Die bonding film and method for producing same, dicing die bonding body film and method for producing same, and method for producing semiconductor device

By using a surface treatment agent to treat silver-containing particles and glutaric acid in the grain bonding film, the heat dissipation of the semiconductor device is improved, the problem of insufficient heat dissipation in the prior art is solved, and efficient heat conduction effect is achieved.

CN119096339APending Publication Date: 2024-12-06RESONAC CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380036859.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-12-22
Filing Date
2023-12-20
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

The thermal dissipation properties of the conventional semiconductor devices are insufficient and there is room for improvement.

Method used

By adding silver-containing particles and glutaric acid treated with a surface treatment agent to the grain bonding film, the thermal conductivity of the grain bonding film is improved, and a semiconductor device with excellent heat dissipation is produced.

Benefits of technology

The heat dissipation of semiconductor devices has been improved. By combining the distribution of high-content silver-containing particles in the grain bonding film and the combination of glutaric acid, the heat conductivity is significantly improved and the demand for efficient heat dissipation is met.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119096339A_ABST
    Figure CN119096339A_ABST
Patent Text Reader

Abstract

The invention discloses a method for manufacturing a die bonding film. The method for producing a crystal grain bonding film comprises: a first step for preparing a raw material varnish containing silver-containing particles produced by a reduction method or silver-containing particles surface-treated by a surface treatment agent, glutaric acid, and an organic solvent; a second step of mixing the raw material varnish to obtain an adhesive varnish; and a third step in which the adhesive varnish is applied to the support film and the organic solvent is removed, thereby obtaining the crystal grain bonding film. The content of the silver-containing particles is 70% by mass or more based on the total solid content of the adhesive varnish.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a die bonding film and a method for manufacturing the same, a dicing die bonding integrated film and a method for manufacturing the same, and a method for manufacturing a semiconductor device. Background Art

[0002] In the past, semiconductor devices were manufactured through the following processes. First, a semiconductor wafer is attached to a pressure-sensitive adhesive sheet for cutting, and in this state, the semiconductor wafer is singulated into semiconductor chips (cutting process). After that, an ultraviolet irradiation process, a picking process, a crimping process, a cutting process, etc. are implemented. Patent document 1 discloses a pressure-sensitive adhesive sheet (cutting die bonding integrated film), which has both the function of fixing the semiconductor wafer in the cutting process and the function of bonding the semiconductor chip to the substrate in the die bonding process. In the cutting process, a chip with an adhesive layer sheet can be obtained by singulating the semiconductor wafer and the adhesive layer.

[0003] In recent years, devices called power semiconductor devices that control power have become popular. Power semiconductor devices easily generate heat due to the current supplied, and require excellent heat dissipation. Patent document 2 discloses a conductive die bonding film having a higher heat dissipation after curing than before curing and a dicing tape with a die bonding film (dicing die bonding integrated film).

[0004] Previous technical literature

[0005] Patent Literature

[0006] Patent Document 1: Japanese Patent Application Publication No. 2008-218571

[0007] Patent Document 2: Japanese Patent No. 6396189 Summary of the invention

[0008] Technical issues to be solved by the invention

[0009] However, the heat dissipation of semiconductor devices manufactured using conventional die bonding films and dicing die bonding integrated films is insufficient and there is still room for improvement.

[0010] Therefore, an object of the present invention is to provide a die bonding film and a dicing-die bonding integrated film capable of manufacturing a semiconductor device having excellent heat dissipation properties.

[0011] Means for solving technical problems

[0012] The present inventors have conducted intensive studies to solve the above problems and have found that the thermal conductivity of a die bonding film can be improved by making the die bonding film contain silver-containing particles surface-treated with a surface treatment agent and glutaric acid, thereby completing the present invention.

[0013] The present invention provides a method for manufacturing a die bonding film as described in [1] to [5], a method for manufacturing a dicing die bonding integrated film as described in [6], a method for manufacturing a semiconductor device as described in [7], the die bonding film as described in [8] to

[10] , and the dicing die bonding integrated film as described in

[11] .

[0014] [1] A method for manufacturing a grain bonding film, comprising: a first step of preparing a raw material varnish containing silver-containing particles manufactured by a reduction method, glutaric acid and an organic solvent; a second step of mixing the raw material varnish to obtain an adhesive varnish; and a third step of applying the adhesive varnish to a supporting film and removing the organic solvent to obtain a grain bonding film, wherein the content of the silver-containing particles is 70% by mass or more based on the total solid content of the adhesive varnish.

[0015] [2] A method for manufacturing a grain bonding film, comprising: a first step of preparing a raw material varnish containing silver-containing particles surface-treated by a surface treatment agent, glutaric acid and an organic solvent; a second step of mixing the raw material varnishes to obtain an adhesive varnish; and a third step of applying the adhesive varnish to a supporting film and removing the organic solvent to obtain a grain bonding film, wherein the content of the silver-containing particles is 70% by mass or more based on the total solid content of the adhesive varnish.

[0016] [3] The method for producing a die bonding film according to [1] or [2], wherein:

[0017] The second step is a step of mixing the raw material varnishes at a temperature of 50° C. or higher.

[0018] [4] The method for producing a die bonding film according to any one of [1] to [3], wherein:

[0019] The raw varnish further contains a thermosetting resin, a curing agent and an elastomer.

[0020] [5] The method for producing a die bonding film according to any one of [1] to [3], wherein:

[0021] The second step is a step of adding a thermosetting resin, a curing agent, and an elastomer to the mixed raw material varnish to obtain an adhesive varnish further containing them.

[0022] [6] A method for manufacturing a die-bonding integrated film, comprising: a process of preparing a dicing tape having a base material layer and a pressure-sensitive adhesive layer disposed on the base material layer; and a process of laminating a die-bonding film manufactured by the method for manufacturing a die-bonding film described in any one of [1] to [5] to the pressure-sensitive adhesive layer of the dicing tape, and forming an adhesive layer formed by the die-bonding film on the pressure-sensitive adhesive layer.

[0023] [7] A method for manufacturing a semiconductor device, comprising: a process of attaching the adhesive layer of a dicing die bonding integrated film manufactured by the method for manufacturing a dicing die bonding integrated film described in [6] to a semiconductor wafer; a process of singulating the semiconductor wafer and the adhesive layer; a process of picking up a semiconductor chip with an adhesive layer sheet from the dicing tape; and a process of bonding the semiconductor chip with an adhesive layer sheet to a supporting component via the adhesive layer sheet.

[0024] [8] A grain bonding film comprising silver-containing particles produced by a reduction method and glutaric acid,

[0025] The content of the silver-containing particles is 70 mass % or more based on the total amount of the grain bonding film.

[0026] [9] The die bonding film according to [8], further comprising a thermosetting resin, a curing agent, and an elastomer.

[0027]

[10] The die bonding film according to [9], wherein

[0028] The thermosetting resin includes an epoxy resin that is liquid at 25°C.

[0029]

[11] A dicing die bonding integrated film comprising:

[0030] A dicing tape comprising a base material layer and a pressure-sensitive adhesive layer disposed on the base material layer; and an adhesive layer disposed on the pressure-sensitive adhesive layer of the dicing tape and formed from the die bonding film described in any one of [8] to

[10] .

[0031] Effects of the Invention

[0032] According to the present invention, a die bonding film and a dicing die bonding integrated film capable of manufacturing a semiconductor device with excellent heat dissipation are provided. Furthermore, according to the present invention, a method for manufacturing them is provided. Furthermore, according to the present invention, a method for manufacturing a semiconductor device using such a dicing die bonding integrated film is provided. BRIEF DESCRIPTION OF THE DRAWINGS

[0033] Figure 1 It is a schematic cross-sectional view showing one embodiment of a die bonding film.

[0034] Figure 2 It is a schematic cross-sectional view showing one embodiment of a dicing die bonding integrated film.

[0035] Figure 3 It is a schematic cross-sectional view showing one embodiment of a method for manufacturing a semiconductor device.

[0036] Figure 3 (a), (b), (c), (d), (e), and (f) are cross-sectional views schematically showing each step.

[0037] Figure 4 It is a schematic cross-sectional view showing one embodiment of a semiconductor device. DETAILED DESCRIPTION

[0038] Hereinafter, the embodiments of the present invention will be described with reference to the accompanying drawings as appropriate. However, the present invention is not limited to the following embodiments. In the following embodiments, except for the cases specifically described, the constituent elements (including steps, etc.) are not essential. The sizes of the constituent elements in each figure are conceptual sizes, and the relative relationship between the sizes of the constituent elements is not limited to the relationship shown in each figure.

[0039] The same is true for the numerical values ​​and their ranges in this specification, and the present invention is not limited thereto. In this specification, the numerical range represented by "~" represents the range in which the numerical values ​​before and after "~" are included as the minimum and maximum values, respectively. In the numerical ranges recorded in stages in this specification, the upper limit or lower limit recorded in one numerical range may also be replaced by the upper limit or lower limit of the numerical range recorded in other stages. Furthermore, in the numerical ranges recorded in this specification, the upper limit or lower limit of the numerical range may also be replaced by the value shown in the embodiments.

[0040] In this specification, "(meth)acrylate" refers to at least one of acrylate and its corresponding methacrylate. The same applies to other similar expressions such as "(meth)acryloyl". Furthermore, "(poly)" refers to both the case with the "poly" prefix and the case without the "poly" prefix. Furthermore, "A or B" may include either A or B, or both. Furthermore, with respect to the materials exemplified below, unless otherwise specified, one type may be used alone, or two or more types may be used in combination. With respect to the content of each component in the composition, when there are multiple substances corresponding to each component in the composition, unless otherwise specified, it refers to the total amount of the multiple substances present in the composition.

[0041] [Die bonding film]

[0042] Figure 1 FIG. 1 is a schematic cross-sectional view of one embodiment of a die bonding film. Figure 1 As shown, Figure 1 The die bonding film 10A shown may be provided on the support film 20. The die bonding film 10A is thermosetting, and can be in a cured state (C stage) after a curing treatment via a semi-cured (B stage) state.

[0043] The grain bonding film 10A contains silver-containing particles (component (a)) produced by a reduction method and glutaric acid (component (b)), and may further contain a thermosetting resin (component (c)), a curing agent (component (d)), and an elastomer (component (e)) as necessary.

[0044] (a) Component: Silver-containing particles produced by a reduction method or silver-containing particles surface-treated (coated) with a surface treatment agent

[0045] Component (a) is a component for improving the thermal conductivity in the grain bonding film and is a component for improving the heat dissipation of the semiconductor device. The silver-containing particles may be, for example, particles composed of silver (particles composed of silver alone, silver particles) or silver-coated metal particles formed by coating the surface of metal particles (copper particles, etc.) with silver. Examples of silver-coated metal particles include silver-coated copper particles, etc. Component (a) may be particles composed of silver (silver particles).

[0046] The component (a) may be silver particles produced by a reduction method (silver particles produced by a liquid phase (wet) reduction method using a reducing agent). In the liquid phase (wet) reduction method using a reducing agent, a surface treatment agent (lubricant) is usually added from the viewpoint of particle size control and prevention of agglomeration and welding, and the surface of the silver particles produced by the liquid phase (wet) reduction method using a reducing agent is treated (coated) with the surface treatment agent (lubricant). That is, the silver particles (silver-containing particles) produced by the reduction method may be silver particles (silver-containing particles) surface-treated (coated) with a surface treatment agent (lubricant). Examples of the surface treatment agent include fatty acid compounds such as oleic acid (melting point: 13.4°C), myristic acid (melting point: 54.4°C), palmitic acid (melting point: 62.9°C), and stearic acid (melting point: 69.9°C); fatty acid amide compounds such as oleic acid amide (melting point: 76°C) and stearic acid amide (melting point: 100°C); fatty alcohol compounds such as amyl alcohol (melting point: -78°C), hexanol (melting point: -51.6°C), oleyl alcohol (melting point: 16°C), and stearyl alcohol (melting point: 59.4°C); and fatty nitrile compounds such as oleanol nitrile (melting point: -1°C). The surface treatment agent may be a surface treatment agent having a low melting point (e.g., a melting point of 100°C or less) and high solubility in an organic solvent, such as a fatty acid compound. That is, component (a) may be silver particles (silver-containing particles) surface-treated (coated) with a fatty acid compound.

[0047] The shape of the component (a) is not particularly limited, and may be, for example, flake, resin, spherical, or spherical. When the component (a) is spherical, a grain bonding film with improved surface roughness (Ra) tends to be easily obtained.

[0048] The average particle size of the component (a) may be 0.01 to 10 μm. When the average particle size of the component (a) is 0.01 μm or more, there is a tendency that the viscosity of the adhesive varnish is prevented from increasing when it is prepared, the die bonding film can contain the desired amount of the component (a), and the wettability of the die bonding film to the adherend can be ensured to exhibit better adhesion. When the average particle size of the component (a) is 10 μm or less, there is a tendency that the film formability is more excellent, and the thermal conductivity can be improved by adding the component (a), and as a result, the heat dissipation of the semiconductor device can be improved. In addition, there is a tendency that by setting it to such a range, the thickness of the die bonding film can be made thinner, and the semiconductor chip can be stacked higher, and cracks in the chip caused by the protrusion of conductive particles from the die bonding film can be prevented. The average particle size of the component (a) may be 0.1 μm or more, 0.5 μm or more, or 1.0 μm or more, and may be 8.0 μm or less, 5.0 μm or less, or 3.0 μm or less.

[0049] In this specification, the average particle size of the component (a) refers to the particle size when the ratio (volume fraction) to the volume of the entire component (a) is 50% (laser 50% particle size (D 50 )). Average particle size (D 50 ) can be determined by measuring a suspension of the component (a) in water using a laser scattering particle size measuring apparatus (e.g., Microtrac) by a laser scattering method.

[0050] Based on the total amount of the grain bonding film (or the total amount of solid content of the adhesive varnish described later), the content of component (a) is 70% by mass or more. Based on the total amount of the grain bonding film, when the content of component (a) is 70% by mass or more, the thermal conductivity of the grain bonding film can be improved, and as a result, the heat dissipation can be improved. Based on the total amount of the grain bonding film, the content of component (a) can be 72% by mass or more, 74% by mass or more, or 75% by mass or more. There is no particular limit to the upper limit of the content of component (a), but based on the total amount of the grain bonding film, it can be 90% by mass or less, 85% by mass or less, or 80% by mass or less. Based on the total amount of the grain bonding film, when the content of component (a) is 90% by mass or less, the grain bonding film can contain other components more fully. As a result, the wettability of the grain bonding film to the adherend can be ensured and better adhesion can be exerted.

[0051] Based on the total amount (total volume) of the grain bonding film, the content of component (a) can be 24.0 volume % or more, 24.5 volume % or more, or 25.0 volume % or more. Based on the total amount (total volume) of the grain bonding film, when the content of component (a) is 24.0 volume % or more, the thermal conductivity of the grain bonding film can be improved, and as a result, the heat dissipation of the semiconductor device can be improved. Based on the total amount (total volume) of the grain bonding film, the content of component (a) can be 33.0 volume % or less, 30.0 volume % or less, or 28.0 volume % or less. Based on the total amount (total volume) of the grain bonding film, when the content of component (a) is 33.0 volume % or less, the grain bonding film can contain other components more fully. As a result, the wettability of the grain bonding film to the adherend can be ensured and better adhesion can be exerted.

[0052] (a) The content (volume %) of the component is, for example, when the density of the die bonding film is set to x (g / cm 3 ), let the density of component (a) be y(g / cm 3 ), when the mass ratio of the component (a) in the grain bonding film is set to z (mass %), it can be calculated by the following formula (I). In addition, the mass ratio of the component (a) in the grain bonding film can be obtained by, for example, performing a thermogravimetric analysis using a thermogravimetric differential thermal analyzer (TG-DTA). In addition, the density of the grain bonding film and the component (a) can be obtained by measuring the mass and specific gravity using a densimeter.

[0053] (a) Content of component (volume %) = (x / y) × z (I)

[0054] TG-DTA measurement conditions: temperature range 30-600°C (heating rate 30°C / min), maintained at 600°C for 20 minutes

[0055] Air flow rate: 300mL / min

[0056] Thermogravimetric differential thermal analysis apparatus: TG / DTA220 manufactured by Seiko Instruments Inc.

[0057] Density meter: EW-300SG manufactured by ALFA MIRAGE CO., LTD.

[0058] (b) Ingredient: Glutaric acid

[0059] The die bonding film 10A contains the component (b). The die bonding film contains the components (a) and (b), thereby increasing the thermal conductivity of the die bonding film, and as a result, increasing the heat dissipation of the semiconductor device.

[0060] When the total amount of component (a) is 100 parts by mass, the content of component (b) can be 0.1 to 5 parts by mass. When the total amount of component (a) is 100 parts by mass, when the content of component (b) is 0.1 parts by mass or more, there is a tendency that the thermal conductivity of the grain bonding film can be further improved. When the total amount of component (a) is 100 parts by mass, when the content of component (b) is 5 parts by mass or less, there is a tendency that the amount of other components (especially, components (c), (d) and (e)) can be sufficiently ensured, and film formation is excellent.

[0061] The content of component (b) may be 0.2 mass % or more, or 0.3 mass % or less, or 3 mass % or less, based on the total amount of the die bonding film (or the total solid content of the adhesive varnish described later).

[0062] (c) Ingredients: Thermosetting resin

[0063] The component (c) is a component that has the property of curing by forming a three-dimensional bond between molecules by heating or the like, and is a component that exhibits an adhesive effect after curing. The component (c) may be an epoxy resin. The component (c) may contain an epoxy resin that is liquid at 25° C. The epoxy resin may be used without particular limitation as long as it is a resin having an epoxy group in the molecule. The epoxy resin may have two or more epoxy groups in the molecule.

[0064] Examples of the epoxy resin include bisphenol A epoxy resin, bisphenol F epoxy resin, bisphenol S epoxy resin, phenol novolac epoxy resin, cresol novolac epoxy resin, bisphenol A novolac epoxy resin, bisphenol F novolac epoxy resin, stilbene epoxy resin, triazine skeleton-containing epoxy resin, fluorene skeleton-containing epoxy resin, trisphenol methane epoxy resin, biphenyl epoxy resin, xylylene epoxy resin, biphenylaralkyl epoxy resin, naphthalene epoxy resin, dicyclopentadiene epoxy resin, polyfunctional phenols, diglycidyl ether compounds of polycyclic aromatics such as anthracene, etc. Among these, the epoxy resin may be a bisphenol epoxy resin or a cresol novolac epoxy resin from the viewpoint of heat resistance of the cured product.

[0065] The epoxy resin may contain an epoxy resin that is liquid at 25°C (hereinafter, sometimes referred to as "liquid epoxy resin"). By containing such a liquid epoxy resin, there is a tendency to easily obtain a die bonding film with improved surface roughness (Ra). Examples of commercially available liquid epoxy resins include EXA-830CRP (product name, manufactured by DIC Corporation) and YDF-8170C (product name, manufactured by NIPPON STEEL Chemical & Material Co., Ltd.).

[0066] The epoxy equivalent of the epoxy resin is not particularly limited and may be 90 to 300 g / eq or 110 to 290 g / eq. When the epoxy equivalent of the epoxy resin is within such a range, the fluidity of the adhesive composition when forming the die bonding film tends to be easily ensured while maintaining the bulk strength of the die bonding film.

[0067] Based on the total amount of the grain bonding film (or the total solid content of the adhesive varnish described later), the content of component (c) can be greater than 1 mass %, greater than 3 mass % or greater than 5 mass %, or less than 15 mass %, less than 12 mass % or less than 10 mass %.

[0068] When component (c) contains a liquid epoxy resin, the mass ratio of the liquid epoxy resin to the total amount of component (c) (mass of the liquid epoxy resin / total mass of component (c)) can be 20% or more, 30% or more, 40% or more, or 100% or less, 90% or less, 80% or less, or 70% or more.

[0069] (d) Ingredient: Curing agent

[0070] (d) component can be a phenolic resin that can become a curing agent for epoxy resin. As long as the phenolic resin is a resin with phenolic hydroxyl group in the molecule, it can be used without particular limitation. As phenolic resin, for example, phenol, cresol, resorcinol, catechol, bisphenol A, bisphenol F, phenylphenol, aminophenol and / or α-naphthol, β-naphthol, dihydroxynaphthalene and other phenols and formaldehyde and other compounds with aldehyde groups are condensed or co-condensed under an acidic catalyst to obtain a novolac type phenol resin, by allylated bisphenol A, allylated bisphenol F, allylated naphthalene diol, phenol novolac, phenol and / or naphthols and dimethoxy-p-xylene or bis (methoxymethyl) biphenyl synthesized phenol aralkyl resin, naphthol aralkyl resin, biphenyl aralkyl type phenol resin, phenyl aralkyl type phenol resin, etc.

[0071] The hydroxyl equivalent of the phenolic resin may be 40 to 300 g / eq, 70 to 290 g / eq, or 100 to 280 g / eq. When the hydroxyl equivalent of the phenolic resin is 40 g / eq or more, the storage modulus of the film tends to be further improved, and when it is 300 g / eq or less, the adverse conditions caused by the generation of foaming, degassing, etc. can be prevented.

[0072] From the viewpoint of curability, the ratio of the epoxy equivalent of the epoxy resin as the component (c) to the hydroxy equivalent of the phenolic resin as the component (d) (epoxy equivalent of the epoxy resin as the component (c) / hydroxy equivalent of the phenolic resin as the component (d)) can be 0.30 / 0.70 to 0.70 / 0.30, 0.35 / 0.65 to 0.65 / 0.35, 0.40 / 0.60 to 0.60 / 0.40 or 0.45 / 0.55 to 0.55 / 0.45. When the equivalent ratio is 0.30 / 0.70 or more, there is a tendency to obtain more sufficient curability. When the equivalent ratio is 0.70 / 0.30 or less, the viscosity can be prevented from becoming too high, and more sufficient fluidity can be obtained.

[0073] Based on the total amount of the grain bonding film (or the total solid content of the adhesive varnish described later), the content of component (d) can be greater than 1 mass %, greater than 3 mass % or greater than 5 mass %, or less than 15 mass %, less than 12 mass % or less than 10 mass %.

[0074] (e) Ingredients: Elastomer

[0075] As (e) component, a polyimide resin, an acrylic resin, a urethane resin, a polyphenylene ether resin, a polyetherimide resin, a phenoxy resin, a modified polyphenylene ether resin etc. are mentioned, for example.

[0076] (e) component is these resins, and may be a resin having a crosslinking functional group, or may be an acrylic resin having a crosslinking functional group. Here, acrylic resin refers to a polymer containing a structural unit derived from (meth)acrylate. Acrylic resin may be a polymer containing a structural unit derived from (meth)acrylate having a crosslinking functional group such as an epoxy group, an alcoholic hydroxyl group or a phenolic hydroxyl group, a carboxyl group, etc. as a structural unit. In addition, acrylic resin may also be an acrylic rubber such as a copolymer of (meth)acrylate and acrylonitrile.

[0077] Examples of commercially available products of acrylic resins include SG-70L, SG-708-6, WS-023EK30, SG-280EK23, HTR-860P-3, HTR-860P-3CSP, and HTR-860P-3CSP-3DB (all manufactured by Nagase ChemteX Corporation).

[0078] The glass transition temperature (Tg) of the component (e) may be -50 to 50°C or -30 to 20°C. When the Tg of the acrylic resin is above -50°C, the viscosity of the die bonding film decreases, and thus the operability tends to be further improved. When the Tg of the acrylic resin is below 50°C, the fluidity of the adhesive composition when forming the die bonding film tends to be more fully ensured. Here, the (Tg) of the component (e) refers to a value measured using a DSC (differential scanning calorimeter) (e.g., manufactured by Rigaku Corporation, product name: Thermo Plus 2).

[0079] The weight average molecular weight (Mw) of the component (e) may be 50,000 to 1.6 million, 100,000 to 1.4 million, or 300,000 to 1.2 million. When the Mw of the component (e) is 50,000 or more, the film-forming property tends to be better. When the Mw of the component (e) is 1.6 million or less, the fluidity of the adhesive composition when forming a grain bonding film tends to be better. In addition, Mw is a value measured by gel permeation chromatography (GPC) and converted using a calibration curve based on standard polystyrene.

[0080] The measuring device and measuring conditions of the Mw of the component (e) are as follows, for example.

[0081] Pump: L-6000 (manufactured by Hitachi, Ltd.)

[0082] Column: A column made by connecting Gelpack GL-R440 (manufactured by Resonac Holdings Corporation.), Gelpack GL-R450 (manufactured by Resonac Holdings Corporation.), and Gelpack GL-R400M (manufactured by Resonac Holdings Corporation.) (each 10.7 mm (diameter) × 300 mm) in this order

[0083] Eluent: Tetrahydrofuran (hereinafter referred to as "THF")

[0084] Sample: 120 mg of the sample dissolved in 5 mL of THF

[0085] Flow rate: 1.75mL / min

[0086] Based on the total amount of the grain bonding film (or the total solid content of the adhesive varnish described later), the content of component (e) can be greater than 1 mass %, greater than 3 mass % or greater than 5 mass %, or less than 15 mass %, less than 12 mass % or less than 10 mass %.

[0087] (f) Ingredient: Curing accelerator

[0088] The grain bonding film 10A may further contain a curing accelerator (component (f)). The grain bonding film contains component (f), thereby having a tendency to be able to take into account both adhesion and connection reliability. Examples of component (f) include imidazoles and their derivatives, organic phosphorus compounds, secondary amines, tertiary amines, quaternary ammonium salts, and the like. Among these, component (f) may be imidazoles and their derivatives from the viewpoint of reactivity.

[0089] Examples of the imidazoles include 2-methylimidazole, 1-benzyl-2-methylimidazole, 1-cyanoethyl-2-phenylimidazole, and 1-cyanoethyl-2-methylimidazole.

[0090] The content of component (f) may be 0.001 to 1 mass % based on the total amount of the die bonding film (or the total solid content of the adhesive varnish described later). When the content of component (f) is within such a range, both adhesion and connection reliability tend to be achieved.

[0091] The die bonding film 10A may further contain a coupling agent, an antioxidant, a rheology control agent, a leveling agent, etc. as other components other than components (a) to (f). Examples of the coupling agent include 3-ureidopropyltriethoxysilane, 3-mercaptopropyltrimethoxysilane, 3-phenylaminopropyltrimethoxysilane, and 3-(2-aminoethyl)aminopropyltrimethoxysilane. The content of the other components may be 0.01 to 3% by mass based on the total amount of the die bonding film.

[0092] [Method for manufacturing die bonding film]

[0093] Figure 1 The grain bonding film 10A shown can be obtained by a method comprising the following steps, namely, a first step of preparing a raw material varnish containing component (a) (silver-containing particles manufactured by a reduction method or silver-containing particles surface-treated by a surface treatment agent), component (b) and an organic solvent; a second step of mixing the raw material varnishes to obtain an adhesive varnish; and a third step of applying the adhesive varnish to a supporting film and removing the organic solvent to obtain a grain bonding film.

[0094] The first step is a step of preparing a raw material varnish containing the component (a) (silver-containing particles produced by a reduction method or silver-containing particles surface-treated with a surface treatment agent), the component (b) and an organic solvent.

[0095] The organic solvent is not particularly limited as long as it can dissolve the components other than component (a). As the organic solvent, for example, aromatic hydrocarbons such as toluene, xylene, mesitylene, cumene, and p-isopropylbenzene can be cited; aliphatic hydrocarbons such as hexane and heptane; cycloalkanes such as methylcyclohexane; cyclic ethers such as tetrahydrofuran and 1,4-dioxane; ketones such as acetone, methyl ethyl ketone, methyl isobutyl ketone, cyclohexanone, and 4-hydroxy-4-methyl-2-pentanone; esters such as methyl acetate, ethyl acetate, butyl acetate, methyl lactate, ethyl lactate, and γ-butyrolactone; carbonates such as ethylene carbonate and propylene carbonate; amides such as N,N-dimethylformamide, N,N-dimethylacetamide, and N-methyl-2-pyrrolidone. Among these, from the viewpoint of solubility and boiling point, the organic solvent can be toluene, xylene, methyl ethyl ketone, methyl isobutyl ketone, or cyclohexanone. The solid content concentration in the raw material varnish may be 10 to 80% by mass based on the total amount of the raw material varnish.

[0096] The raw material varnish can be obtained by, for example, adding each component to a container used in a stirrer. In this case, the order of adding each component is not particularly limited and can be appropriately set according to the properties of each component.

[0097] The second step is a step of mixing the raw material varnishes to obtain an adhesive varnish.

[0098] Mixing can be carried out by appropriately combining a homodispersor, a three-in-one motor, a stirrer, a planetary mixer, a pounding machine, or other common mixers. The mixer may also be equipped with a heating device such as a heater unit that can manage the temperature conditions of the raw material varnish (or adhesive varnish). When a homodispersor is used for mixing, the rotation speed of the homodispersor may be 4000 revolutions per minute or more.

[0099] The second step may be a step of mixing the raw material varnishes at a temperature of 50°C or above. The mixing temperature can be adjusted as needed using a heating device, a heat-insulating device, etc. When the mixing temperature is 50°C or above, for example, the resulting grain bonding film is in a cured state (C stage) after the curing treatment, and it is easy to form a sintered body of the (a) component, which can further improve the thermal conductivity of the grain bonding film. The mixing temperature may also be above 55°C, above 60°C, above 65°C, or above 70°C. The upper limit of the mixing temperature may be, for example, below 120°C, below 110°C, below 100°C, below 90°C, or below 80°C. The mixing time may be, for example, above 1 minute, above 5 minutes, above 10 minutes, or above 20 minutes, or may be below 80 minutes, below 60 minutes, or below 40 minutes.

[0100] The components (c), (d), (e), (f) and other components can be contained in the raw material varnish or the adhesive varnish independently at any stage according to the properties of each component. For example, in the first step, a raw material varnish further containing these components is prepared, and in the second step, the raw material varnishes can be mixed to obtain an adhesive varnish containing the components (a), (b), (c), (d), (e), (f) and other components. Also, for example, in the first step, a raw material varnish is prepared, and in the second step, the raw material varnishes can be mixed, and these components are added to the mixed raw material varnish, thereby obtaining an adhesive varnish containing the components (a), (b), (c), (d), (e), (f) and other components. Furthermore, for example, in the first step, a raw material varnish further containing components (c) and (d) is prepared, and in the second step, the raw material varnishes can be mixed to obtain an adhesive varnish containing components (a), (b), (c), (d), (e), (f) and other components by adding components (e), (f) and other components to the mixed raw material varnish. In the second step, when at least one component selected from the group consisting of components (c), (d), (e), (f) and other components is added to the mixed raw material varnish, after the addition of the component, mixing can be performed, for example, at a temperature condition lower than 50° C. (for example, room temperature (25° C.)). The mixing condition at this time can be at room temperature (25° C.) for 0.1 to 48 hours.

[0101] In this way, an adhesive varnish containing predetermined components can be obtained. The obtained adhesive varnish may be subjected to vacuum degassing or the like to remove air bubbles in the varnish.

[0102] The content of the silver-containing particles is 70% by mass or more based on the total solid content of the adhesive varnish. In this specification, the solid content of the adhesive varnish refers to the total amount of components other than the organic solvent.

[0103] The third step is a step of applying an adhesive varnish to the support film 20 and removing the organic solvent to obtain the die bonding film 10A.

[0104] The supporting film 20 is not particularly limited, and examples thereof include films of polytetrafluoroethylene, polyethylene, polypropylene, polymethylpentene, polyethylene terephthalate, polyimide, etc. The supporting film may be subjected to a demolding treatment. The thickness of the supporting film 20 may be, for example, 10 to 200 μm or 20 to 170 μm.

[0105] As a method for applying the adhesive varnish to the support film 20 , a known method can be used, and examples thereof include a knife coating method, a roll coating method, a spray coating method, a gravure coating method, a bar coating method, and a curtain coating method.

[0106] The organic solvent after the adhesive varnish is applied to the support film can be removed by heat drying. The heat drying is not particularly limited as long as the organic solvent used is fully volatilized. For example, the heat drying temperature can be 50 to 200° C. and the heat drying time can be 0.1 to 30 minutes. The heat drying can also be performed in stages at different heat drying temperatures or heat drying times.

[0107] The thickness of the die bonding film 10A can be appropriately adjusted according to the application, for example, it can be 3 to 200 μm. When the thickness of the die bonding film 10A is 3 μm or more, there is a tendency that the bonding strength with the semiconductor wafer becomes sufficient, and when it is 200 μm or less, there is a tendency that the thermal conductivity becomes sufficient. From the perspective of bonding strength and thinning of semiconductor devices, the thickness of the die bonding film 10A can be 5 to 100 μm or 10 to 50 μm.

[0108] The thermal conductivity (25°C±1°C) of the die bonding film 10A after heat curing at 170°C for 3 hours (C-stage state) can be 4.0 W / m·K or more. When the thermal conductivity is 4.0 W / m·K or more, there is a tendency that the heat dissipation of the semiconductor device is better. The thermal conductivity can be 4.5 W / m·K or more, 5.0 W / m·K or more, 5.5 W / m·K or more, or 6.0 W / m·K or more. The upper limit of the thermal conductivity (25°C±1°C) of the die bonding film 10A in the C-stage state is not particularly limited and can be 30 W / m·K or less.

[0109] The thermal conductivity (25°C±1°C) of the grain bonding film 10A after heat curing at 170°C for 3 hours (C stage state) can be measured, for example, by the following method. First, the grain bonding film is cut into a specified size, and a specified number of film sheets are prepared in such a way that the thickness becomes 200μm when stacked. For example, in the case of using a grain bonding film with a thickness of 25μm, 8 film sheets are prepared. In the case of using a grain bonding film with a thickness of 10μm, 20 film sheets are prepared. These film sheets are laminated on a hot plate at 70°C using a rubber roller to prepare a laminate with a thickness of 200μm. Next, a sample in the C stage state is obtained by heat curing each laminate at 170°C for 3 hours in a clean oven (manufactured by ESPEC Corp.). The obtained sample is cut into 1cm×1cm, used as a film for thermal conductivity measurement, and the thermal conductivity is measured under the following measurement items / conditions.

[0110] (Calculation of thermal conductivity)

[0111] The thermal conductivity λ in the thickness direction of the film for measuring thermal conductivity was calculated by the following formula.

[0112] Thermal conductivity λ(W / m·K)=thermal diffusivity α(m 2 / s)×specific heat Cp(J / kg·K)×density ρ(g / cm 3 )

[0113] The thermal diffusivity α, the specific heat Cp, and the density ρ were measured by the following method. A larger thermal conductivity λ means that the heat dissipation in the semiconductor device is more excellent.

[0114] (Measurement of Thermal Diffusivity α)

[0115] The thermal conductivity film was blackened on both sides by graphite spraying to prepare a measurement sample. The thermal diffusivity α of the thermal conductivity film was determined by a laser flash method (xenon flash method) using the following measurement apparatus under the following conditions.

[0116] ·Measurement device: Thermal diffusivity measurement device (manufactured by NETZSCH Japan KK, product name: LFA447 nanoflash)

[0117] Pulse width of pulse light irradiation: 0.1ms

[0118] · Applied voltage for pulse light irradiation: 236V

[0119] · Sample treatment: Both sides of the thermal conductivity measurement film were blackened with graphite spray.

[0120] ·Measurement atmosphere temperature: 25℃±1℃

[0121] (Measurement of specific heat Cp (25°C))

[0122] The specific heat Cp (25° C.) of the film for measuring thermal conductivity can be determined, for example, by performing differential scanning calorimetry (DSC) under the following conditions using the following measuring apparatus.

[0123] · Measurement device: Differential scanning calorimeter (manufactured by PerkinElmer Japan Co., Ltd., product name: Pyris1)

[0124] · Reference material: sapphire

[0125] Heating rate: 10℃ / min

[0126] Heating temperature range: room temperature (25℃) ~ 60℃

[0127] (Determination of density ρ)

[0128] The density ρ of the film for measuring thermal conductivity is measured by the Archimedean method under the following conditions using the following measuring apparatus, for example.

[0129] ·Measurement device: Electronic density meter (manufactured by ALFA MIRAGE CO., LTD., product name: SD200L)

[0130] Water temperature: 25℃

[0131] The die bonding film contains components (a) and (b), thereby improving thermal conductivity, and as a result, improving heat dissipation of the semiconductor device. Therefore, the die bonding film can be combined with a dicing film having a pressure-sensitive adhesive layer and can be suitably used as a dicing die bonding integrated film.

[0132] [Dicing and Die Bonding Integrated Film]

[0133] Figure 2 It is a schematic cross-sectional view showing one embodiment of a dicing die bonding integrated film. Figure 2 The dicing die bonding integrated film 100 shown includes: a dicing tape 50 (dicing film) including a base material layer 40 and a pressure-sensitive adhesive layer 30 provided on the base material layer 40; and an adhesive layer 10 formed by a die bonding film 10A provided on the pressure-sensitive adhesive layer 30 of the dicing tape 50. The dicing die bonding integrated film 100 may also be in the form of a film, a sheet, a tape, etc. The dicing die bonding integrated film 100 may include a support film 20 on the surface of the adhesive layer 10 on the side opposite to the pressure-sensitive adhesive layer 30.

[0134] As the base material layer 40 on the dicing tape 50, for example, plastic films such as polytetrafluoroethylene film, polyethylene terephthalate film, polyethylene film, polypropylene film, polymethylpentene film, polyimide film, etc. can be cited. In addition, the base material layer 40 can also be subjected to surface treatments such as primer coating, UV treatment, corona discharge treatment, grinding treatment, and etching treatment as needed.

[0135] The pressure-sensitive adhesive layer 30 on the dicing tape 50 is not particularly limited as long as it has sufficient adhesive strength to prevent the semiconductor chips from flying during dicing and has low adhesive strength to the extent that the semiconductor chips are not damaged in the subsequent pickup process of the semiconductor chips. The dicing tape previously known in the field of dicing tapes can be used. The pressure-sensitive adhesive layer 30 can be a pressure-sensitive adhesive layer formed by a non-ultraviolet curing pressure-sensitive adhesive (pressure-sensitive adhesive), or a pressure-sensitive adhesive layer formed by an ultraviolet curing pressure-sensitive adhesive. In the case where the pressure-sensitive adhesive layer is a pressure-sensitive adhesive layer formed by an ultraviolet curing pressure-sensitive adhesive, the adhesiveness of the pressure-sensitive adhesive layer can be reduced by irradiating ultraviolet rays.

[0136] From the viewpoint of economic efficiency and film handling properties, the thickness of the dicing tape 50 (the base material layer 40 and the pressure-sensitive adhesive layer 30 ) may be 60 to 150 μm or 70 to 130 μm.

[0137] Figure 2 The dicing die bonding integrated film 100 shown can be obtained by a manufacturing method including the steps of preparing a die bonding film 10A, preparing a dicing tape 50 including a base material layer 40 and a pressure-sensitive adhesive layer 30 provided on the base material layer 40, and bonding the die bonding film 10A and the pressure-sensitive adhesive layer 30 of the dicing tape 50. As a method of bonding the die bonding film 10A and the pressure-sensitive adhesive layer 30 of the dicing tape 50, a known method can be used.

[0138] [Semiconductor device and method of manufacturing the same]

[0139] Figure 3 It is a schematic cross-sectional view showing one embodiment of a method for manufacturing a semiconductor device. Figure 3 (a), (b), (c), (d), (e) and (f) are cross-sectional views schematically showing the respective steps. The method for manufacturing a semiconductor device comprises: a step of attaching a semiconductor wafer W to the adhesive layer 10 of the dicing die bonding integrated film 100 (wafer lamination step, see Figure 3 (a), (b)); the process of singulating the semiconductor wafer W and the adhesive layer 10 (cutting process, reference Figure 3 (c)); as needed, the pressure-sensitive adhesive layer 30 (through the substrate layer 40) irradiated with ultraviolet light step (ultraviolet irradiation step, reference Figure 3 (d)); a process of picking up the semiconductor chip 60 with the adhesive layer sheet from the dicing tape 50 (the pressure-sensitive adhesive layer 30) (pick-up process, reference Figure 3 (e)); a step of bonding the semiconductor chip 60 with the adhesive layer to the supporting member 80 via the adhesive layer 10a (semiconductor chip bonding step, reference Figure 3 and, if necessary, a step of thermally curing the adhesive layer sheet 10a of the semiconductor chip 60 with the adhesive layer sheet bonded to the support member 80 (thermal curing step).

[0140] (Wafer Lamination Process)

[0141] In this process, first, the dicing die bonding integrated film 100 is placed in a predetermined device. Next, the surface Ws of the semiconductor wafer W is attached to the adhesive layer 10 of the dicing die bonding integrated film 100 (see FIG. 1 ). Figure 3 (a) and (b)). The circuit surface of the semiconductor wafer W may also be provided on the surface opposite to the surface Ws.

[0142] Examples of the semiconductor wafer W include single crystal silicon, polycrystalline silicon, various ceramics, and compound semiconductors such as gallium arsenide.

[0143] <Cutting process>

[0144] In this process, the semiconductor wafer W and the adhesive layer 10 are cut into individual pieces (see Figure 3 (c)). At this time, a part of the pressure-sensitive adhesive layer 30 or the entire pressure-sensitive adhesive layer 30 and a part of the base layer 40 may be cut into individual pieces. Thus, the dicing die-bonding integrated film 100 also functions as a dicing piece.

[0145] <Ultraviolet irradiation process>

[0146] When the pressure-sensitive adhesive layer 30 is a pressure-sensitive adhesive layer formed of an ultraviolet curable pressure-sensitive adhesive, the method for manufacturing a semiconductor device may also include an ultraviolet irradiation step. In this step, the pressure-sensitive adhesive layer 30 (via the substrate layer 40) is irradiated with ultraviolet rays (see Figure 3 (d)). In the ultraviolet irradiation, the wavelength of the ultraviolet rays may be 200 to 400 nm. In the ultraviolet irradiation conditions, the illumination and the irradiation amount may be 30 to 240 mW / cm 2 The range is 50~500mJ / cm 2 range.

[0147] (Picking process)

[0148] In this step, the semiconductor chips 60 with adhesive layers that have been singulated are separated from each other by expanding the base layer 40, and the semiconductor chips 60 with adhesive layers that are lifted by the needles 72 are sucked from the base layer 40 side by the suction chuck 74 and picked up from the pressure-sensitive adhesive layer 30a (see FIG. Figure 3 (e)). In addition, the semiconductor chip 60 with an adhesive layer sheet has a semiconductor chip Wa and an adhesive layer sheet 10a. The semiconductor chip Wa is a chip formed by singulating the semiconductor wafer W, and the adhesive layer sheet 10a is a sheet formed by singulating the adhesive layer 10. In addition, the pressure-sensitive adhesive layer 30a is a layer formed by singulating the pressure-sensitive adhesive layer 30. The pressure-sensitive adhesive layer 30a can remain on the base layer 40 after picking up the semiconductor chip 60 with an adhesive layer sheet. In this process, it is not necessarily necessary to expand the base layer 40, but the pick-up property can be further improved by expanding the base layer 40.

[0149] The push-up amount of the needle 72 can be set appropriately. Furthermore, from the perspective of ensuring sufficient pickup performance even for ultra-thin wafers, for example, two or three stages of push-up can be performed. In addition, the semiconductor chip 60 with the adhesive layer can be picked up by a method other than the method using the suction chuck 74.

[0150] <Semiconductor chip bonding process>

[0151] In this step, the picked-up semiconductor chip 60 with the adhesive layer sheet is bonded to the supporting member 80 (see FIG. 1 ) via the adhesive layer sheet 10a by thermal compression bonding. Figure 3 (f)) A plurality of semiconductor chips 60 with adhesive layers may be bonded to the support member 80 .

[0152] The heating temperature in the thermocompression bonding may be, for example, 80 to 160° C. The load in the thermocompression bonding may be, for example, 5 to 15 N. The heating time in the thermocompression bonding may be, for example, 0.5 to 20 seconds.

[0153] <Thermosetting process>

[0154] In this process, the adhesive layer 10a in the semiconductor chip 60 with an adhesive layer bonded to the supporting member 80 is thermally cured. By (further) thermally curing the adhesive layer 10a or the cured product 10ac of the adhesive layer that bonds the semiconductor chip Wa to the supporting member 80, the semiconductor chip Wa can be more firmly bonded and fixed. In addition, when the component (a) is silver particles (preferably silver particles produced by a reduction method), the adhesive layer 10a or the cured product 10ac of the adhesive layer is (further) thermally cured, thereby having a tendency to more easily become a sintered body of the silver particles. In the case of thermal curing, pressure can also be applied simultaneously to cure it. The heating temperature in this process can be appropriately changed according to the constituent components of the adhesive layer 10a. The heating temperature can be, for example, 60 to 200°C, 90 to 190°C, or 120 to 180°C. The heating time can be 30 minutes to 5 hours, 1 to 3 hours, or 2 to 3 hours. Alternatively, the temperature or pressure may be changed stepwise.

[0155] The adhesive layer sheet 10a can be cured by a semiconductor chip bonding process or a thermal curing process to become a cured adhesive layer sheet 10ac. When the component (a) is silver particles (preferably silver particles produced by a reduction method), the cured adhesive layer sheet 10ac can contain a silver particle sintered body. Therefore, the obtained semiconductor device can have excellent heat dissipation.

[0156] The method for manufacturing a semiconductor device may also include, as needed, a step of electrically connecting the end of the terminal portion (internal lead) of the support component to the electrode pad on the semiconductor chip using a bonding wire (wire bonding step). As the bonding wire, for example, gold wire, aluminum wire, copper wire, etc. are used. The temperature during wire bonding may be in the range of 80 to 250°C or 80 to 220°C. The heating time may be from several seconds to several minutes. Wire bonding may also be performed by using both ultrasonic vibration energy and pressure-applied compression energy while heating within the above-mentioned temperature range.

[0157] The method for manufacturing a semiconductor device may also include a process (sealing process) of sealing a semiconductor chip with a sealing material as required. This process is performed to protect a semiconductor chip or a bonding wire mounted on a supporting member. This process can be performed by forming a sealing resin (sealing resin) with a mold. As a sealing resin, for example, an epoxy resin can be used. By burying the supporting member and the residue by heat and pressure during sealing, peeling caused by bubbles in the bonding interface can be prevented.

[0158] The method for manufacturing a semiconductor device may also include a step (post-curing step) of completely curing the sealing resin that is not fully cured in the sealing step as needed. In the sealing step, even if the adhesive layer is not thermally cured, in this step, the adhesive layer can be thermally cured while curing the sealing resin to bond and fix. The heating temperature in this step can be appropriately set according to the type of sealing resin, for example, it can be in the range of 165 to 185° C., and the heating time can be about 0.5 to 8 hours.

[0159] The method for manufacturing a semiconductor device may also include, as needed, a step of heating a semiconductor chip with an adhesive layer bonded to a supporting member using a reflow furnace (heating and melting step). In this step, the resin-sealed semiconductor device may also be surface-mounted on the supporting member. As a surface mounting method, for example, solder may be supplied to a printed wiring board in advance, and then heated and melted by warm air or the like, and then reflowed. As a heating method, for example, hot air reflow, infrared reflow, etc. may be mentioned. Furthermore, the heating method may heat the entire device or may heat a part of the device. The heating temperature may be, for example, in the range of 240 to 280°C.

[0160] Figure 4 It is a schematic cross-sectional view showing one embodiment of a semiconductor device. Figure 4 The semiconductor device 200 shown includes a semiconductor chip Wa, a supporting member 80 on which the semiconductor chip Wa is mounted, and an adhesive member 12. The adhesive member 12 is disposed between the semiconductor chip Wa and the supporting member 80 to bond the semiconductor chip Wa to the supporting member 80. The adhesive member 12 is a cured product of a grain bonding film (cured product 10ac of an adhesive layer sheet). The connection terminal (not shown) of the semiconductor chip Wa can also be electrically connected to an external connection terminal (not shown) via a wire 70. The semiconductor chip Wa can also be sealed by a sealing material layer 92 formed by a sealing material. Solder balls 94 can also be formed on the surface opposite to the surface 80A of the supporting member 80 for electrical connection to an external substrate (motherboard) (not shown).

[0161] The semiconductor chip Wa may be, for example, an IC (integrated circuit), etc. As the supporting member 80, for example, lead frames such as 42 alloy lead frames and copper lead frames; plastic films such as polyimide resins and epoxy resins; modified plastic films obtained by impregnating and curing plastics such as polyimide resins and epoxy resins in glass nonwoven fabrics, etc.; ceramics such as alumina, etc. may be cited.

[0162] The semiconductor device 200 includes the cured product of the die bonding film as an adhesive member, and thus has excellent heat dissipation properties.

[0163] Example

[0164] Hereinafter, the present invention will be specifically described based on Examples, but the present invention is not limited to these.

[0165] (Reference Example 1, Examples 1 to 3, and Comparative Examples 1 to 7)

[0166] [Fabrication of Die-bonding Film]

[0167] <Preparation of adhesive varnish>

[0168] A mixed varnish was prepared by adding cyclohexanone as an organic solvent to the components (a), (b) or (b'), (c), (d) and (e) according to the symbols and composition ratios shown in Tables 1 and 2 (unit: parts by mass). The mixed varnish was stirred at 4000 rpm for 20 minutes at a mixing temperature of 70°C using a homodispersor (manufactured by Tajima Chemical Machinery Co., Ltd., TKHOMO MIXER MARK II). Next, the mixed varnish was placed at 20 to 30°C, and then the components (f) and (g) were added to the mixed varnish, and stirred overnight at 250 rpm using a three-in-one motor. Thus, adhesive varnishes of Reference Example 1, Examples 1 to 3, and Comparative Examples 1 to 7 were prepared in which the total content of components (a), (b) or (b'), (c), (d), (e), (f), and (g) was 61 to 62 mass %.

[0169] The symbols for the components in Tables 1 and 2 are as follows.

[0170] (a) Component: Silver-containing particles produced by a reduction method (silver-containing particles surface-treated (coated) with a surface treatment agent)

[0171] (a-1) Silver particles AG-3-1F (product name, manufactured by DOWA Electronics Materials Co., Ltd., shape: spherical, average particle size (laser 50% particle size (D 50 )):1.4μm)

[0172] Component (b) or component (b'):

[0173] (b-1) Glutaric acid

[0174] (b'-1) Suberic acid

[0175] (b'-2) Azelaic acid

[0176] (b'-3) Propionic acid

[0177] (b'-4) Oxalic acid

[0178] (b'-5)malonic acid

[0179] (b'-6)Maleic acid

[0180] (b'-7) Adipic acid

[0181] (c) Ingredients: Thermosetting resin

[0182] (c-1) N-500P-10 (product name, manufactured by DIC Corporation, cresol novolac type epoxy resin, epoxy equivalent: 204 g / eq, softening point: 84° C.)

[0183] (c-2) EXA-830CRP (product name, manufactured by DIC Corporation, bisphenol F type epoxy resin, epoxy equivalent: 159 g / eq, liquid at 25°C)

[0184] (d) Ingredient: Curing agent

[0185] (d-1) MEH-7800M (product name, manufactured by MEIWA KAGAKU KOUGYOU CO., LTD., phenyl aralkyl type phenol resin, hydroxyl equivalent: 174 g / eq, softening point: 80° C.)

[0186] (e) Ingredients: Elastomer

[0187] (e-1) HTR-860P-3CSP (product name, manufactured by Nagase ChemteX Corporation, acrylic rubber, weight average molecular weight: 800,000, Tg: -7°C)

[0188] (f) Component: Curing accelerator

[0189] (f-1) 1B2MZ (product name, manufactured by SHIKOKU CHEMICALS CORPORATION, 1-benzyl-2-methylimidazole)

[0190] (g) Ingredient: coupling agent

[0191] (g-1) Z-6119 (product name, manufactured by Dow Toray Co., Ltd., 3-ureidopropyltriethoxysilane)

[0192] <Production of Die-bonding Film>

[0193] A grain bonding film was prepared using each of the above-mentioned adhesive varnishes. Each adhesive varnish was subjected to vacuum degassing, and the subsequent adhesive varnish was applied to a polyethylene terephthalate (PET) film (thickness: 38 μm) that had been subjected to a demolding treatment as a supporting film. The applied adhesive varnish was heated and dried in two stages at different temperatures, at 90°C for 5 minutes and then at 130°C for 5 minutes, thereby obtaining a grain bonding film of Reference Example 1, Examples 1 to 3, and Comparative Examples 1 to 7 with a thickness of 25 μm in a B-stage state on the supporting film.

[0194] <Calculation of volume %>

[0195] (a) The content (volume %) of the component is set to x (g / cm 3 ), let the density of component (a) be y(g / cm 3 ), when the mass ratio of the component (a) in the grain bonding film is set to z (mass %), it is calculated by the following formula (I). In addition, the mass ratio of the component (a) in the grain bonding film is obtained by thermogravimetric analysis using a thermogravimetric differential thermal analyzer (TG-DTA). In addition, the density of the grain bonding film and the component (a) is obtained by measuring the mass and specific gravity using a densimeter.

[0196] (a) Content of component (volume %) = (x / y) × z (I)

[0197] TG-DTA measurement conditions: temperature range 30-600°C (heating rate 30°C / min), maintained at 600°C for 20 minutes

[0198] Air flow rate: 300mL / min

[0199] Thermogravimetric differential thermal analysis apparatus: TG / DTA220 manufactured by Seiko Instruments Inc.

[0200] Density meter: EW-300SG manufactured by ALFA MIRAGE CO., LTD.

[0201] [Evaluation of Die-bonding Film (Measurement of Thermal Conductivity)]

[0202] (Preparation of Film for Measurement of Thermal Conductivity)

[0203] The grain bonding film was cut into a specified size, and 8 film sheets were prepared in the grain bonding film (thickness: 25 μm) of Reference Example 1, Examples 1 to 3, and Comparative Examples 1 to 7. Next, a laminate having a thickness of 200 μm was prepared by laminating these film sheets on a hot plate at 70°C using a rubber roller. Next, each laminate was thermally cured at 170°C for 3 hours in a clean oven (manufactured by ESPEC Corp.) to obtain a sample in a C stage state. The prepared sample was cut into 1 cm×1 cm pieces, used as a film for measuring thermal conductivity, and the thermal conductivity was measured under the following measurement items / conditions. The results are shown in Tables 1 and 2.

[0204] (Calculation of thermal conductivity)

[0205] The thermal conductivity λ in the thickness direction of the film for measuring thermal conductivity was calculated by the following formula.

[0206] Thermal conductivity λ(W / m·K)=thermal diffusivity α(m 2 / s)×specific heat Cp(J / kg·K)×density ρ(g / cm 3 )

[0207] The thermal diffusivity α, the specific heat Cp, and the density ρ were measured by the following method. A larger thermal conductivity λ means that the heat dissipation in the semiconductor device is more excellent.

[0208] (Measurement of Thermal Diffusivity α)

[0209] The thermal conductivity film was blackened on both sides by graphite spraying to prepare a measurement sample. The thermal diffusivity α of the thermal conductivity film was determined by the laser flash method (xenon flash method) under the following conditions using the following measurement apparatus.

[0210] ·Measurement device: Thermal diffusivity measurement device (manufactured by NETZSCH Japan KK, product name: LFA447 nanoflash)

[0211] Pulse width of pulse light irradiation: 0.1ms

[0212] · Applied voltage for pulse light irradiation: 236V

[0213] · Sample treatment: Both sides of the thermal conductivity measurement film were blackened with graphite spray.

[0214] ·Measurement atmosphere temperature: 25℃±1℃

[0215] (Measurement of specific heat Cp (25°C))

[0216] The specific heat Cp (25° C.) of the film for measuring thermal conductivity was determined by performing differential scanning calorimetry (DSC) under the following conditions using the following measuring apparatus.

[0217] · Measurement device: Differential scanning calorimeter (manufactured by PerkinElmer Japan Co., Ltd., product name: Pyris1)

[0218] · Reference material: sapphire

[0219] Heating rate: 10℃ / min

[0220] Heating temperature range: room temperature (25℃) ~ 60℃

[0221] (Determination of density ρ)

[0222] The density ρ of the film for measuring thermal conductivity was measured by the Archimedean method under the following conditions using the following measuring apparatus.

[0223] ·Measurement device: Electronic density meter (manufactured by ALFA MIRAGE CO., LTD., product name: SD200L)

[0224] Water temperature: 25℃

[0225] [Table 1]

[0226]

[0227]

[0228] As shown in Table 1, the die bonding films containing glutaric acid of Examples 1 to 3 are superior in thermal conductivity compared to the die bonding film containing no glutaric acid (other acids) of Reference Example 1. Furthermore, as shown in Table 2, the die bonding films containing various acids of Comparative Examples 1 to 7 are insufficient in thermal conductivity compared to the die bonding film of Reference Example 1, and it is clear that the effect of improving the thermal conductivity is a specific effect that appears when glutaric acid is used. From the above, it can be confirmed that the dicing die bonding integrated film of the present invention can manufacture a semiconductor device with excellent heat dissipation.

[0229] Explanation of symbols

[0230] 10-adhesive layer, 10A-die bonding film, 10a-adhesive layer sheet, 10ac-cured product of adhesive layer sheet, 12-adhesive component, 20-support film, 30, 30a-pressure-sensitive adhesive layer, 40-base material layer, 50-dicing tape, 60-semiconductor chip with adhesive layer sheet, 70-wire, 72-needle, 74-suction chuck, 80-support component, 92-sealing material layer, 94-solder ball, 100-dicing die bonding integrated film, 200-semiconductor device, W-semiconductor wafer, Wa-semiconductor chip.

Claims

1. A method for manufacturing a die bonding film, comprising: In the first step, a raw material varnish containing silver particles produced by a reduction method, glutaric acid and an organic solvent is prepared; In the second step, the raw material varnishes are mixed to obtain an adhesive varnish; and In a third step, the adhesive varnish is applied to a support film and the organic solvent is removed to obtain a die bonding film. The content of the silver-containing particles is 70% by mass or more based on the total solid content of the adhesive varnish.

2. A method for manufacturing a die bonding film, comprising: In the first step, a raw material varnish containing silver particles surface-treated by a surface treatment agent, glutaric acid, and an organic solvent is prepared; In the second step, the raw material varnishes are mixed to obtain an adhesive varnish; and In a third step, the adhesive varnish is applied to a support film and the organic solvent is removed to obtain a die bonding film. The content of the silver-containing particles is 70% by mass or more based on the total solid content of the adhesive varnish.

3. The method for manufacturing a die bonding film according to claim 1 or 2, wherein: The second step is a step of mixing the raw material varnishes at a temperature of 50° C. or higher.

4. The method for manufacturing a die bonding film according to claim 1 or 2, wherein: The raw varnish further contains a thermosetting resin, a curing agent and an elastomer.

5. The method for manufacturing a die bonding film according to claim 1 or 2, wherein: The second step is a step of adding a thermosetting resin, a curing agent, and an elastomer to the mixed raw material varnish to obtain an adhesive varnish further containing them.

6. A method for manufacturing a dicing die bonding integrated film, comprising: A step of preparing a dicing tape having a substrate layer and a pressure-sensitive adhesive layer disposed on the substrate layer; and A step of bonding a die bonding film manufactured by the method for manufacturing a die bonding film according to claim 1 or 2 to the pressure-sensitive adhesive layer of the dicing tape, and forming an adhesive layer composed of the die bonding film on the pressure-sensitive adhesive layer.

7. A method for manufacturing a semiconductor device, comprising: a step of attaching the adhesive layer of the dicing die bonding integrated film manufactured by the manufacturing method of the dicing die bonding integrated film according to claim 6 to a semiconductor wafer; The step of singulating the semiconductor wafer and the adhesive layer; A step of picking up the semiconductor chip with the adhesive layer from the dicing tape; and A step of bonding the semiconductor chip with the adhesive layer sheet to a supporting member via the adhesive layer sheet.

8. A grain bonding film comprising silver-containing particles produced by a reduction method and glutaric acid, The content of the silver-containing particles is 70 mass % or more based on the total amount of the grain bonding film. 9 . The die bonding film according to claim 8 , further comprising a thermosetting resin, a curing agent and an elastomer.

10. The die bonding film according to claim 9, wherein The thermosetting resin includes an epoxy resin that is liquid at 25°C.

11. A dicing die bonding integrated film comprising: A dicing tape comprising a substrate layer and a pressure-sensitive adhesive layer disposed on the substrate layer; and The adhesive layer is disposed on the pressure-sensitive adhesive layer of the dicing tape and is formed of the die bonding film according to any one of claims 8 to 10.