Optical glass, preforms and optical components
By adjusting the component ratios of B2O3, La2O3 and Al2O3, optical glass with excellent chemical durability and small specific gravity was prepared, which solved the durability of existing glass in an acidic environment and met the needs of lightweight and miniaturization of optical systems. .
Patent Information
- Application Number
- CN202211199050.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2018-06-12
- Filing Date
- 2018-07-13
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2038-07-13
AI Technical Summary
The existing medium-refractive glass has insufficient durability under the influence of water or acid, and is prone to deterioration especially when used outdoors, making it difficult to meet the needs of lightweight and miniaturization of optical systems.
By adjusting the component ratios of B2O3, La2O3 and Al2O3, optical glass with a refractive index of more than 1.62 and an Abbe number of more than 40 and more than 65 are prepared, and its chemical durability is optimized to ensure the stability of the glass in an acidic environment.
It has achieved the preparation of optical glass with good chemical durability and small specific gravity, which is suitable for the lightweight and miniaturization of optical components, and reduces the impact of the deterioration of glass due to acid rain and other environments.
Smart Images

Figure CN115536267B_ABST
Abstract
Description
[0001] This application is a divisional application of the application with application number 201810768582.6, application date July 13, 2018, and invention name “Optical glass, preform and optical element”. Technical Field
[0002] The invention relates to optical glass, preform and optical element. Background Art
[0003] In recent years, the digitization and high definition of equipment using optical systems are developing rapidly. In the field of various optical equipment such as photographic equipment such as digital cameras and camcorders, or image reproduction (projection) equipment such as projectors and projection televisions, there is a growing demand to reduce the number of optical elements such as lenses and prisms used in the optical system and to make the entire optical system lighter and smaller.
[0004] In the optical glass used to make optical elements, especially those with a refractive index (n) of 1.62 or more, which can achieve lightweight and miniaturization of the entire optical system and chromatic aberration correction, are widely used. d ) and has an Abbe number (ν d ) is in high demand for medium refractive index, low dispersion glass.
[0005] As such medium refractive index low dispersion glass, a glass composition represented by Patent Documents 1 and 2 is known. 2 O 3 -La 2 O 3 The glass composition composed of the system is easily affected by water or acid due to the characteristics of the glass components generally used, and the durability is not sufficient. Therefore, when the glass is polished, the glass may deteriorate, and defects may occur in the manufacturing process.
[0006] In addition, since surveillance cameras and car cameras, which have been increasingly in demand in recent years, are often used outdoors, they are often exposed to wind and rain, water vapor in the atmosphere, etc. When using an imaging element using a conventional glass composition, the durability of the glass components described in Patent Documents 1 and 2 is not sufficient when used outdoors for a long time.
[0007] Prior art literature
[0008] Patent Literature
[0009] Patent Document 1: Japanese Patent Application Laid-Open No. 55-080736
[0010] Patent Document 2: Japanese Patent Application Laid-Open No. 11-139844 Summary of the invention
[0011] The present invention has been developed in view of the above problems. The object of the present invention is to produce an optical glass having optical constants within the above predetermined ranges and having good chemical durability and a low specific gravity.
[0012] The present inventors have repeatedly conducted intensive experimental studies to solve the above problems and have found that by adjusting the content of each component to B 2 O 3 Composition exceeding 0-45.0%, La 2 O 3 Composition 15.0~55.0%, Al 2 O 3 When the content of the component exceeds 0 to 30.0%, a glass that solves the above-mentioned problems can be obtained, and the present invention has been completed. Specifically, the present invention provides the following.
[0013] (1) An optical glass, wherein, in terms of mass %,
[0014] Contains: B 2 O 3 Ingredients exceeding 0-45.0%,
[0015] La 2 O 3 Ingredients 15.0~55.0%,
[0016] Al 2 O 3 Ingredients exceeding 0 to 30.0%,
[0017] The chemical durability (acid resistance) measured by the powder method is level 1 to level 4.
[0018] It has a refractive index (n d ) and has an Abbe number (ν d ).
[0019] (2) The optical glass according to (1), wherein (SiO 2 +Al 2 O 3 +Ln 2 O 3 ) / (RO+Rn 2 O+ZnO+B 2 O 3 +nd×10) is greater than 0.50 (wherein Ln is selected from at least one of the group consisting of La, Gd, Y, and Lu, R is selected from at least one of the group consisting of Mg, Ca, Sr, and Ba, and Rn is selected from at least one of the group consisting of Li, Na, and K).
[0020] (3) A preform comprising the optical glass described in (1) or (2).
[0021] (4) An optical element comprising the optical glass according to any one of (1) to (2).
[0022] (5) An optical device comprising the optical element described in (4).
[0023] According to the present invention, a glass having optical constants within a predetermined range and good chemical durability can be produced. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] Figure 1 is the refractive index (n) of the glass of the embodiment of the present invention. d ) and the Abbe number (ν d )’s relationship diagram. DETAILED DESCRIPTION
[0025] Hereinafter, the embodiment of the glass of the present invention is described in detail, but the present invention is not limited to any of the following embodiments, and can be appropriately changed to implement within the scope of the purpose of the present invention. In addition, for the part of repeated description, sometimes the description is appropriately omitted, but it is not used to limit the gist of the invention.
[0026] [Glass composition]
[0027] The composition range of each component constituting the optical glass of the present invention is described below. In this specification, unless otherwise specified, the content of each component is expressed in mass % relative to the total amount of glass material in oxide conversion composition. Here, "oxide conversion composition" is the composition of each component contained in the glass, assuming that the oxides, complex salts, metal fluorides, etc. used as raw materials for the glass components of the present invention are all decomposed and converted into oxides when melted, and the total amount of the generated oxides is set to 100 mass%.
[0028] B 2 O 3 The component is an essential component, and when contained in excess of 0%, it has the effect of improving the meltability and the resistance to devitrification. 2 O 3 The content of the component is preferably more than 0%, more preferably 5.0% or more, further preferably 10.0% or more, further preferably 15.0% or more, further preferably 20.0% or more, and most preferably 25.0% or more.
[0029] On the other hand, by 2 O 3 The content of the component is set to 45.0% or less, which can suppress the deterioration of the chemical durability of the glass.2 O 3 The content of the component is preferably 45.0% or less, more preferably 40.0% or less, more preferably 35.0% or less, and further preferably 33.0% or less.
[0030] B 2 O 3 Ingredients, you can use H 3 BO 3 、Na 2 B 4 O 7 、Na 2 B 4 O 7 10H 2 O. BPO 4 etc as raw materials.
[0031] La 2 O 3 The component is an essential component. When it is contained in an amount of 15.0% or more, it increases the refractive index of the glass and the Abbe number of the glass. 2 O 3 The content of the component is preferably 15.0% or more, more preferably 18.0% or more, further preferably 20.0% or more, and further preferably 23.0% or more. In the case where an optical glass having a refractive index of 1.73 or more is required, La is particularly preferably 2 O 3 The component is set to 40.0% or more. 2 O 3 When the content is 40.0 or more, it is easy to obtain high refractive index while improving chemical durability.
[0032] On the other hand, by 2 O 3 The content of the component is set to 55.0% or less, and the stability of the glass is improved, and devitrification can be reduced. 2 O 3 The content of the component is preferably 55.0% or less, more preferably 53.0% or less, and further preferably 50.0% or less.
[0033] La 2 O 3 Ingredients, you can use La 2 O 3 、La(NO 3 ) 3 ·XH 2 O (X is an arbitrary integer) etc. as raw materials.
[0034] Al 2 O 3Al is an essential component and has the effect of improving devitrification resistance and chemical durability. 2 O 3 The content of the component is preferably more than 0%, more preferably more than 0.5%, further preferably more than 1.0%, further preferably more than 1.5%, further preferably more than 2.0%, and most preferably more than 3.0%. In particular, when containing 10.0% or more SiO 2 In the case of Al 2 O 3 The component is set to 8.0% or more. This can suppress the SiO 2 The crystallization caused by the components can obtain glass with excellent resistance to devitrification.
[0035] On the other hand, by 2 O 3 The content of the component is set to 30.0% or less, which can suppress the excessive Al 2 O 3 The devitrification resistance and refractive index decrease caused by Al 2 O 3 The content of the component is preferably 30.0% or less, more preferably 28.0% or less, further preferably 26.0% or less, further preferably 24.0% or less, further preferably 22.0% or less, further preferably 20.0% or less.
[0036] Al 2 O 3 Ingredients, Al can be used 2 O 3 、Al(OH) 3 , AlF 3 、Al(PO 3 ) 3 etc as raw materials.
[0037] SiO 2 The component is an optional component, and when contained in excess of 0%, devitrification resistance and chemical durability are improved. 2 The content of the component is preferably more than 0%, more preferably 3.0% or more, and further preferably 5.0% or more.
[0038] On the other hand, by 2 When the content of the component is set to less than 40.0%, a higher refractive index can be easily obtained, and the deterioration of the meltability and the excessive increase in viscosity can be suppressed. 2 The content of the component is preferably less than 40.0%, more preferably 38.0% or less, further preferably 35.0% or less, and further preferably 30.0% or less.
[0039] SiO 2 Ingredients, SiO 2 , K 2 SiF 6 、Na 2 SiF 6 etc as raw materials.
[0040] The sum (mass sum) of the contents of RO components (wherein R is one or more selected from the group consisting of Mg, Ca, Sr, and Ba) is preferably less than 30.0%. This can suppress the deterioration of chemical durability and the reduction of devitrification resistance caused by the excessive inclusion of RO components.
[0041] Therefore, the mass sum of the RO components is preferably less than 30.0%, more preferably less than 20.0%, more preferably less than 10.0%, more preferably less than 8.0%, and even more preferably less than 5.0%.
[0042] Preferably, Ln 2 O 3 The sum (mass sum) of the contents of the components (wherein Ln is one or more selected from the group consisting of La, Gd, Y, and Lu) is in the range of 30.0% to 70.0%.
[0043] In particular, by setting the sum to 30.0% or more, the refractive index and Abbe number of the glass can be increased, so that glass having a desired refractive index and Abbe number can be easily obtained. 2 O 3 The mass sum of the components is preferably 30.0% or more, more preferably 35.0% or more, further preferably 40.0% or more, and further preferably 45.0% or more.
[0044] On the other hand, by setting the sum to 70.0% or less, the liquidus temperature of the glass is lowered, and thus the devitrification of the glass can be reduced. 2 O 3 The mass sum of the components is preferably 70.0% or less, more preferably 65.0% or less, and further preferably 63.0% or less.
[0045] In mass ratio (SiO 2 +Al 2 O 3 ) / (B 2 O 3 ) is 0.1 or more, the effect of improving the chemical durability of the glass is easily obtained. 2 +Al 2 O 3 ) / (B 2 O 3) is preferably at least 0.1, more preferably at least 0.2, further preferably at least 0.23, further preferably at least 0.5.
[0046] On the other hand, by setting the mass ratio to 10.0 or less, it is possible to suppress the deterioration of the meltability of the glass raw material and the excessive increase in viscosity. 2 +Al 2 O 3 ) / (B 2 O 3 ) has no particular upper limit, but is preferably 10.0 or less, more preferably 8.0 or less, further preferably 6.0 or less, further preferably 5.0 or less, further preferably 4.0 or less, further preferably 3.0 or less, further preferably 2.0 or less, and most preferably 1.0 or less.
[0047] In addition, in the absence of B 2 O 3 In the case of components, (SiO 2 +Al 2 O 3 ) / (B 2 O 3 ) is set to infinity.
[0048] In the mass ratio (Al 2 O 3 / Ln 2 O 3 ) is 0.01 or more, the effect of improving the devitrification resistance is easily obtained.
[0049] Therefore, (Al 2 O 3 / Ln 2 O 3 ) is preferably at least 0.01, more preferably at least 0.03, further preferably at least 0.05, further preferably at least 0.08, and most preferably at least 0.10.
[0050] On the other hand, by setting the mass ratio to 1.0 or less, it is possible to suppress the deterioration of the meltability of the glass raw material and the excessive increase in viscosity. 2 O 3 / Ln 2 O 3 ) is preferably 1.0 or less, more preferably 0.9 or less, further preferably 0.8 or less, further preferably 0.7 or less, further preferably 0.6 or less, and most preferably 0.55 or less.
[0051] In addition, in the absence of Ln 2 O 3In the case of Al 2 O 3 / Ln 2 O 3 The value of is set to infinity.
[0052] In (SiO 2 +Al 2 O 3 +Ln 2 O 3 ) / (RO+Rn 2 O+ZnO+B 2 O 3 When the quotient of (x / z + nd×10) is 0.50 or more, it is easy to obtain desired optical constants while improving chemical durability and devitrification resistance.
[0053] Therefore, (SiO 2 +Al 2 O 3 +Ln 2 O 3 ) / (RO+Rn 2 O+ZnO+B 2 O 3 The quotient value of (x = 10 + nd×10) is preferably 0.50 or more, more preferably 0.80 or more, further preferably 1.00 or more, and most preferably 1.25 or more.
[0054] On the other hand, by setting the quotient to 10.00 or less, it is possible to suppress the deterioration of the meltability of the glass raw material and the excessive increase in viscosity. 2 +Al 2 O 3 +Ln 2 O 3 ) / (RO+Rn 2 O+ZnO+B 2 O 3 The quotient value of (x + nd×10) is preferably 10.00 or less, more preferably 8.00 or less, further preferably 5.00 or less, further preferably 4.50 or less, and most preferably 4.30 or less.
[0055] Y 2 O 3 The component is an arbitrary component, and when it contains more than 0%, the material cost of the glass can be suppressed while maintaining a high refractive index and a high Abbe number, and the specific gravity of the glass can be reduced compared with other rare earth components. 2 O 3The content of the component may preferably exceed 0%, more preferably 1.0% or more, further preferably 3.0% or more, further preferably 5.0% or more, further preferably 8.0% or more, further preferably 10.0% or more.
[0056] On the other hand, by 2 O 3 The content of the component is set to 30.0% or less, which can improve the devitrification resistance of the glass. 2 O 3 The content of the component is preferably 30.0% or less, more preferably 25.0% or less, further preferably 20.0% or less, and further preferably 15.0% or less.
[0057] Y 2 O 3 Ingredients, you can use Y 2 O 3 , YF 3 etc as raw materials.
[0058] G 2 O 3 The component is an arbitrary component, and when contained in excess of 0%, the refractive index of the glass can be increased and the Abbe number can be increased.
[0059] On the other hand, due to the high cost of Gd among rare earth elements, 2 O 3 The content of Gd is set to 35.0% or less, which can suppress the increase of specific gravity and reduce the material cost of glass, so that optical glass can be produced more cheaply. 2 O 3 The content of the component is preferably 35.0% or less, more preferably 30.0% or less, further preferably 25.0% or less, and further preferably 20.0% or less.
[0060] In particular, by 2 O 3 The material cost can be further reduced by setting the content of Gd to less than 10.0%. 2 O 3 The content of the component is preferably less than 10.0%, more preferably less than 5.0%, further preferably less than 1.0%, and further preferably less than 0.1%. From the viewpoint of reducing material cost and suppressing increase in specific gravity, Gd may not be contained. 2 O 3 Element.
[0061] G 2 O 3 Ingredients, Gd can be used 2 O 3 , GdF3 etc as raw materials.
[0062] Lu 2 O 3 The component is an arbitrary component, and when contained in excess of 0%, the refractive index of the glass can be increased and the Abbe number can be increased.
[0063] On the other hand, due to the 2 O 3 The content of the component is set below 10.0%, which reduces the material cost of the glass, thereby making it possible to produce optical glass more cheaply. In addition, it can improve the resistance of the glass to devitrification. 2 O 3 The content of the component is preferably 10.0% or less, more preferably 5.0% or less, further preferably 3.0% or less, further preferably 1.0% or less, further preferably 0.1% or less. From the viewpoint of reducing material costs, Lu may not be contained. 2 O 3 Element.
[0064] Lu 2 O 3 Ingredients, you can use Lu 2 O 3 etc as raw materials.
[0065] Yb 2 O 3 The component is an arbitrary component, and when contained in excess of 0%, the refractive index of the glass can be increased and the Abbe number can be increased.
[0066] On the other hand, due to the 2 O 3 The content of the component is set to 10.0% or less, which can reduce the material cost of the glass, so that optical glass can be produced more cheaply. In addition, the devitrification resistance of the glass can be improved. 2 O 3 The content of the component is preferably 10.0% or less, more preferably 5.0% or less, further preferably 3.0% or less, further preferably 1.0% or less, further preferably 0.1% or less. From the viewpoint of reducing material cost, Yb may not be contained. 2 O 3 Element.
[0067] Yb 2 O 3 Ingredients, you can use Yb 2 O 3 etc as raw materials.
[0068] ZrO 2The component is an arbitrary component, and when contained in excess of 0%, the refractive index and the Abbe number of the glass can be increased, and the devitrification resistance can be improved.
[0069] On the other hand, by 2 The content of the component is set to 10.0% or less, which can reduce the risk of excessive ZrO 2 Therefore, ZrO 2 The content of the component is preferably 10.0% or less, more preferably 7.0% or less, further preferably 5.0% or less, further preferably 3.0% or less, further preferably 2.0% or less, further preferably 1.0% or less, further preferably 0.1% or less.
[0070] ZrO 2 Composition, ZrO can be used 2 , ZrF 4 etc as raw materials.
[0071] TiO 2 The component is an arbitrary component, and when contained in excess of 0%, the refractive index of the glass can be increased.
[0072] On the other hand, by 2 The content of the component is set below 10.0%, which can reduce the risk of excessive TiO 2 The devitrification caused by the TiO component can suppress the decrease in the transmittance of the glass to visible light (especially wavelengths below 500nm). 2 The content of the component is preferably 10.0% or less, more preferably 8.0% or less, further preferably 6.0% or less, further preferably 4.0% or less, further preferably 2.0% or less, further preferably 1.0% or less, further preferably 0.5% or less, further preferably 0.1% or less.
[0073] Nb 2 The O5 component is an optional component, and when contained in a content exceeding 0%, the refractive index of the glass can be increased.
[0074] On the other hand, by 2 O 5 The content of the component is set to 15.0% or less, which can reduce the excessive Nb 2 O 5 The devitrification caused by Nb components can be suppressed, and the decrease in the transmittance of glass to visible light (especially wavelengths below 500nm) can be suppressed. 2 O 5The content of the component is preferably 15.0% or less, more preferably 12.0% or less, further preferably 10.0% or less, further preferably 8.0% or less, further preferably 5.0% or less, further preferably 4.0% or less.
[0075] Nb 2 O 5 Ingredients, Nb can be used 2 O 5 etc as raw materials.
[0076] Ta 2 O 5 The component is an optional component, and when contained in excess of 0%, the refractive index of the glass can be increased and the devitrification resistance can be improved.
[0077] On the other hand, due to the expensive Ta 2 O 5 If the content is set below 10.0%, the material cost of the glass will be reduced, so that optical glass can be produced more cheaply. 2 O 5 The content of the component is preferably 10.0% or less, more preferably 5.0% or less, further preferably 3.0% or less, further preferably 1.0% or less, further preferably 0.1% or less. From the viewpoint of reducing material cost, Ta may not be contained. 2 O 5 Element.
[0078] Ta 2 O 5 Ingredients, you can use Ta 2 O 5 etc as raw materials.
[0079] WO 3 The component is an optional component, and when contained in excess of 0%, the refractive index of the glass can be increased and the devitrification resistance can be improved.
[0080] On the other hand, by 3 The content of the component is set to 10.0% or less, which can reduce the 3 The coloring of glass caused by the components can increase the visible light transmittance. 3 The content of the component is preferably 10.0% or less, more preferably 8.0% or less, further preferably 6.0% or less, further preferably 4.0% or less, further preferably 1.0% or less, further preferably 0.5% or less, further preferably 0.1% or less.
[0081] WO 3 Ingredients, can use WO 3 etc as raw materials.
[0082] The ZnO component is an optional component, and when contained in excess of 0%, the low temperature melting property is improved.
[0083] On the other hand, by setting the content of the ZnO component to 25.0% or less, it is possible to suppress the decrease in the Abbe number and the decrease in the devitrification resistance caused by the excessive ZnO component. Therefore, the content of the ZnO component is preferably 25.0% or less, more preferably 20.0% or less, more preferably 15.0% or less, more preferably 12.0% or less, further preferably 10.0% or less, further preferably 8.0% or less, further preferably 6.0% or less, further preferably 4.0% or less, further preferably 2.0% or less, further preferably 1.0% or less.
[0084] ZnO component, ZnO, ZnF 2 etc as raw materials.
[0085] The MgO component is an optional component, and when the MgO component is contained in excess of 0%, the low temperature melting property is improved.
[0086] On the other hand, by setting the content of the MgO component to 15.0% or less, it is possible to suppress the deterioration of chemical durability and the reduction of devitrification resistance caused by the excessive inclusion of the MgO component. Therefore, the content of the MgO component is preferably 15.0% or less, more preferably 10.0% or less, further preferably 8.0% or less, further preferably 5.0% or less, further preferably 3.0% or less, further preferably 1.0% or less, and most preferably 0.1% or less.
[0087] MgO component, MgCO 3 MgF 2 etc as raw materials.
[0088] The CaO component is an optional component, and when contained in excess of 0%, the low temperature melting property is improved.
[0089] On the other hand, by setting the content of the CaO component to 15.0% or less, the deterioration of chemical durability and the reduction of devitrification resistance caused by the excessive inclusion of the CaO component can be suppressed. Therefore, the content of the CaO component is preferably 15.0% or less, more preferably 10.0% or less, further preferably 8.0% or less, further preferably 5.0% or less, further preferably 3.0% or less, and most preferably 1.0% or less.
[0090] CaO component, CaCO 3 , CaF 2 etc as raw materials.
[0091] The SrO component is an optional component, and when contained in excess of 0%, the low temperature melting property is improved.
[0092] On the other hand, by setting the content of the SrO component to 15.0% or less, the deterioration of chemical durability and the reduction of devitrification resistance caused by the excessive inclusion of the SrO component can be suppressed. Therefore, the content of the SrO component is preferably 15.0% or less, more preferably 10.0% or less, further preferably 8.0% or less, further preferably 5.0% or less, further preferably 3.0% or less, further preferably 1.0% or less, and most preferably 0.1% or less.
[0093] SrO components can use Sr(NO 3 ) 2 , SrF 2 etc as raw materials.
[0094] The BaO component is an optional component, and when the content exceeds 0%, the low-temperature melting property is improved.
[0095] On the other hand, by setting the content of the BaO component to 20.0% or less, the deterioration of chemical durability and the reduction of devitrification resistance caused by the excessive inclusion of the BaO component can be suppressed. Therefore, the content of the BaO component is preferably 20.0% or less, more preferably 15.0% or less, more preferably 10.0% or less, further preferably 8.0% or less, further preferably 5.0% or less, further preferably 3.0% or less, further preferably 1.0% or less, and most preferably 0.1% or less.
[0096] BaO component, BaCO 3 ,Ba(NO 3 ) 2 , BaF 2 etc as raw materials.
[0097] Li 2 The O component is an optional component, and when contained in a content exceeding 0%, the low temperature melting property and the formability of the glass are improved.
[0098] On the other hand, by 2 The content of O component is set to 8.0% or less, which can suppress the excessive Li 2 O component causes deterioration of chemical durability. 2 The content of the O component is preferably 8.0% or less, more preferably 6.0% or less, further preferably 5.0% or less, further preferably 4.0% or less, further preferably 3.0% or less, further preferably 2.0% or less, and most preferably 1.0% or less.
[0099] Li 2O component, Li 2 CO 3 、LiNO 3 , Li 2 CO 3 etc as raw materials.
[0100] Na 2 The O component is an optional component, and when contained in excess of 0%, the low temperature melting property is improved.
[0101] On the other hand, by 2 The content of O component is set to 8.0% or less, which can suppress the excessive Na 2 O component causes deterioration of chemical durability. 2 The content of the O component is preferably 8.0% or less, more preferably 6.0% or less, further preferably 4.0% or less, further preferably 2.0% or less, further preferably 1.0% or less, and most preferably 0.1% or less.
[0102] Na 2 O component, Na 2 CO 3 、NaNO 3 , NaF, Na 2 SiF 6 etc as raw materials.
[0103] K 2 The O component is an optional component, and when contained in excess of 0%, the low temperature melting property is improved.
[0104] On the other hand, by 2 The content of O component is set to 8.0% or less, which can suppress the excessive K 2 O component causes deterioration of chemical durability. 2 The content of the O component is preferably 8.0% or less, more preferably 6.0% or less, further preferably 4.0% or less, further preferably 2.0% or less, further preferably 1.0% or less, and most preferably 0.1% or less.
[0105] K 2 O component, K can be used 2 CO 3 、KNO 3 , KF, KHF 2 , K 2 SiF 6 etc as raw materials.
[0106] R 2The total content of the O component (wherein Rn is selected from one or more of the group consisting of Li, Na, and K) is preferably 8.0% or less. This can suppress the 2 Therefore, the total content (mass sum) is preferably 8.0% or less, more preferably 6.0% or less, further preferably 5.0% or less, further preferably 4.0% or less, further preferably 3.0% or less, further preferably 2.0% or less, and most preferably 1.0% or less.
[0107] On the other hand, by making this sum greater than 0%, deterioration of meltability and excessive increase in viscosity can be suppressed. 2 The mass sum of the O component is preferably more than 0%, more preferably more than 0.1%, and even more preferably 0.5% or more.
[0108] GeO 2 The component is an optional component, and when contained in excess of 0%, the refractive index of the glass can be increased and the devitrification resistance can be improved.
[0109] However, due to the GeO 2 The raw material price of GeO is high, so if its content is high, the production cost will increase. 2 The content of the component is preferably 10.0% or less, more preferably 5.0% or less, further preferably 3.0% or less, further preferably 1.0% or less, further preferably 0.1% or less. From the viewpoint of reducing material cost, GeO may not be contained. 2 Element.
[0110] GeO 2 Composition, GeO 2 etc as raw materials.
[0111] Ga 2 O 3 The component is an optional component, and when contained in excess of 0%, the refractive index of the glass can be increased and the devitrification resistance can be improved.
[0112] However, due to the 2 O 3 The raw material price of Ga is high, so if its content is high, the production cost will be high. 2 O 3 The content of the component is preferably 10.0% or less, more preferably 5.0% or less, further preferably 3.0% or less, further preferably 1.0% or less, further preferably 0.1% or less. From the viewpoint of reducing material cost, Ga may not be contained. 2 O 3 Element.
[0113] Ga 2 O 3 Ingredients, Ga can be used 2 O 3 etc as raw materials.
[0114] P 2 O 5 The component is an arbitrary component, and when contained in excess of 0%, the liquidus temperature of the glass is lowered to improve the devitrification resistance.
[0115] On the other hand, by 2 O 5 The content of the component is set to 30.0% or less, which can suppress the reduction of the chemical durability of the glass, especially the water resistance. 2 O 5 The content of the component is preferably 30.0% or less, more preferably 20.0% or less, further preferably 15.0% or less, further preferably 10.0% or less, further preferably 5.0% or less, further preferably 1.0% or less, and most preferably 0.1% or less.
[0116] P 2 O 5 Ingredients, Al(PO 3 ) 3 、Ca(PO 3 ) 2 、Ba(PO 3 ) 2 、BPO 4 , H 3 PO 4 etc as raw materials.
[0117] Bi 2 O 3 The component is an arbitrary component, and when contained in excess of 0%, the refractive index can be increased and the glass transition point can be lowered.
[0118] On the other hand, by 2 O 3 The content of the component is set to 5.0% or less, which can suppress the coloring of the glass and improve the resistance to devitrification. 2 O 3 The content of the component is preferably 5.0% or less, more preferably 3.0% or less, further preferably 1.0% or less, and most preferably 0.1% or less.
[0119] Bi 2 O 3 Ingredients, Bi can be used 2 O 3 etc as raw materials.
[0120] TeO 2 The component is an arbitrary component, and when contained in excess of 0%, the refractive index can be increased and the glass transition point can be lowered.
[0121] On the other hand, TeO 2 There is a problem that when the glass raw material is melted in a platinum crucible or in a melting tank whose portion in contact with the molten glass is made of platinum, it may alloy with platinum. 2 The content of the component is preferably 5.0% or less, more preferably 3.0% or less, further preferably 1.0% or less, and most preferably 0.1% or less.
[0122] TeO 2 Ingredients, TeO can be used 2 etc as raw materials.
[0123] SnO 2 The component is an optional component, and when contained in excess of 0%, oxidation of the molten glass is reduced to make it clear and the visible light transmittance of the glass can be increased.
[0124] On the other hand, by 2 The content of the component is set to 3.0% or less, which can reduce the coloring of the glass caused by the reduction of the molten glass and reduce the devitrification of the glass. 2 The alloying of components and melting equipment (especially precious metals such as Pt) can therefore be expected to extend the service life of melting equipment. 2 The content of the component is preferably 3.0% or less, more preferably 1.0% or less, further preferably 0.5% or less, and most preferably 0.1% or less.
[0125] SnO 2 As ingredients, SnO, SnO 2 、SnF 2 、SnF 4 etc as raw materials.
[0126] Sb 2 O 3 The component is an arbitrary component, and when contained in excess of 0%, the molten glass can be defoamed.
[0127] On the other hand, if Sb 2 O 3 If the content of the component is too high, the transmittance in the short wavelength region of the visible light region will deteriorate. 2 O 3 The content of the component is preferably 1.0% or less, more preferably 0.7% or less, further preferably 0.5% or less, further preferably 0.2% or less, and most preferably 0.1% or less.
[0128] Sb 2 O 3 Ingredients, Sb can be used 2 O 3 , Sb 2 O 5 、Na 2 H 2 Sb 2 O 7 ·5H 2 O etc. as raw materials.
[0129] In addition, the component for clarifying and degassing the glass is not limited to the above-mentioned Sb. 2 O 3 As the component, a clarifier, a defoaming agent or a combination of these agents known in the field of glass manufacturing can be used.
[0130] The component F is an optional component, and when contained in a content exceeding 0%, the Abbe number of glass is increased, the glass transition point is lowered, and the devitrification resistance can be improved.
[0131] However, when the content of the F component, i.e., the total amount of F in the fluorides replacing a part or all of the oxides of one or more of the above-mentioned metal elements, exceeds 15.0%, the volatilization amount of the F component increases, making it difficult to obtain stable optical constants and homogeneous glass.
[0132] Therefore, the content of the component F is preferably 15.0% or less, more preferably 12.0% or less, further preferably 10.0% or less, further preferably 5.0% or less, further preferably 3.0% or less, and most preferably 1.0% or less.
[0133] The F component can be obtained by using, for example, ZrF 4 , AlF 3 , NaF, CaF 2 etc. are contained in the glass as raw materials.
[0134] In terms of mass and (ZrO 2 +TiO 2 +Nb 2 O 5 +Ta 2 O 5 +WO 3 +Bi 2 O 3 +TeO 2 ) is 20.0% or less, the effect of improving the devitrification resistance is easily obtained, and the excessive decrease in the Abbe number can be suppressed, and low dispersion performance is easily obtained. 2 +TiO 2 +Nb2 O 5 +Ta 2 O 5 +WO 3 +Bi 2 O 3 +TeO 2 ) is preferably 20.0% or less, more preferably 15.0% or less, further preferably 10.0% or less, further preferably 5.0% or less, further preferably 3.0% or less, further preferably 1.0% or less, and most preferably 0.1% or less.
[0135] In the mass ratio (Ln 2 O 3 When the ratio (R / RO) is 1.0 or more, the effect of improving the chemical durability of the glass is easily obtained.
[0136] Therefore, (Ln 2 O 3 The mass ratio of R / RO is preferably 1.0 or more, more preferably 3.0 or more, further preferably 5.0 or more, further preferably 10.0 or more, further preferably 20.0 or more, and most preferably 30.0 or more.
[0137] In addition, since the RO component is not contained, the effect of improving chemical durability can be more easily obtained. 2 O 3 The upper limit of the mass ratio of R2 / RO is not particularly limited and may be an infinite value.
[0138] In the mass ratio (Ln 2 O 3 / Rn 2 When O) is 3.0 or more, the effect of improving the chemical durability of glass is easily obtained.
[0139] Therefore, (Ln 2 O 3 / Rn 2 The mass ratio of O) is preferably 3.0 or more, more preferably 5.0 or more, further preferably 8.0 or more, further preferably 10.0 or more, further preferably 15.0 or more, further preferably 20.0 or more, further preferably 25.0 or more, and most preferably 30.0 or more.
[0140] In addition, since it does not contain Rn 2 O component, it is easier to obtain the effect of improving chemical durability, so (Ln 2 O 3 / Rn 2 The upper limit of the mass ratio of (O) is not particularly limited and may be set to be infinite.
[0141] In the mass product (BaO×Gd 2 O 3 ) is less than 8.0, the specific gravity and cost of the glass can be easily suppressed. 2 O 3 ) is preferably less than 8.0, more preferably less than 7.0, further preferably less than 6.0, further preferably less than 5.0, further preferably less than 4.0, further preferably less than 3.0, further preferably less than 2.0, further preferably less than 1.0, and most preferably less than 0.1.
[0142] In mass product (SiO 2 +Al 2 O 3 +B 2 O 3 )×Rn 2 When O is 500 or less, it is easy to obtain the effect of improving the chemical durability of glass while maintaining a high refractive index and a high Abbe number. 2 +Al 2 O 3 +B 2 O 3 )×Rn 2 The mass product of O is preferably 500 or less, more preferably 450 or less, further preferably 400 or less, further preferably 350 or less, further preferably 300 or less, further preferably 250 or less, further preferably 200 or less, further preferably 150 or less, and most preferably 100 or less.
[0143] In terms of mass and (SiO 2 +Al 2 O 3 ) is 5.0% or more, the effect of improving the chemical durability of the glass is easily obtained. 2 +Al 2 O 3 ) is preferably 5.0% or more, more preferably 7.0% or more, further preferably 9.0% or more, and further preferably 10.0% or more.
[0144] On the other hand, by setting the mass sum to 55.0% or less, it is possible to suppress the deterioration of the meltability of the glass raw material and the excessive increase in viscosity. 2 +Al 2 O 3) is preferably 55.0% or less, more preferably 50.0% or less, more preferably 45.0% or less, further preferably 40.0% or less, further preferably 38.0% or less, further preferably 35.0% or less, further preferably 32.0% or less, and most preferably 30.0% or less.
[0145] In terms of mass and (ZrO 2 When the content of ZrO is less than 25.0%, the effect of suppressing the decrease of Abbe number (increase of dispersion) is easily obtained. 2 The mass sum of ZnO (ZnO) is preferably less than 25.0%, more preferably less than 20.0%, more preferably less than 15.0%, more preferably less than 10.0%, more preferably less than 8.5%, and further preferably less than 6.0%.
[0146] <About ingredients that should not be contained>
[0147] Next, components that should not be contained in the optical glass of the present invention and components that are not suitable for being contained are described.
[0148] Other components may be added as needed within the range that does not affect the properties of the glass of the present invention. However, in addition to Ti, Zr, Nb, W, La, Gd, Y, Yb, and Lu, when a small amount of transition metal components such as V, Cr, Mn, Fe, Co, Ni, Cu, Ag, and Mo are contained alone or in combination, even if a small amount is contained, the glass will still be colored and have the property of absorbing specific wavelengths in the visible region. Therefore, in optical glasses that use wavelengths in the visible region, it is preferred that these components are substantially not contained.
[0149] Due to Nd 2 O 3 The composition has a strong influence on the coloring of glass, so it is ideal to contain substantially no Nd. 2 O 3 Ingredients, that is, they are not completely free of except for unavoidable mixing.
[0150] Because Er 2 O 3 The component has a strong influence on the coloring of glass, so it is ideal to contain substantially no Er. 2 O 3 Ingredients, that is, they are not completely free of except for unavoidable mixing.
[0151] Furthermore, since lead compounds such as PbO are components with a high environmental load, it is ideal that lead compounds such as PbO are not substantially contained, that is, not completely contained except for unavoidable contamination.
[0152] In addition, due to As 2O 3 Arsenic compounds such as As are components with high environmental loads, so the 2 O 3 Arsenic compounds such as arsenic, that is, it is not completely free of them except for the inevitable mixture.
[0153] Furthermore, in recent years, there is a trend to avoid the use of Th, Cd, Tl, Os, Be, and Se as harmful chemical substances, and environmental protection measures are required not only in the manufacturing process of glass but also in the processing process and post-commercialization treatment. Therefore, when the environmental impact is important, it is preferred that these components are substantially not contained.
[0154] [Physical properties]
[0155] The optical glass of the present invention preferably has a medium refractive index and a high Abbe number (low dispersion). In particular, the refractive index (n d ) is preferably 1.62 or more, more preferably 1.65 or more, more preferably 1.67 or more, and further preferably 1.71 or more. d ) is preferably 1.85 or less, more preferably 1.83 or less, and further preferably 1.82 or less.
[0156] In addition, the Abbe number (ν d ) is preferably 40 or more, more preferably 43 or more, further preferably 45 or more, further preferably 48 or more, and most preferably 50 or more. d ) is preferably 65 or less, more preferably 63 or less, further preferably 60 or less, further preferably 57 or less.
[0157] By having such a medium refractive index, a large amount of light refraction can be obtained even if the optical element is thinned. In addition, by having such low dispersion, the deviation of focus (chromatic aberration) caused by the wavelength of light when used as a single lens can be reduced. Therefore, for example, when an optical system is formed by combining with an optical element having high dispersion (low Abbe number), the chromatic aberration can be reduced as a whole of the optical system, and high imaging characteristics can be achieved.
[0158] As described above, the optical glass of the present invention is useful in optical design, and particularly, when constituting an optical system, it is possible to achieve miniaturization of the optical system while achieving high imaging characteristics, thereby expanding the degree of freedom of optical design.
[0159] Here, it is preferred that the refractive index (n d ) and Abbe number (ν d ) satisfies (-0.01ν d +2.15)≦nd ≦(-0.01ν d In the glass of the composition specified in the present invention, even if the refractive index (n d ) and Abbe number (ν d ) satisfies this relationship and stable glass can be obtained.
[0160] Therefore, in the optical glass of the present invention, it is preferred that the refractive index (n d ) and Abbe number (ν d ) satisfies n d ≧(-0.01ν d +2.15), and more preferably satisfying n d ≧(-0.01ν d +2.17).
[0161] On the other hand, in the optical glass of the present invention, it is preferred that the refractive index (n d ) and Abbe number (ν d ) satisfies n d ≦(-0.01ν d +2.30), and more preferably satisfying n d ≦(-0.01ν d +2.28).
[0162] Preferably, the specific gravity of the optical glass of the present invention is small. More specifically, the specific gravity of the optical glass of the present invention is 5.00 or less. As a result, since the mass of the optical element and the optical device using the optical element is reduced, it can contribute to the lightweight of the optical device. Therefore, the specific gravity of the optical glass of the present invention is preferably 5.00 or less, more preferably 4.70 or less, and preferably 4.50 or less. In addition, the specific gravity of the optical glass of the present invention is generally 2.80 or more, more specifically 3.00 or more, and further specifically 3.20 or more.
[0163] The specific gravity of the optical glass of the present invention is measured based on the Japan Optical Glass Industry Association Standard JOGIS05-1975 "Method for measuring specific gravity of optical glass".
[0164] The optical glass of the present invention preferably has high acid resistance. In particular, the chemical durability (acid resistance) measured by the glass powder method according to JOGIS06-2009 is preferably 1 to 4, and more preferably 1 to 3.
[0165] This improves the processability of optical glass and reduces the clouding of glass caused by acid rain, etc. when used for automotive applications, thereby making it easier to produce optical elements using glass.
[0166] Here, "acid resistance" refers to the durability of glass against corrosion caused by acid, and the acid resistance can be measured by the Japan Optical Glass Industry Association Standard "Method for Determination of Chemical Durability of Optical Glass" JOGIS06-2009. In addition, "chemical durability (acid resistance) measured by powder method is 1 to 3 levels" means that the chemical durability (acid resistance) measured based on JOGIS06-2009 is the weight loss rate of the sample before and after the measurement, which is less than 0.65% by mass.
[0167] In addition, "Level 1" of chemical durability (acid resistance) means that the weight loss rate of the sample before and after measurement is less than 0.20 mass%, "Level 2" means that the weight loss rate of the sample before and after measurement is 0.20 mass% or more and less than 0.35 mass%, "Level 3" means that the weight loss rate of the sample before and after measurement is 0.35 mass% or more and less than 0.65 mass%, "Level 4" means that the weight loss rate of the sample before and after measurement is 0.65 mass% or more and less than 1.20 mass%, "Level 5" means that the weight loss rate of the sample before and after measurement is 1.20 mass% or more and less than 2.20 mass%, and "Level 6" means that the weight loss rate of the sample before and after measurement is 2.20 mass% or more.
[0168] The value of the product (d×RA) of the specific gravity (d) of the glass and the grade (RA) of the acid resistance by the powder method is preferably low. More specifically, the value of the product (d×RA) in the present invention is 20.0 or less.
[0169] This makes it possible to produce a lens that is excellent in acid resistance and light in specific gravity, and thus it is easy to produce an optical element that is lightweight and resistant to acid rain and the like and is suitable for use in vehicles and surveillance cameras.
[0170] Therefore, the product value of (d×RA) in the present invention is preferably 20.0 or less, more preferably 18.0 or less, further preferably 15.0 or less, and further preferably 13.0 or less.
[0171] The lower limit of the product value of (d×RA) of the optical glass of the present invention is not particularly limited, but is generally 1.0 or more, more specifically 2.0 or more, and even more specifically 3.0 or more.
[0172] The optical glass of the present invention preferably has high devitrification resistance, and more specifically, has a low liquidus temperature.
[0173] That is, the liquidus temperature of the optical glass of the present invention is preferably 1300°C or less, more preferably 1250°C or less, further preferably 1200°C or less, further preferably 1150°C or less, further preferably 1100°C or less. Thus, even if the molten glass is discharged at a lower temperature, the crystallization of the produced glass is reduced, so that the devitrification when the glass is formed from the molten state can be reduced, and the influence on the optical characteristics of the optical element using the glass can be reduced. In addition, even if the melting temperature of the glass is lowered, the glass can be formed, so by suppressing the energy consumed when the glass is formed, the manufacturing cost of the glass can be reduced.
[0174] On the other hand, the lower limit of the liquidus temperature of the optical glass of the present invention is not particularly limited, and the liquidus temperature of the glass produced by the present invention is generally 800° C. or higher, specifically 850° C. or higher, and more specifically 900° C. or higher.
[0175] In addition, the "liquid phase temperature" in this specification refers to the lowest temperature at which no crystals are confirmed when observing the presence of crystals under a microscope with a magnification of 100 times after keeping it in a temperature gradient furnace with a temperature gradient of 1000°C to 1300°C for 30 minutes and taking it out of the furnace and cooling it.
[0176] [Manufacturing method]
[0177] The optical glass of the present invention is produced, for example, as follows. That is, the components of the above raw materials are uniformly mixed in a manner such that the components are within a predetermined content range, the prepared mixture is put into a platinum crucible, and melted in an electric furnace at a temperature range of 1100 to 1350° C. for 2 to 6 hours depending on the melting difficulty of the glass composition, stirred and homogenized, and then cooled to an appropriate temperature, and then cast into a mold and slowly cooled to produce the glass.
[0178] [Glass forming]
[0179] The glass of the present invention can be melt-formed by a known method. The method for forming the glass melt is not limited.
[0180] [Glass molded body and optical element]
[0181] The glass of the present invention can be made into a glass molded body using a method such as grinding and polishing. That is, the glass can be made into a glass molded body by mechanical processing such as grinding and polishing. In addition, the method for making a glass molded body is not limited to these methods.
[0182] As described above, the glass formed body formed from the glass of the present invention has excellent durability and therefore good workability, and is less susceptible to degradation of the glass due to acid rain or the like, and therefore can be suitably used in automotive applications or the like.
[0183] Example
[0184] Tables 1 to 17 show the compositions of the glasses of the present invention and comparative examples, and the refractive indices (n d ), Abbe number (ν d ), specific gravity (d), powder method acid resistance grade (RA), liquidus temperature. In addition, the following examples are for illustrative purposes only, and the present invention is not limited to these examples.
[0185] The glasses of the embodiments and comparative examples of the present invention are made of high-purity raw materials used for ordinary optical glasses, such as oxides, hydroxides, carbonates, nitrates, fluorides, and metaphosphate compounds, which are respectively selected as raw materials for various components. After being weighed and uniformly mixed in the proportions of the compositions of the embodiments shown in the table, they are put into a platinum crucible and melted in an electric furnace at a temperature range of 1100 to 1350° C. for 2 to 5 hours depending on the melting difficulty of the glass composition. After being stirred for homogenization, they are cast into a mold, etc., and slowly cooled to produce the glass.
[0186] The refractive index (n d ) and Abbe number (ν d ) is expressed as the measured value of the d line (587.56 nm) of the helium lamp. In addition, the Abbe number (ν d ) using the refractive index of the d-line and the refractive index of the F-line (486.13 nm) of the hydrogen lamp (n F ), the refractive index relative to the C line (656.27nm) (n C ) value, according to the Abbe number (ν d )=[(n d -1) / (n F -n C )] is calculated using the formula.
[0187] The specific gravity of the glass of the examples and comparative examples was measured based on the Japan Optical Glass Industry Association Standard JOGIS05-1975 “Method for measuring specific gravity of optical glass”.
[0188] The acid resistance of the glass of the embodiment and comparative example was measured based on the Japanese Optical Glass Industry Association standard "Method for Determining the Chemical Durability of Optical Glass" JOGIS06-2009. That is, a glass sample crushed into a particle size of 425 to 600 μm was placed in a specific gravity bottle and placed in a platinum basket. The platinum basket was placed in a quartz glass round-bottom flask filled with a 0.01N nitric acid aqueous solution and treated in a boiling water bath for 60 minutes. The weight loss rate (mass %) of the treated glass sample was calculated, and the case where the weight loss rate (mass %) was less than 0.20 was set to level 1, the case where the weight loss rate was 0.20 to less than 0.35 was set to level 2, the case where the weight loss rate was 0.35 to less than 0.65 was set to level 3, the case where the weight loss rate was 0.65 to less than 1.20 was set to level 4, the case where the weight loss rate was 1.20 to less than 2.20 was set to level 5, and the case where the weight loss rate was more than 2.20 was set to level 6. At this time, a smaller number means that the acid resistance of the glass is better.
[0189] The liquidus temperature of the glass of the embodiment and comparative example was maintained in a temperature gradient furnace with a temperature gradient of 1000°C to 1300°C for 30 minutes. After being taken out of the furnace and cooled, no lowest temperature of crystals was confirmed when observing the presence of crystals under a microscope with a magnification of 100 times.
[0190] In addition, when it is described as "1000 or less", it means that no crystals are confirmed at least at 1000°C.
[0191] Table 1
[0192]
[0193] Table 2
[0194]
[0195] Table 3
[0196]
[0197] Table 4
[0198]
[0199] Table 5
[0200]
[0201] Table 6
[0202]
[0203] Table 7
[0204]
[0205] Table 8
[0206]
[0207] Table 9
[0208]
[0209] Table 10
[0210]
[0211] Table 11
[0212]
[0213] Table 12
[0214]
[0215] Table 13
[0216]
[0217] Table 14
[0218]
[0219] Table 15
[0220]
[0221] Table 16
[0222]
[0223] Table 17
[0224]
[0225] As shown in the table, due to the B 2 O 3 The composition is more than 0-45.0%, La 2 O 3 Composition: 15.0~55.0%, Al 2 O 3 Since the content of the component is more than 0 to 30.0%, an optical glass having excellent durability and desired optical constants can be obtained.
[0226] In addition, the refractive index (n d ) are all above 1.62, and the refractive index (n d ) is below 1.85, all within the expected range.
[0227] In addition, the Abbe number (ν d ) are all below 65, and the Abbe number (ν d ) are above 40, which are all within the expected range.
[0228] In addition, the optical glass of the present invention forms stable glass and is unlikely to suffer from devitrification during glass production. This can also be inferred from the fact that the liquidus temperature of the optical glass of the present invention is 1300° C. or lower, more specifically, 1150° C. or lower.
[0229] In addition, the specific gravity of the optical glass of the examples of the present invention is 5.00 or less. Therefore, it can be seen that the specific gravity of the optical glass of the examples of the present invention is small.
[0230] Furthermore, the chemical durability (acid resistance) of the optical glasses of Examples of the present invention measured by a powder method was in the range of 1 to 4, which was within the desired range.
[0231] Therefore, the refractive index (n d ) and Abbe number (ν d ) are all within the desired range, and the chemical durability (acid resistance) measured by the powder method is all 1 to 4, all within the desired range. Therefore, it can be seen that the optical glass of the examples of the present invention is excellent in chemical durability (acid resistance).
[0232] On the other hand, since the La of the optical glass of Comparative Example A 2 O 3 The component is less than 15.0%, so it is impossible to obtain a glass material with excellent chemical durability in the medium refractive index and low dispersion region. In addition, since the optical glass of Comparative Example B does not contain Al 2 O 3 composition, therefore, the stability of the glass is poor and there is no vitrification.
[0233] Furthermore, by forming a glass block using the optical glass of the embodiment of the present invention, grinding and polishing the glass block to form a lens or prism, various lens or prism shapes can be stably formed.
[0234] The present invention has been described in detail above for the purpose of illustration. This embodiment is only for the purpose of illustration. It should be understood that those skilled in the art can make more changes without departing from the concept and scope of the present invention.
Claims
1. An optical glass, wherein: In terms of mass%, it contains The mass ratio (Al2O3 / Ln2O3) is 0.08 or more, wherein Ln is selected from at least one of the group consisting of La, Gd, Y, and Lu, The mass product (SiO2+Al2O3+B2O3)×Rn2O is 44.70 or more and 100 or less, wherein Rn is at least one selected from the group consisting of Li, Na, and K, The chemical durability, i.e. acid resistance, determined by the powder method is level 1 to level 4. Having a refractive index (n) of 1.62 or more and 1.67 or less d ) and has an Abbe number (ν d ).
2. The optical glass according to claim 1, characterized in that: (SiO2+Al2O3+Ln2O3) / The quotient of (RO+Rn2O+ZnO+B2O3+nd×10) is greater than 0.50, wherein Ln is selected from at least one of the group consisting of La, Gd, Y, and Lu, R is selected from at least one of the group consisting of Mg, Ca, Sr, and Ba, and Rn is selected from at least one of the group consisting of Li, Na, and K.
3. A preform, comprising the optical glass according to claim 1 or 2.
4. An optical element, comprising the optical glass according to claim 1 or 2. 5 . An optical device comprising the optical element according to claim 4 .
Citation Information
Patent Citations
Optical glass
JP1999139844A
Optical glass, preform, and optical element
CN103313947A
Optical glass and optical element
CN104341102A
Optical Glass, Lens Pre-forming Body And Optical Element
CN104860531A
Optical glass, preformed body, and optical element
CN105565659A