A method for recovering AgWCC block scraps by treating with molten caustic soda
Through the molten caustic soda treatment method, the electrolytic recycling of silver and chemical precipitation of molten caustic soda is used to purify and electrolyte the recovery of silver and chemical precipitation, which solves the problems of low recycling efficiency and high pollution of AgWCC block scraps, and achieves efficient and environmentally friendly silver and WO3 recycling. Avoid emissions of harmful substances.
Patent Information
- Application Number
- CN202211234577.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-10-10
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2042-10-10
Abstract
Description
Technical Field
[0001] The invention belongs to the field of alloy waste recycling, and in particular relates to a method for recycling AgWCC block scraps through molten caustic soda treatment. Background Art
[0002] AgWCC material is one of the most important and largest-volume static contact materials for circuit breakers. AgWCC material is generally made using a powder metallurgy sintering process, which produces a large amount of scraps. AgWCC contact materials and their scraps can be divided into powder scraps and block scraps according to their shapes. Block scraps are difficult to recycle and have problems such as low recycling efficiency and high pollution. The difficulty in handling block scraps is mainly because AgWCC scraps contain both tough Ag and high-strength WC, which makes it difficult to carry out refinement processes such as crushing before scrap recycling.
[0003] In the industry, direct nitric acid dissolution wet method is commonly used for recycling AgWCC scraps. Since WC and graphite are not treated in advance, silver liquid is easily absorbed by graphite and WC during the acid dissolution process, resulting in incomplete recovery and low silver recovery rate. At the same time, the block scraps also have the problem of slow reaction.
[0004] Application No. CN 111118289 A discloses a decarbonization-nitric acid dissolution recovery process, but does not study the crushing of AgWCC block scraps into fine particles. In fact, conventional crushing, ball milling, rolling and other methods are difficult to achieve ideal crushing effects on AgWCC materials. At the same time, this scheme still uses nitric acid to dissolve Ag to recover Ag. This method cannot avoid the emission of a large amount of harmful substances during the recovery process, such as nitric oxide, nitrogen dioxide, hydrazine hydrate, ammonia and other wastes. Summary of the invention
[0005] The purpose of the present invention is to overcome the shortcomings and deficiencies of the prior art and to provide a method for recovering AgWCC block scraps by treating with molten caustic soda.
[0006] The technical solution adopted by the present invention is as follows: A method for recovering AgWCC block scraps by treating with molten caustic soda, comprising the following steps:
[0007] (1) Soaking: Soak the AgWCC block corner material in pure water to fully absorb water;
[0008] (2) Crushing: Separating the soaked AgWCC block scraps from pure water and arranging them in a corundum boat, and then pushing the corundum boat into a heating furnace. During the heating process, water vapor expands and explodes the AgWCC block scraps from the inside, causing the AgWCC block scraps to explode and delaminate or form internal cracks, thereby forming AgWCC scraps.
[0009] (3) Purification by molten caustic soda: The AgWCC scraps are transferred to a pure silver crucible, molten caustic soda is added, oxygen is continuously introduced into the resistance furnace and heated, and after sufficient reaction, the mixture is filtered and separated to obtain a solid silver scrap skeleton and a liquid mixed solution of Na2WO4 and caustic soda;
[0010] (4) Electrolytic recovery of silver: sintering the silver horn skeleton into a crude silver slab in a graphite boat, placing the crude silver slab into an electrolytic cell for anode electrolysis, and recovering electrolytic silver powder at the cathode;
[0011] (5) Chemical precipitation to recover WO3: Add excess hydrochloric acid to the mixed solution of Na2WO4 and caustic soda obtained in step (3) to obtain H2WO4 precipitate, and adjust the pH value. Wash the H2WO4 precipitate with pure water and filter to remove impurities to obtain a mixture of H2WO4 and water. Heat the H2WO4 and water mixture in an oven to dehydrate and obtain WO3 powder.
[0012] It is further configured that, in step (1), the soaking time of the AgWCC block scrap material is 24-48 hours.
[0013] A further configuration is that in step (2), the heating furnace is a medium frequency induction heating furnace, the heating temperature is controlled at 800-950° C., and the heating time is 10-60 s.
[0014] It is further configured that in step (3), the heating temperature of the resistance furnace is 600-700°C, the heating time is 4-6h, and the oxygen flow rate is 0.5-1.0m³ / h.
[0015] It is further configured that in step (4), the electrolyte in the electrolytic cell is a 5-15wt% silver nitrate solution, and the electrolysis voltage is 2.5-5.0V.
[0016] Further configuration is that in step (5), the hydrochloric acid is 37 wt % concentrated hydrochloric acid, the pH value adjustment range is 6.3-6.8, the heating dehydration temperature is 200-300° C., and the heating dehydration time is 5-20 h.
[0017] The beneficial effects of the present invention are as follows:
[0018] 1. This scheme takes advantage of the fact that there are about 2-3% pores in the sintered contact material, and uses water immersion plus induction heating to quickly heat up the temperature to create defects inside the contact to provide a guarantee for further recycling in the later stage. The induction heating efficiency of the contact scrap can reach 100℃ / s. At 100℃, liquid water quickly transforms into gaseous water and the volume increases by more than 1,300 times. If the temperature continues to rise to about 900℃, the volume of water vapor will increase by about 3 times. That is, within 10s, the volume of water vapor inside the material will expand by 3,900 times. The volume of water vapor will gather and increase in a short time, which can cause the AgWCC scrap to withstand huge internal stress and explode. Layered cracks, microcracks, pores, etc. are created inside the scrap block to make recycling easier.
[0019] 2. Use molten caustic soda and oxygen to remove WC and C components in the scraps at the same time. In the process of molten caustic soda to purify the scraps, Ag neither undergoes phase change nor participates in any chemical reaction. Compared with the traditional nitric acid dissolution process of Ag, the problem of Ag loss caused by incomplete solution separation and flushing consumption during the recovery process is greatly reduced. The recovery rate of Ag in the scraps is more than 99.8%, the purity of the recovered electrolytic Ag is more than 99.95%, the recovery rate of W in WC is more than 98.0%, and the purity of the recovered WO3 powder is 99.9%.
[0020] 3. This recycling method only needs to use caustic soda and hydrochloric acid and other chemicals in the recycling process to recover the final products of the reaction, Ag, WO3, CO2 gas, and NaCl solution. Ag and WO3 can be recycled and reused, and CO2 and NaCl solutions are environmentally friendly. Compared with the conventional nitric acid dissolution recovery process, it eliminates the discharge of harmful gases such as nitric oxide, nitrogen dioxide, ammonia water, and hydrazine hydrate, and is a green and environmentally friendly recycling process. DETAILED DESCRIPTION
[0021] In order to make the purpose, technical solutions and advantages of the present invention more clear, the present invention will be described in further detail below.
[0022] Embodiment 1
[0023] Weigh 5kg of AgWC12C3 block scraps and soak them all in pure water for 24 hours. Arrange the soaked scraps in a corundum boat, push the corundum boat into an induction furnace, set the maximum temperature of the induction furnace to 900℃, and heat for 10s to make the scraps explode.
[0024] To ensure that WC reacts completely, the amount of caustic soda added is in excess of the weight of WC, i.e. 0.6kg. The cracked block scraps are loaded into a silver crucible together with 0.6kg NaOH, and oxygen is continuously introduced at an oxygen flow rate of 1m³ / hour. The crucible is placed in a resistance furnace and heated to 650℃, so that the WC in the scraps is reacted into Na2WO4 and C is reacted into CO2.
[0025] The silver scraps purified by caustic soda are sintered into plates, and the plate-shaped silver scraps are hung in a 10wt% silver nitrate solution electrolytic cell as anode. The cell voltage is adjusted to 4.5V, and pure electrolytic silver powder is recovered at the cathode.
[0026] The mixed solution of Na2WO4 and caustic soda was filtered to remove impurities, 37wt% concentrated hydrochloric acid was added to the filtrate to precipitate H2WO4, and the pH value was adjusted to 6.5 to ensure complete precipitation and complete reaction of NaOH. The H2WO4 scraps were filtered and washed to obtain a mixture of H2WO4 and water, and the mixture was dried and dehydrated in an oven at 300°C for 5 hours to obtain pure WO3 powder.
[0027] The purity of recovered electrolytic Ag is over 99.96% after testing, and the purity of recovered WO3 powder is 99.91%; the recovery rate of electrolytic Ag powder is 99.85%, and the recovery rate of W in WC is 98.52%.
[0028] Embodiment 2
[0029] Weigh 10kg of AgWC22C3 block scraps and soak them all in pure water for 48 hours. Arrange the soaked scraps in a corundum boat, push the corundum boat into an induction furnace, set the maximum temperature of the induction furnace to 800℃, and heat for 15s to make the scraps burst.
[0030] To ensure that WC reacts completely, the amount of caustic soda added is in excess of the weight of WC, i.e. 2.2kg. The cracked block scraps are loaded into a silver crucible together with 2.2kg NaOH, and oxygen is continuously introduced at an oxygen flow rate of 0.8m³ / hour. The crucible is placed in a resistance furnace and heated to 600℃, so that the WC in the scraps is reacted into Na2WO4 and C is reacted into CO2.
[0031] The silver scraps purified by caustic soda are sintered into plates, and the plate-shaped silver scraps are hung in a 15wt% silver nitrate solution electrolytic cell as anode. The cell voltage is adjusted to 2.5V, and pure electrolytic silver powder is recovered at the cathode.
[0032] The mixed solution of Na2WO4 and caustic soda was filtered to remove impurities, 37wt% concentrated hydrochloric acid was added to the filtrate to precipitate H2WO4, and the pH value was adjusted to 6.8 to ensure complete precipitation and complete reaction of NaOH. The H2WO4 scraps were filtered and washed to obtain a mixture of H2WO4 and water, and the mixture was dried and dehydrated in an oven at 280°C for 10 hours to obtain pure WO3 powder.
[0033] The purity of recovered electrolytic Ag is above 99.95% after testing, and the purity of recovered WO3 powder is 99.95%; the recovery rate of electrolytic Ag powder is 99.85%, and the recovery rate of W in WC is 98.13%.
[0034] Embodiment 3
[0035] Weigh 15kg of AgWC15C3 block scraps and soak them all in pure water for 36 hours. Arrange the soaked scraps in a corundum boat, push the corundum boat into an induction furnace, set the maximum temperature of the induction furnace to 950℃, and heat for 25s to make the scraps burst.
[0036] To ensure that WC reacts completely, NaOH is added in excess according to the weight of WC, i.e. 2.2kg. The cracked block scraps and 2.2kg NaOH are placed in a silver crucible, oxygen is continuously introduced at an oxygen flow rate of 1m³ / hour, and the crucible is placed in a resistance furnace and heated to 700℃, so that the WC in the scraps is reacted into Na2WO4 and C is reacted into CO2.
[0037] The silver scraps purified by caustic soda are sintered into plates, and the plate-shaped silver scraps are hung in a 12wt% silver nitrate solution electrolytic cell as anode. The cell voltage is adjusted to 3.5V, and pure electrolytic silver powder is recovered at the cathode.
[0038] The mixed solution of Na2WO4 and caustic soda was filtered to remove impurities, 37wt% concentrated hydrochloric acid was added to the filtrate to precipitate H2WO4, and the pH value was adjusted to 6.3 to ensure complete precipitation and complete reaction of NaOH. The H2WO4 scraps were filtered and washed to obtain a mixture of H2WO4 and water, and the mixture was dried and dehydrated in an oven at 300°C for 20 hours to obtain pure WO3 powder.
[0039] The purity of recovered electrolytic Ag is over 99.97% after testing, and the purity of recovered WO3 powder is 99.91%; the recovery rate of electrolytic Ag powder is 99.87%, and the recovery rate of W in WC is 98.35%.
[0040] Embodiment 4
[0041] Weigh 20kg of AgWC27C3 block scraps and soak them all in pure water for 24 hours. Arrange the soaked scraps in a corundum boat, push the corundum boat into the induction furnace, set the maximum temperature of the induction furnace to 920℃, and heat for 30s to make the scraps burst.
[0042] To ensure that WC reacts completely, the amount of caustic soda added is in excess of the weight of WC, i.e. 5.4kg. The cracked block scraps and 5.4kg NaOH are placed in a silver crucible, oxygen is continuously introduced at an oxygen flow rate of 1m³ / hour, and the crucible is placed in a resistance furnace and heated to 650℃, so that the WC in the scraps is reacted into Na2WO4 and C is reacted into CO2.
[0043] The silver scraps purified by caustic soda are sintered into plates, and the plate-shaped silver scraps are hung in a 10wt% silver nitrate solution electrolytic cell as anode. The cell voltage is adjusted to 4.0V, and pure electrolytic silver powder is recovered at the cathode.
[0044] The mixed solution of Na2WO4 and caustic soda was filtered to remove impurities, 37wt% concentrated hydrochloric acid was added to the filtrate to precipitate H2WO4, and the pH value was adjusted to 6.8 to ensure complete precipitation and complete reaction of NaOH. The H2WO4 scraps were filtered and washed to obtain a mixture of H2WO4 and water, and the mixture was dried and dehydrated in an oven at 200°C for 12 hours to obtain pure WO3 powder.
[0045] The purity of recovered electrolytic Ag is over 99.98% after testing, and the purity of recovered WO3 powder is 99.90%; the recovery rate of electrolytic Ag powder is 99.90%, and the recovery rate of W in WC is 98.61%.
[0046] Embodiment 5
[0047] Weigh 8kg of AgWC15C2 block scraps and soak them all in pure water for 48 hours. Arrange the soaked scraps in a corundum boat, push the corundum boat into an induction furnace, set the maximum temperature of the induction furnace to 850℃, and heat for 40s to make the scraps burst.
[0048] To ensure that WC reacts completely, the amount of caustic soda added is in excess of the weight of WC, i.e. 1.2kg. The cracked block scraps are loaded into a silver crucible together with 1.2kg NaOH, and oxygen is continuously introduced at an oxygen flow rate of 1m³ / hour. The crucible is placed in a resistance furnace and heated to 600℃, so that the WC in the scraps is reacted into Na2WO4 and C is reacted into CO2.
[0049] The silver scraps purified by caustic soda are sintered into plates, and the plate-shaped silver scraps are hung in a 5wt% silver nitrate solution electrolytic cell as anode. The cell voltage is adjusted to 5.0V, and pure electrolytic silver powder is recovered at the cathode.
[0050] The mixed solution of Na2WO4 and caustic soda was filtered to remove impurities, 37wt% concentrated hydrochloric acid was added to the filtrate to precipitate H2WO4, and the pH value was adjusted to 6.7 to ensure complete precipitation and complete reaction of NaOH. The H2WO4 scraps were filtered and washed to obtain a mixture of H2WO4 and water, and the mixture was dried and dehydrated in an oven at 250°C for 10 hours to obtain pure WO3 powder.
[0051] The purity of recovered electrolytic Ag is over 99.96% after testing, and the purity of recovered WO3 powder is 99.92%; the recovery rate of electrolytic Ag powder is 99.92%, and the recovery rate of W in WC is 98.57%.
[0052] The above disclosure is only the preferred embodiment of the present invention, which certainly cannot be used to limit the scope of the present invention. Therefore, equivalent changes made according to the claims of the present invention are still within the scope of the present invention.
Claims
1. A method for recovering AgWCC block scraps by treating with molten caustic soda, characterized in that The following steps are involved: (1) Soaking: Soak the AgWCC block corner material in pure water to fully absorb water; (2) Crushing: Separating the soaked AgWCC block scraps from pure water and arranging them in a corundum boat, and then pushing the corundum boat into a heating furnace. During the heating process, water vapor expands and explodes the AgWCC block scraps from the inside, causing the AgWCC block scraps to explode and delaminate or form internal cracks, thereby forming AgWCC scraps. (3) Purification by molten caustic soda: The AgWCC scraps are transferred to a pure silver crucible, molten caustic soda is added, oxygen is continuously introduced into the resistance furnace and heated, and after sufficient reaction, the mixture is filtered and separated to obtain a solid silver scrap skeleton and a liquid mixed solution of Na2WO4 and caustic soda; (4) Electrolytic recovery of silver: sintering the silver horn skeleton into a crude silver slab in a graphite boat, placing the crude silver slab into an electrolytic cell for anode electrolysis, and recovering electrolytic silver powder at the cathode; (5) Chemical precipitation to recover WO3: Add excess hydrochloric acid to the mixed solution of Na2WO4 and caustic soda obtained in step (3) to obtain H2WO4 precipitate, and adjust the pH value. Wash the H2WO4 precipitate with pure water and filter to remove impurities to obtain a mixture of H2WO4 and water. Heat the H2WO4 and water mixture in an oven to dehydrate and obtain WO3 powder.
2. The method for recovering AgWCC block scraps by molten caustic soda treatment according to claim 1, characterized in that: In step (1), the soaking time of the AgWCC block scrap is 24-48 hours.
3. The method for recovering AgWCC block scraps by molten caustic soda treatment according to claim 1, characterized in that: In step (2), the heating furnace is a medium frequency induction heating furnace, the heating temperature is controlled at 800-950°C, and the heating time is 10-60s.
4. The method for recovering AgWCC block scraps by molten caustic soda treatment according to claim 1, characterized in that: In step (3), the resistance furnace is heated to a temperature of 600-700°C, a heating time of 4-6 hours, and an oxygen flow rate of 0.5-1.0 m³ / h.
5. The method for recovering AgWCC block scraps by molten caustic soda treatment according to claim 1, characterized in that: In step (4), the electrolyte in the electrolytic cell is a 5-15wt% silver nitrate solution, and the electrolysis voltage is 2.5-5.0V.
6. The method for recovering AgWCC block scraps by molten caustic soda treatment according to claim 1, characterized in that: In step (5), the hydrochloric acid is 37 wt % concentrated hydrochloric acid, the pH value is adjusted in the range of 6.3-6.8, the heating dehydration temperature is 200-300° C., and the heating dehydration time is 5-20 h.