A method for growing TeO2 thin film using ALD technology

By combining ALD technology with the precursor sources of alcohol tellurium and water, the problems of poor uniformity and shape retention of TeO2 films are solved, and the preparation of high-purity and high-uniformity TeO2 films is achieved to meet the needs of the optical and electrical fields.

CN115584480BActive Publication Date: 2024-10-08SUZHOU ORIGIN DEPOSITION MATERIALS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202210872376.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-07-20
Publication Date
2024-10-08
Estimated Expiration
2042-07-20

AI Technical Summary

Technical Problem

The uniformity and shape retention of TeO2 films in the existing technology are poor, making it difficult to meet the demand for high-quality films in the optical and electrical fields.

Method used

ALD technology is used to combine alcohol tellurium and water as precursor sources, and through wet chemical treatment and vapor deposition, atomic level control and three-dimensional conformality of TeO2 films are achieved, which is suitable for substrates of different shapes and materials.

Benefits of technology

The prepared TeO2 film has high purity, good uniformity, and a uniformity of less than 4%. It is suitable for use in the optical and electrical fields, and the process conditions are easy to control, the cost is low, and the safety is high.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115584480B_ABST
    Figure CN115584480B_ABST
Patent Text Reader

Abstract

The present invention discloses a method for growing a TeO2 thin film using an ALD technique, comprising the following steps: (1) placing a substrate after wet chemical treatment in a reaction chamber of an atomic layer deposition device, introducing a tellurium precursor source to chemically adsorb on the surface of the substrate; the tellurium precursor source is tellurium alcohol; (2) after the chemical adsorption in step (1) is saturated, introducing an inert gas into the reaction chamber for purging, and then introducing an oxygen source for reaction; the oxygen source is water; (3) after the reaction in step (3) is completed, introducing an inert gas into the reaction chamber for purging; (4) repeating steps (1) to (3) to grow the TeO2 thin film on the surface of the substrate. The present invention uses tellurium alcohol as a tellurium precursor source and water as an oxygen source to prepare a uniform TeO2 thin film on substrates of different materials or morphologies using the ALD technique, the process is controllable and the precision is high, and it is suitable for the needs of high-quality TeO2 thin films in the fields of optics and electronics.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of nanomaterials, and in particular to a method for growing a TeO2 film using an ALD technique. Background Art

[0002] TeO2 thin films have high refractive index, good nonlinear optical properties and excellent electrical semiconductor properties, and are widely used in optics, electronics, optoelectronics and other fields. Currently, TeO2 thin films are mainly prepared by thermal evaporation, magnetron sputtering or sol-gel method, but the uniformity and shape retention of the films grown by these methods are poor. In order to meet the demand for high-quality TeO2 thin films in the fields of optics, electronics, etc., it is urgent to develop a method for preparing highly uniform TeO2 thin films.

[0003] Atomic layer deposition (ALD) is a method in which precursors are alternately introduced into a reaction chamber in the form of gas phase and a gas-curing chemical reaction occurs on the substrate surface to form a thin film. ALD usually consists of two half-reaction sequences, A and B, and has the characteristics of surface self-limitation. Surface self-limitation includes chemical adsorption self-limitation and sequential reaction self-limitation, which is the most basic and core feature of atomic layer deposition technology. The most essential reason for surface self-limitation is that there is chemical adsorption-monomolecule adsorption between the precursor and the deposition surface. It can be controlled at the atomic layer level and has excellent three-dimensional conformality.

[0004] Based on the above background, the present invention provides a method for growing a TeO2 thin film using ALD technology. The prepared TeO2 thin film has good uniformity and can be applied to the fields of optics, electronics, etc. Summary of the invention

[0005] The technical problem to be solved by the present invention is to provide a method for growing TeO2 thin film using ALD technology.

[0006] In order to solve the above technical problems, the present invention provides the following technical solutions:

[0007] A first aspect of the present invention provides a method for growing a TeO2 thin film using an ALD technique, comprising the following steps:

[0008] (1) placing the substrate after wet chemical treatment in a reaction chamber of an atomic layer deposition device, introducing a tellurium precursor source to chemically adsorb on the surface of the substrate; the tellurium precursor source is tellurium alcohol;

[0009] (2) After the chemical adsorption in step (1) is saturated, an inert gas is introduced into the reaction chamber for purging, and then an oxygen source is introduced for reaction; the oxygen source is water;

[0010] (3) After the reaction in step (3) is completed, an inert gas is introduced into the reaction chamber for purging to complete a single growth cycle;

[0011] (4) Repeat the above growth cycle to grow the TeO2 thin film on the substrate surface.

[0012] Furthermore, in step (1), the wet chemical treatment is specifically: using one or more solvents selected from HF, methanol, acetone, isopropanol, and water to clean the substrate.

[0013] Furthermore, the substrate is cleaned with acetone, methanol, isopropanol and pure water for 5 to 10 minutes in sequence to remove organic matter on the surface, and then the cleaned silicon wafer is immersed in an HF solution to etch and remove the oxide layer on the surface of the substrate.

[0014] Wet chemical treatment of the substrate can effectively reduce the roughness of the substrate surface, remove surface pollutants, reduce impurities and defects, improve nucleation conditions, facilitate the deposition of the film, and obtain a smooth and flat film.

[0015] Furthermore, in step (1), the substrate includes silicon, silicon dioxide, silicon nitride, silicon carbide, glass, sapphire, gallium nitride, stainless steel with a planar or non-planar surface. The ALD technology is not limited to the shape of the substrate and is suitable for uniformly growing TeO2 thin films on substrates with non-planar surfaces.

[0016] Furthermore, in step (1), the tellurium alcoholate is tellurium methanol (Te(OMe)4), tellurium ethanol (Te(OEt)4) or tellurium isopropoxide (Te(OiPr)4).

[0017] Furthermore, taking silicon wafer as substrate and tellurium precursor source as Te(OEt)4 as an example, the reaction is as follows:

[0018] Te(OEt)4(s)+H2O(g)→TeO2(s)+C2H5OH(g).

[0019] The present invention selects alcohol tellurium compounds as tellurium precursor sources. The tellurium in the alcohol tellurium compounds has a suitable valence state and can generate a higher vapor pressure at a relatively low temperature, reaching adsorption saturation on the substrate surface in a short time. It also has good thermal stability and can undergo an adsorption reaction with water to generate TeO2, thereby achieving stable atomic layer deposition and cyclic growth. In addition, the tellurium precursor source used in the present invention, after reacting with an oxygen source, generates only one solid product, tellurium dioxide, under the temperature conditions of the reaction chamber, while the remaining reactants and products are in a gaseous state and can be carried out by the inert gas subsequently purged, thereby ensuring the purity of the product.

[0020] Furthermore, the tellurium precursor source and the oxygen source are charged into the reaction chamber in a pulsed form in the presence of a carrier gas, and the carrier gas is nitrogen with a purity of not less than 99.999%.

[0021] Furthermore, before growing the TeO2 film, the reaction chamber and the tellurium precursor source are heated.

[0022] Furthermore, the heating temperature of the tellurium precursor source is 70-150° C. By heating the tellurium precursor source, the saturated vapor pressure of the precursor source in the precursor source bottle is increased, the amount of the tellurium precursor source carried by the carrier gas is increased, and the deposition rate is improved.

[0023] Furthermore, the heating temperature of the reaction chamber is 150-400° C. By heating the reaction chamber, the chemical adsorption of the tellurium precursor source and its reaction with water are promoted, thereby increasing the film deposition rate.

[0024] Furthermore, in step (2) and step (3), an inert gas is introduced into the reaction chamber for purging to remove excess precursor sources in the reaction chamber and on the substrate.

[0025] Furthermore, in step (2) and step (3), the inert gas is one of Ar, N2, and He; and the purity of the inert gas is not less than 99.999%.

[0026] The second aspect of the present invention provides a TeO2 film prepared by the method described in the first aspect.

[0027] The third aspect of the present invention provides an application of the TeO2 film described in the second aspect in the field of optics and electronics.

[0028] Compared with the prior art, the present invention has the following beneficial effects:

[0029] (1) The present invention uses tellurium alcohol as a tellurium precursor source and water as an oxygen source in combination with ALD technology to prepare TeO2 thin film. The required reactants are easy to produce and have low cost. The preparation method is simple and the conditions are easy to control. The preparation process is airtight and has no safety hazards. The TeO2 thin film prepared by combining the above materials with ALD technology has high purity and good uniformity, with an inhomogeneity of less than 4%.

[0030] (2) The method used in the present invention to prepare TeO2 thin film is suitable for substrates of different shapes and materials, and the thickness of the TeO2 thin film can be precisely controlled by limiting the process parameters. The prepared high-purity and high-uniformity TeO2 thin film meets the application requirements in the optical and electrical fields. BRIEF DESCRIPTION OF THE DRAWINGS

[0031] Figure 1 The growth of TeO2 film as the heating temperature of tellurium precursor source changes;

[0032] Figure 2 The growth of TeO2 film as the temperature of the reaction chamber changes;

[0033] Figure 3is the XRD pattern of TeO2 thin film;

[0034] Figure 4 The non-uniformity of the TeO2 film prepared by repeating Example 3 three times. DETAILED DESCRIPTION

[0035] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art of the present invention. The terms used herein in the specification of the present invention are only for the purpose of describing specific embodiments and are not intended to limit the present invention. The term "and / or" used herein includes any and all combinations of one or more related listed items.

[0036] The present invention provides a method for growing a TeO2 thin film using an ALD technique, comprising the following steps:

[0037] (1) Pretreatment of the substrate: Use one or more solvents selected from HF, methanol, acetone, isopropanol, and water to clean the substrate to remove surface contaminants; after drying the pretreated substrate, quickly place it in the reaction chamber of the atomic layer deposition equipment, reduce the vacuum to less than 1 Torr, and raise the temperature of the reaction chamber to 150-400°C.

[0038] (2) Introducing a tellurium precursor source: heating the tellurium precursor source bottle to 70-150° C., and pulse the tellurium precursor source vapor into the reaction chamber through a carrier gas, with the pulse time preferably being 1-3 s; and introducing an inert gas into the reaction chamber for purging.

[0039] (3) Introducing an oxygen source: The oxygen source water vapor is pulsed into the reaction chamber through a carrier gas. After the reaction is completed, an inert gas is introduced into the reaction chamber for purging to complete a single growth cycle.

[0040] (4) Repeat the above growth cycle to grow a TeO2 film of target thickness on the substrate surface.

[0041] In the present invention, the substrate is preferably pretreated by using acetone, methanol, isopropanol, and pure water to clean the surface of the substrate in sequence, and then immersing the substrate in an HF solution.

[0042] In the present invention, the tellurium precursor source is preferably tellurium alcoholate, more preferably Te(OMe)4, Te(OEt)4 or Te(OiPr)4.

[0043] In the present invention, the precursor source bottle is preferably heated to 80-150°C, for example, 120°C.

[0044] In the present invention, the reaction chamber is preferably heated to 200-300°C, for example, 200°C, 240°C, or 300°C.

[0045] In the present invention, the carrier gas is preferably high-purity nitrogen; the flow rate of the carrier gas is preferably 10 to 50 sccm, for example, 20 sccm.

[0046] In the present invention, the inert gas is preferably high-purity Ar, high-purity N2 or high-purity He; the purge time of the inert gas is 10 to 50 seconds, such as 20 seconds, 30 seconds, or 40 seconds.

[0047] The present invention is further described below in conjunction with the accompanying drawings and specific embodiments so that those skilled in the art can better understand the present invention and implement it, but the embodiments are not intended to limit the present invention.

[0048] Example 1

[0049] This example explores the effect of the heating temperature of the tellurium precursor source on the growth of TeO2 thin film. Silicon wafer is used as the substrate and Te(OEt)4 is used as the tellurium precursor source as an example. The specific operation is as follows:

[0050] (1) Use acetone, methanol, isopropanol, and pure water to clean the surface of the silicon wafer for 5 minutes in sequence to remove the surface organic matter. Then place the treated silicon wafer in the HF solution for 30 seconds to etch away the natural oxide layer on the surface of the silicon wafer. Place the treated silicon wafer in the ALD equipment reaction chamber within 1 minute and evacuate it to less than 1Torr.

[0051] (2) Input deposition working parameters: the heating temperature of Te(OEt)4 is set to 60-150℃; the water temperature is room temperature; the heating temperature of the reaction chamber is set to 200℃. Set the pipeline carrier gas auxiliary and the flow rate to 20sccm. Before coating, the reaction chamber and the source bottle are heated stably for about 1h, during which high-purity nitrogen is introduced into the reaction chamber of the ALD equipment for purging.

[0052] (3) Coating was started by introducing Te(OEt)4 into the reaction chamber through high-purity nitrogen gas with a pulse time of 3 s, and then 20 sccm of high-purity nitrogen gas was introduced for 20 s of purge.

[0053] (4) Water is introduced into the reaction chamber via a carrier gas to react with Te(OEt)4 adsorbed on the silicon wafer to form a single-layer TeO2 film. Then, 20 sccm of high-purity nitrogen is introduced for 20 seconds to complete a single growth cycle.

[0054] (5) Repeat the above growth cycle to obtain TeO2 thin film.

[0055] In this embodiment, the heating temperature of Te(OEt)4 is set to 60℃, 70℃, 80℃, 100℃, 120℃, and 150℃ respectively to study the effect of Te(OEt)4 on the growth of TeO2 thin film at different heating temperatures. The number of repeated growth cycles is controlled to be the same. The results are as follows: Figure 1 As shown in the figure, when the heating temperature of Te(OEt)4 is 60℃, the thickness of the film is extremely small and the effective growth of the film cannot be achieved. When the heating temperature is greater than 70℃, the growth of the film can be achieved, and the film thickness increases with the increase of the heating temperature. When the heating temperature is 80-150℃, the thickness of the film does not differ much, indicating that the saturated adsorption of the precursor can be achieved within this temperature range.

[0056] Example 2

[0057] This example explores the effect of reaction chamber temperature on the growth of TeO2 thin film. Silicon wafer is used as substrate and Te(OEt)4 is used as tellurium precursor source. The specific operation is as follows:

[0058] (1) Use acetone, methanol, isopropanol, and pure water to clean the surface of the silicon wafer for 5 minutes in sequence to remove the surface organic matter. Then place the treated silicon wafer in the HF solution for 30 seconds to etch away the natural oxide layer on the surface of the silicon wafer. Place the treated silicon wafer in the ALD equipment reaction chamber within 1 minute and evacuate it to less than 1Torr.

[0059] (2) Input deposition working parameters: the heating temperature of Te(OEt)4 is set to 120℃; the water temperature is room temperature; the heating temperature of the reaction chamber is set to 100-350℃. Set the pipeline carrier gas auxiliary and the flow rate to 20sccm. Before coating, the reaction chamber and the source bottle are heated stably for about 1h, during which high-purity nitrogen is introduced into the reaction chamber of the ALD equipment for purging.

[0060] (3) Coating was started by introducing Te(OEt)4 into the reaction chamber through high-purity nitrogen gas with a pulse time of 3 s, and then 20 sccm of high-purity nitrogen gas was introduced for 20 s of purge.

[0061] (4) Water is introduced into the reaction chamber via a carrier gas to react with Te(OEt)4 adsorbed on the silicon wafer to form a single-layer TeO2 film. Then, 20 sccm of high-purity nitrogen is introduced for 20 seconds to complete a single growth cycle.

[0062] (5) Repeat the above growth cycle to obtain TeO2 thin film.

[0063] In this embodiment, the heating temperature of the reaction chamber is set to 100°C, 150°C, 170°C, 200°C, 250°C, 300°C, 330°C, and 350°C respectively to study the effect of the temperature of the reaction chamber on the growth of TeO2 thin film. The number of repeated growth cycles is controlled to be the same. The results are as follows: Figure 2It is shown that when the temperature of the reaction chamber is 100-200℃, the thickness of the deposited film increases with the increase of temperature, but the non-uniformity of the film prepared in this temperature range is greater than 5%; when the temperature of the reaction chamber is 200-300℃, the thickness of the deposited film is basically constant, and the non-uniformity of the film is less than 4%; when the temperature of the reaction chamber is greater than 300℃, the thickness of the deposited film begins to decrease with the increase of temperature. It can be seen that in order to obtain a TeO2 film with suitable film thickness and uniformity, the suitable range of the heating temperature of the reaction chamber is 200-300℃.

[0064] Example 3

[0065] This embodiment relates to a method for growing a TeO2 thin film using ALD technology, wherein Te(OEt)4 is selected as a tellurium precursor source and pure water is used as an oxygen source, and specifically includes the following steps:

[0066] (1) Use acetone, methanol, isopropanol, and pure water to clean the surface of the silicon wafer for 5 minutes in sequence to remove the surface organic matter. Then place the treated silicon wafer in the HF solution for 30 seconds to etch away the natural oxide layer on the surface of the silicon wafer. Place the treated silicon wafer in the ALD equipment reaction chamber within 1 minute and evacuate it to less than 1Torr.

[0067] (2) Input deposition working parameters: the heating temperature of Te(OEt)4 is set to 120℃; the water temperature is room temperature; the heating temperature of the reaction chamber is set to 250℃. Set the pipeline carrier gas auxiliary and the flow rate to 20sccm. Before coating, the reaction chamber and the source bottle are heated stably for about 1h, during which high-purity nitrogen is introduced into the reaction chamber of the ALD equipment for purging.

[0068] (3) Coating was started by introducing Te(OEt)4 into the reaction chamber through carrier gas with a pulse time of 2 s, and then 20 sccm of high-purity nitrogen was introduced for 20 s of purge.

[0069] (4) Water is introduced into the reaction chamber via a carrier gas to react with Te(OEt)4 adsorbed on the silicon wafer to form a single-layer TeO2 film. Then, 20 sccm of high-purity nitrogen is introduced for 20 seconds to complete a single growth cycle.

[0070] (5) Repeat the above growth cycle 500 times to obtain a 10 nm thick TeO2 film.

[0071] The film prepared in this example was characterized by X-ray diffraction (XRD). Figure 3 As shown, diffraction peaks belonging to the (1 1 1), (2 0 0), (2 1 2), and (3 2 2) crystal planes of TeO2 can be observed, further indicating that the TeO2 thin film was successfully prepared by combining the above-mentioned precursor source with the ALD technology.

[0072] To further verify the uniformity and repeatability of the TeO2 thin film grown by the above method, the preparation was repeated three times, and the uniformity of the prepared thin films 1, 2, and 3 was tested. The test method is as follows: 5 sites were taken from the prepared TeO2 thin film, the thickness value of each point was measured, and the non-uniformity of each thin film was calculated (non-uniformity = variance / film thickness). The test results are shown in Table 1 below:

[0073] Table 1 Sample uniformity test results

[0074] sample Film 1 Film 2 Film 3 Site 1(nm) 10.30 10.20 10.40 Site 2 (nm) 10.00 9.90 10.10 Site 3 (nm) 10.50 10.30 10.50 Site 4 (nm) 10.70 10.90 10.90 Site 5 (nm) 10.80 10.60 10.70 Average value (nm) 10.46 10.38 10.52 Standard Deviation 0.32 0.38 0.30 Inhomogeneity 3.06% 3.66% 2.85%

[0075] like Figure 4 As shown, the non-uniformity of the repeatedly prepared films 1 to 3 is less than 4%, which also shows that the present invention can prepare a TeO2 film with good uniformity through the ALD technology.

[0076] Comparative Example 1

[0077] This comparative example relates to a method for growing a TeO2 thin film using ALD technology, wherein Te(OEt)4 is selected as a tellurium precursor source and O3 is selected as an oxygen source, and specifically comprises the following steps:

[0078] (1) Use acetone, methanol, isopropanol, and pure water to clean the surface of the silicon wafer for 5 minutes in sequence to remove the surface organic matter. Then place the treated silicon wafer in the HF solution for 30 seconds to etch away the natural oxide layer on the surface of the silicon wafer, and place the treated silicon wafer in the ALD equipment reaction chamber within 1 minute.

[0079] (2) Input deposition working parameters: The heating temperature of Te(OEt)4 is set to 120℃; the parameters of the ozone generator are set to: set the power to 150W, set the O2 pressure to 0.05Mpa, and set the O2 flow rate to 1LPM; the heating temperature of the reaction chamber is set to 250℃. Set the O3 flow rate to 15sccm, the pipeline needs carrier gas assistance, and set the flow rate to 20sccm. Before coating, first heat the reaction chamber and the source bottle stably for about 1h, during which time high-purity nitrogen is introduced into the reaction chamber of the ALD equipment for purge.

[0080] (3) Coating was started by introducing Te(OEt)4 into the reaction chamber through carrier gas with a pulse time of 2 s, and then 20 sccm of high-purity nitrogen was introduced for 20 s of purge.

[0081] (4) O3 is introduced into the reaction chamber via carrier gas, but it does not react with Te(OEt)4 adsorbed on the silicon wafer, and a TeO2 film cannot be obtained.

[0082] Comparative Example 2

[0083] This comparative example relates to a method for growing a TeO2 thin film using ALD technology, wherein bis(trimethylsilyl)tellurium (Te(TMS)2) is selected as a tellurium precursor source and water is used as an oxygen source, and the operation is the same as in Example 1. After 400 deposition cycles, it was determined that no TeO2 thin film was grown on the substrate.

[0084] In addition, ozone and oxygen were used to replace water as oxygen sources to prepare TeO2 thin films. The operation was the same as that in Comparative Example 1. When oxygen was used as the oxygen source, the O2 flow rate was set to 15 sccm. When ozone and oxygen were used as the oxygen source, no TeO2 thin film was prepared.

[0085] The above-described embodiments are only preferred embodiments for fully illustrating the present invention, and the protection scope of the present invention is not limited thereto. Equivalent substitutions or changes made by those skilled in the art based on the present invention are within the protection scope of the present invention. The protection scope of the present invention shall be subject to the claims.

Claims

1. A method for growing TeO2 thin film using ALD technology, characterized in that: The following steps are involved: (1) Placing the substrate after wet chemical treatment in the reaction chamber of an atomic layer deposition device, and introducing a tellurium precursor source to chemically adsorb on the surface of the substrate; the tellurium precursor source is Te(OEt)4; the wet chemical treatment is specifically as follows: using acetone, methanol, isopropanol, and pure water to clean the substrate in sequence for 5 to 10 minutes to remove organic matter on the surface, and then soaking the cleaned silicon wafer in an HF solution to etch and remove the oxide layer on the surface of the substrate; (2) After the chemical adsorption in step (1) is saturated, nitrogen or an inert gas is introduced into the reaction chamber for purging, and then an oxygen source is introduced for reaction; the oxygen source is water; (3) After the reaction in step (2) is completed, nitrogen or an inert gas is introduced into the reaction chamber for purging to complete a single growth cycle; (4) Repeating the above growth cycle to grow the TeO2 thin film on the substrate surface; Before growing the TeO2 film, the reaction chamber and the tellurium precursor source are heated; the heating temperature of the tellurium precursor source is 120-150°C; the heating temperature of the reaction chamber is 150-400°C.

2. The method according to claim 1, characterized in that In step (1), the substrate includes silicon, silicon dioxide, silicon nitride, silicon carbide, glass, sapphire, gallium nitride, or stainless steel having a planar or non-planar surface.

3. The method according to claim 1, characterized in that The tellurium precursor source and the oxygen source are charged into the reaction chamber in a pulsed form in the presence of a carrier gas, and the carrier gas is nitrogen with a purity of not less than 99.999%.

4. The method according to claim 1, characterized in that: In step (2) and step (3), the inert gas is Ar or He; the purity of the nitrogen or inert gas is not less than 99.999%.

5. A TeO2 thin film prepared according to the method according to any one of claims 1 to 4.

6. Use of the TeO2 thin film according to claim 5 in the fields of optics and electronics.