weight of SiO2, and a density of 2.14 g / cm³. 3 Up to 2.19 g / cm 3 Density within the range, characterized in that, The quartz glass has a homogeneity defined by the fact that the molded body has a first volume region with a maximum density and a second volume region with a minimum density, wherein the density difference between the maximum density and the minimum density is less than 0.026 g / cm3 3 .

21. The molded body according to claim 20, characterized in that, At least 80% of the pores have a diameter of less than 15µm.

22. The molded body according to claim 20, characterized in that, At least 80% of the pores have a diameter of less than 10µm.

23. The molded body according to claim 20, characterized in that, At least 80% of the pores have a diameter of less than 5µm.

Citation Information

Patent Citations

  • Manufacture of opaque quartz glass composite material, used as starting material of permanent shaping-die manufacture of solar silicon melting, involves forming composite slip by mixing quartz glass granules and homogenous base slip

    DE10344189A1

  • Moulding having a high content of silicon dioxide, and process for the production of such mouldings

    DE4338807C1

  • Method of production of a cast part made out of a composite material, as a cast part consisting out of a ceramic or glass composite

    EP1516864A2

  • SiO2 SLURRY FOR THE PRODUCTION OF QUARTZ GLASS AS WELL AS THE APPLICATION OF THE SLURRY

    EP2069244B1

  • Method for producing a coated component of quartz glass or fused silica

    EP2878584A1