Preparation method of antibacterial needle-punched filter felt with dye adsorption effect
By preparing and modifying porous titanium dioxide microspheres for in-situ polymerization on needle-punched felt, the problem of conventional needle-punched felt being unable to treat dye wastewater was solved, achieving efficient adsorption and antibacterial effects.
Patent Information
- Application Number
- CN202211025012.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-08-25
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2042-08-25
AI Technical Summary
Conventional needle-punched filter felt cannot effectively screen out dyes in dye wastewater, and bacteria in the dye wastewater can clog the pores and produce an unpleasant odor.
Porous titanium dioxide microspheres were prepared and grafted to give them double bonds. Then, they were polymerized in situ with organic monomers on needle-punched felt. The porous titanium dioxide was then loaded onto the needle-punched felt using ultraviolet light curing, which endowed it with dye adsorption and antibacterial functions.
It achieves efficient adsorption of dyes and antibacterial properties of needle-punched felt, avoids pore clogging, and improves the durability and effectiveness of use.
Smart Images

Figure CN115595793B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of needle-punched felt preparation, and in particular relates to a method for preparing an antibacterial needle-punched filter felt with dye adsorption efficacy. Background Art
[0002] At present, dye wastewater is a type of seriously polluted wastewater, and sedimentation method is often used to treat dye wastewater. However, the sedimentation method has a long cycle and many operating procedures. Using needle felt as filter material to treat dye wastewater has the characteristics of simple operation, high treatment efficiency and low cost. However, conventional needle-punched filter felt cannot be used to treat dye wastewater because the dye is at the molecular level, and the filter felt is a material with holes. Its gaps are large, far exceeding the size of dye molecules, making it impossible to effectively screen the dye. The development of needle-punched felt that can adsorb dyes has certain practical significance. In addition, there are often some bacteria in dye wastewater. These bacteria will gather together to block the holes of the needle-punched felt. Over time, organic humus will be produced, producing an unpleasant odor. If the needle-punched filter felt can be given a certain antibacterial property while adsorbing the dye, it will be expected to avoid the embarrassing odor produced during wastewater treatment.
[0003] Through the above analysis, the problems and defects of the prior art are as follows: conventional needle-punched filter felt cannot be used to treat dye wastewater and cannot effectively screen dyes. Bacteria in dye wastewater will clog the holes of the needle-punched felt, produce organic humus, and produce unpleasant odors. Summary of the invention
[0004] In view of the problems existing in the prior art, the present invention provides a method for preparing an antibacterial needle-punched filter felt with dye adsorption efficacy.
[0005] The present invention is implemented by first preparing porous titanium dioxide microspheres with dye adsorption and antibacterial functions, then grafting and modifying them with a silane coupling agent to give them double bonds that can undergo polymerization reactions, and then, under the action of a photoinitiator, titanium dioxide with double bonds and organic monomers undergo in-situ polymerization reactions on the needle felt. The loading of porous titanium dioxide microspheres on the needle felt gives the needle felt dye adsorption and antibacterial functions.
[0006] A method for preparing an antibacterial needle-punched filter felt having dye adsorption efficacy specifically comprises:
[0007] Step 1, using water and hexadecyltrimethylammonium bromide as phase A, and using ethanol, butyl titanate, cyclohexane and n-pentanol as phase B, mixing phase A and phase B evenly, placing in a high shear homogenizer and stirring at high speed for 20 minutes, then taking out and placing in a hydrothermal reactor, reacting for 7 hours, taking out and centrifuging and washing, then placing the obtained powder in a muffle furnace at 600° C. and calcining for 5 hours, and finally dispersing the calcined powder in a mixed solution of water and ethanol to obtain a porous titanium dioxide microsphere dispersion;
[0008] Step 2: adding a silane coupling agent to the titanium dioxide microsphere dispersion obtained in step 1, grafting and modifying the porous titanium dioxide microspheres at 70° C. to obtain a titanium dioxide microsphere dispersion with double bonds, which is set aside;
[0009] Step 3, dissolving the photoinitiator in the organic monomer to obtain a mixed solution, then spraying the mixed solution on the needle-punched felt, and rolling it with a rolling mill to obtain a needle-punched filter felt loaded with the organic monomer and the photoinitiator for standby use;
[0010] Step 4, spraying the titanium dioxide microsphere dispersion with double bonds obtained in step 2 onto the needle-punched filter felt obtained in step 3, and rolling it with a rolling car, and then irradiating the needle-punched filter felt with ultraviolet light. After drying, an antibacterial needle-punched filter felt with dye adsorption effect can be obtained.
[0011] Furthermore, in step 1, the rotation speed of the high shear homogenizer is 3500 r / min; after being placed in the hydrothermal reactor, the stirring rate is controlled to be 150 r / min, and the timing is started when the temperature rises to 120°C.
[0012] Furthermore, the particle size of the titanium dioxide microspheres in step 1 is 300-600 nm.
[0013] Furthermore, in step 1, the calcined powder is dispersed in a mixture of water and ethanol, wherein the mass ratio of water to ethanol is 7:3.
[0014] Furthermore, the silane coupling agent in step 2 is γ-methacryloxypropyltrimethoxysilane.
[0015] Furthermore, the photoinitiator in step three is one of diphenyl-(2,4,6-trimethylbenzoyl)phosphine oxide and 2-hydroxy-2-methyl-1-phenylacetone.
[0016] Furthermore, the amount of the photoinitiator in step three is 1%-1.5% of the organic monomer.
[0017] Furthermore, the organic monomer in step three is one of hydroxyethyl acrylate and hydroxypropyl acrylate.
[0018] Furthermore, the needle-punched felt in step three is one of polyester and polypropylene.
[0019] Furthermore, the central wavelength of the ultraviolet light in step 4 is 365 nm.
[0020] In combination with the above technical solutions and the technical problems solved, please analyze the advantages and positive effects of the technical solutions to be protected by the present invention from the following aspects:
[0021] First, in view of the technical problems existing in the above-mentioned prior art and the difficulty of solving the problems, the technical solutions to be protected by the present invention and the results and data during the research and development process are closely combined to analyze in detail and deeply how the technical solutions of the present invention solve the technical problems, and some creative technical effects brought about after solving the problems. The specific description is as follows:
[0022] The nano-scale porous titanium dioxide in the present invention has a high specific surface area and can achieve adsorption of anionic dyes; the crystal form of titanium dioxide is anatase type, which has certain antibacterial effects. Directly loading porous titanium dioxide on needle-punched felt by rolling, dipping or spraying cannot ensure firmness, and titanium dioxide will fall off; if an adhesive is applied, the adhesive will block the pores of titanium dioxide, thereby causing titanium dioxide to lose its adsorption capacity. For this reason, the present application proposes to first chemically modify the porous titanium dioxide so that it has double bonds, and then the titanium dioxide with double bonds will react with organic monomers in situ under the action of ultraviolet light initiators to achieve a firm load of porous titanium dioxide on the needle-punched felt. The porous titanium dioxide microspheres are loaded on the needle-punched filter felt by ultraviolet light curing, and the adsorption and antibacterial properties of the porous titanium dioxide are utilized to obtain an antibacterial needle-punched filter felt with dye adsorption efficacy.
[0023] Step one in the present invention is to obtain porous titanium dioxide microspheres with dye adsorption and antibacterial functions; compared with carbon dioxide microspheres without pores, porous titanium dioxide microspheres have a larger specific surface area and a stronger ability to adsorb dyes. At the same time, it is also easier to "lock" the adsorbed dyes to prevent them from migrating or precipitating from the surface of the microspheres.
[0024] Step 2 in the present invention is to graft-modify porous titanium dioxide microspheres with a silane coupling agent with double bonds to obtain titanium dioxide microspheres with double bonds. The double bonds can give the titanium dioxide microspheres reactivity. The titanium dioxide modified by the silane coupling agent is similar to an organic monomer and can undergo polymerization reaction with other monomers under the action of an initiator. In order to prevent the silane coupling agent from clogging the pores of the titanium dioxide microspheres during the grafting modification process, the present invention adopts a technology different from the conventional silane coupling agent modification. The present application adopts an intermittent feeding method, that is, the silane coupling agent is added to the titanium dioxide microsphere dispersion in batches to prevent the grafting rate from being fast and the coupling agent from aggregating, thereby avoiding the clogging of the microsphere pores.
[0025] The third step of the present invention is to load the organic monomer and the photoinitiator on the needle-punched felt.
[0026] Step 4 in the present invention is to mix the reactive titanium dioxide with the monomer and initiator in step 3. Under the irradiation of ultraviolet light, a polymerization reaction occurs between the monomers, thereby fixing the porous titanium dioxide on the needle felt, while giving the needle felt dye adsorption properties and antibacterial properties, preventing the porous titanium dioxide from falling off, and improving its fixation on the needle felt. Similarly, the present application has thought of the problem that when ultraviolet light triggers the reaction of organic monomers and titanium dioxide, the polymerization reaction products will block the titanium dioxide pores, and a strategy of first loading the organic monomers and photoinitiators on the needle felt, and then applying titanium dioxide for reaction is proposed. In this case, titanium dioxide will be polymerized and cured in situ with the pre-loaded organic monomers, and the organic monomers will not leak into the pores of the titanium dioxide microspheres, thus avoiding pore blockage.
[0027] Second, considering the technical solution as a whole or from the perspective of the product, the technical effects and advantages of the technical solution to be protected by the present invention are described in detail as follows:
[0028] The present invention first prepares porous titanium dioxide microspheres with dye adsorption and antibacterial functions, and then uses a silane coupling agent to graft and modify the microspheres so that they have double bonds that can undergo polymerization reactions. Then, under the action of a photoinitiator, the titanium dioxide with double bonds and an organic monomer undergo an in-situ polymerization reaction on the needle-punched felt. The loading of the porous titanium dioxide microspheres on the needle-punched felt gives the needle-punched felt dye adsorption and antibacterial functions. Ultraviolet light initiates in-situ polymerization, which has the advantages of high efficiency and short time. After in-situ polymerization, the titanium dioxide microspheres are firmly attached to the needle-punched felt and will not fall off, thereby ensuring the long-term use thereof. The needle-punched filter felt of the present invention is cleverly designed, and not only has the function of adsorbing dyes but also has antibacterial properties; in the needle-punched filter felt of the present invention, the porous titanium dioxide loading is highly firm and not easy to fall off.
[0029] Third, as auxiliary evidence of the inventiveness of the claims of the present invention, it is also reflected in the following important aspects:
[0030] The technical solution of the present invention fills the technical gap in the industry at home and abroad: needle felt has the advantage of low price for filtering wastewater, which is unmatched by membrane materials. However, needle felt made of non-woven fabrics has rarely been used for filtering dye wastewater before, because the pores of needle felt are relatively large, far exceeding the molecular size of the dye, making it difficult to intercept it. The present invention loads porous titanium dioxide microspheres with dye adsorption and antibacterial functions on needle felt, and uses it for filtering dye wastewater. It can not only enable the needle felt to capture dyes, but also disinfect and treat some bacteria in the water body with antibacterial treatment, ensuring that the water body is cleaner and safer.
[0031] (2) Whether the technical solution of the present invention overcomes technical prejudice:
[0032] The present invention first prepares porous titanium dioxide microspheres with dye adsorption and antibacterial functions, then uses a silane coupling agent to graft and modify them so that they carry double bonds that can undergo polymerization reactions, and then under the action of a photoinitiator, the titanium dioxide with double bonds and an organic monomer undergo an in-situ polymerization reaction on the needle-punched felt. The present invention greatly improves the fixation of porous titanium dioxide on the needle-punched felt through in-situ polymerization, and overcomes the problem that when the particles are directly loaded on a substrate such as the needle-punched felt through post-finishing, the particles are easy to fall off and the fixation is poor. BRIEF DESCRIPTION OF THE DRAWINGS
[0033] Figure 1 The present invention is a flowchart of a method for preparing an antibacterial needle-punched filter felt having dye adsorption efficacy provided in an embodiment of the present invention. DETAILED DESCRIPTION
[0034] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.
[0035] In order to enable those skilled in the art to fully understand how to implement the present invention in detail, this section is an explanatory embodiment that expands and describes the technical solution of the claims.
[0036] like Figure 1 As shown, the method for preparing the antibacterial needle-punched filter felt with dye adsorption effect provided by the embodiment of the present invention comprises:
[0037] S101, using water and hexadecyltrimethylammonium bromide as phase A, and ethanol, butyl titanate, cyclohexane and n-pentanol as phase B, mixing phase A and phase B evenly, placing in a high shear homogenizer and stirring at high speed for 20 minutes, then taking out and placing in a hydrothermal reactor, reacting for 7 hours, taking out and centrifuging and washing, then placing the obtained powder in a muffle furnace at 600°C and calcining for 5 hours, and finally dispersing the calcined powder in a mixed solution of water and ethanol to obtain a porous titanium dioxide microsphere dispersion;
[0038] S102, adding a silane coupling agent to the titanium dioxide microsphere dispersion obtained in step S101, grafting and modifying the porous titanium dioxide microspheres at 70° C. to obtain a titanium dioxide microsphere dispersion with double bonds, which is set aside;
[0039] S103, dissolving a photoinitiator in an organic monomer to obtain a mixed solution, spraying the mixed solution on the needle-punched felt, and rolling it with a rolling mill to obtain a needle-punched filter felt for standby use;
[0040] S104, spraying the titanium dioxide microsphere dispersion with double bonds obtained in step S102 onto the needle-punched filter felt obtained in step 3, and rolling it with a rolling car, and then irradiating the needle-punched filter felt with ultraviolet light, and after drying, an antibacterial needle-punched filter felt with dye adsorption effect can be obtained.
[0041] In step S101 of the embodiment of the present invention, the rotation speed of the high shear homogenizer is 3500 r / min; after being placed in the hydrothermal reactor, the stirring rate is controlled to be 150 r / min, and the timing is started when the temperature rises to 120°C.
[0042] The particle size of the titanium dioxide microspheres in step S101 in the embodiment of the present invention is 300-600 nm.
[0043] In step S101 of the embodiment of the present invention, the calcined powder is dispersed in a mixture of water and ethanol, wherein the mass ratio of water to ethanol is 7:3.
[0044] The silane coupling agent in step S102 in the embodiment of the present invention is γ-methacryloxypropyltrimethoxysilane.
[0045] The photoinitiator in step S103 in the embodiment of the present invention is one of diphenyl-(2,4,6-trimethylbenzoyl)phosphine oxide and 2-hydroxy-2-methyl-1-phenylacetone.
[0046] In the embodiment of the present invention, the amount of the photoinitiator in step S103 is 1%-1.5% of the organic monomer.
[0047] The organic monomer in step S103 in the embodiment of the present invention is one of hydroxyethyl acrylate and hydroxypropyl acrylate.
[0048] The needle-punched felt in step S103 in the embodiment of the present invention is one of polyester and polypropylene.
[0049] The central wavelength of the ultraviolet light in step S104 in the embodiment of the present invention is 365 nm.
[0050] The nano-scale porous titanium dioxide in the present invention has a high specific surface area and can achieve adsorption of anionic dyes; the crystal form of titanium dioxide is anatase type, which has certain antibacterial effects. Directly loading porous titanium dioxide on needle-punched felt by rolling, dipping or spraying cannot ensure firmness, and titanium dioxide will fall off; if an adhesive is applied, the adhesive will block the pores of titanium dioxide, thereby causing titanium dioxide to lose its adsorption capacity. For this reason, the present application proposes to first chemically modify the porous titanium dioxide so that it has double bonds, and then the titanium dioxide with double bonds will react with organic monomers in situ under the action of ultraviolet light initiators to achieve a firm load of porous titanium dioxide on the needle-punched felt. The porous titanium dioxide microspheres are loaded on the needle-punched filter felt by ultraviolet light curing, and the adsorption and antibacterial properties of the porous titanium dioxide are utilized to obtain an antibacterial needle-punched filter felt with dye adsorption efficacy.
[0051] Example 1
[0052] (1) Water and hexadecyltrimethylammonium bromide are used as phase A, ethanol, butyl titanate, cyclohexane and n-pentanol are used as phase B, phase A and phase B are mixed evenly, and then placed in a high shear homogenizer with a rotation speed of 3500 r / min for high-speed stirring for 20 minutes, then taken out and placed in a hydrothermal reactor, and the stirring rate is controlled to be 150 r / min. When the temperature rises to 120°C, the timing is started. After the reaction is completed for 7 hours, the mixture is taken out for centrifugation and washing, and then the obtained powder is placed in a muffle furnace at 600°C for calcination for 5 hours. Finally, the calcined powder is dispersed in a mixed solution of water and ethanol with a mass ratio of 7:3 to obtain a porous titanium dioxide microsphere dispersion;
[0053] (2) adding γ-methacryloxypropyltrimethoxysilane as a silane coupling agent to the titanium dioxide microsphere dispersion obtained in (1), grafting and modifying the porous titanium dioxide microspheres at 70° C. to obtain a titanium dioxide microsphere dispersion with double bonds, which is set aside for later use;
[0054] (3) dissolving a photoinitiator, diphenyl-(2,4,6-trimethylbenzoyl)phosphine oxide (1% by mass of the organic monomer) in an organic monomer, hydroxyethyl acrylate, to obtain a mixed solution, and then spraying the mixed solution on a polyester needle-punched felt, and pressing it with a rolling mill to obtain a needle-punched polyester filter felt for standby use;
[0055] (4) Spraying the titanium dioxide microsphere dispersion with double bonds obtained in step 2 onto the polyester needle-punched filter felt obtained in step (3), and rolling it with a rolling mill, and then irradiating the needle-punched felt with ultraviolet light with a central wavelength of 365 nm. After drying, an antibacterial polyester needle-punched filter felt with dye adsorption effect can be obtained.
[0056] The test showed that the particle size of the titanium dioxide microspheres obtained in (1) was 300 nm, and the removal rate of the polyester needle-punched felt obtained by UV curing for 10 mg / L Sudan red dye solution was as high as 98%. The antibacterial test showed that the antibacterial rate for Staphylococcus aureus reached 93%.
[0057] Example 2
[0058] (1) Water and hexadecyltrimethylammonium bromide are used as phase A, ethanol, butyl titanate, cyclohexane and n-pentanol are used as phase B, phase A and phase B are mixed evenly, and then placed in a high shear homogenizer with a rotation speed of 3500 r / min for high-speed stirring for 20 minutes, then taken out and placed in a hydrothermal reactor, and the stirring rate is controlled to be 150 r / min. When the temperature rises to 120°C, the timing is started. After the reaction is completed for 7 hours, the mixture is taken out for centrifugation and washing, and then the obtained powder is placed in a muffle furnace at 600°C for calcination for 5 hours. Finally, the calcined powder is dispersed in a mixed solution of water and ethanol with a mass ratio of 7:3 to obtain a porous titanium dioxide microsphere dispersion;
[0059] (2) adding γ-methacryloxypropyltrimethoxysilane as a silane coupling agent to the titanium dioxide microsphere dispersion obtained in (1), grafting and modifying the porous titanium dioxide microspheres at 70° C. to obtain a titanium dioxide microsphere dispersion with double bonds, which is set aside for later use;
[0060] (3) dissolving a photoinitiator 2-hydroxy-2-methyl-1-phenylpropanone (1.5% by mass of the organic monomer) in an organic monomer hydroxypropyl acrylate to obtain a mixed solution, spraying the mixed solution on a polypropylene needle-punched felt, and rolling it with a rolling mill to obtain a polypropylene needle-punched filter felt for standby use;
[0061] (4) Spraying the titanium dioxide microsphere dispersion with double bonds obtained in step 2 onto the polypropylene needle-punched filter felt obtained in step (3), and rolling it with a rolling mill, and then irradiating the needle-punched filter felt with ultraviolet light having a central wavelength of 365 nm. After drying, an antibacterial polypropylene needle-punched filter felt with dye adsorption effect can be obtained.
[0062] After testing, the particle size of the titanium dioxide microspheres obtained in (1) is 420nm, and the removal rate of the polypropylene needle felt obtained by UV curing treatment for 10mg / L Sudan red dye solution is as high as 97%; after antibacterial testing, the antibacterial rate against Staphylococcus aureus reaches 91%.
[0063] Example 3
[0064] (1) Water and hexadecyltrimethylammonium bromide are used as phase A, ethanol, butyl titanate, cyclohexane and n-pentanol are used as phase B, phase A and phase B are mixed evenly, and then placed in a high shear homogenizer with a rotation speed of 3500 r / min for high-speed stirring for 20 minutes, then taken out and placed in a hydrothermal reactor, and the stirring rate is controlled to be 150 r / min. When the temperature rises to 120°C, the timing is started. After the reaction is completed for 7 hours, the mixture is taken out for centrifugation and washing, and then the obtained powder is placed in a muffle furnace at 600°C for calcination for 5 hours. Finally, the calcined powder is dispersed in a mixed solution of water and ethanol with a mass ratio of 7:3 to obtain a porous titanium dioxide microsphere dispersion;
[0065] (2) adding γ-methacryloxypropyltrimethoxysilane as a silane coupling agent to the titanium dioxide microsphere dispersion obtained in (1), grafting and modifying the porous titanium dioxide microspheres at 70° C. to obtain a titanium dioxide microsphere dispersion with double bonds, which is set aside for later use;
[0066] (3) dissolving a photoinitiator 2-hydroxy-2-methyl-1-phenylpropanone (1.3% by mass of the organic monomer) in an organic monomer hydroxypropyl acrylate to obtain a mixed solution, spraying the mixed solution on a polypropylene needle-punched felt, and rolling it with a rolling mill to obtain a needle-punched polypropylene filter felt for standby use;
[0067] (4) Spraying the titanium dioxide microsphere dispersion with double bonds obtained in step 2 onto the polypropylene needle-punched filter felt obtained in step (3), and rolling it with a rolling mill, and then irradiating the needle-punched filter felt with ultraviolet light having a central wavelength of 365 nm. After drying, an antibacterial polypropylene needle-punched filter felt with dye adsorption effect can be obtained.
[0068] According to the test, the particle size of the titanium dioxide microspheres obtained in (1) is 450nm, and the removal rate of the polypropylene needle felt obtained by UV curing treatment for 10mg / L Sudan red dye solution is as high as 95%; according to the antibacterial test, the antibacterial rate against Staphylococcus aureus is as high as 90%.
[0069] Example 4
[0070] (1) Water and hexadecyltrimethylammonium bromide are used as phase A, ethanol, butyl titanate, cyclohexane and n-pentanol are used as phase B, phase A and phase B are mixed evenly, and then placed in a high shear homogenizer with a rotation speed of 3500 r / min for high-speed stirring for 20 minutes, then taken out and placed in a hydrothermal reactor, and the stirring rate is controlled to be 150 r / min. When the temperature rises to 120°C, the timing is started. After the reaction is completed for 7 hours, the mixture is taken out for centrifugation and washing, and then the obtained powder is placed in a muffle furnace at 600°C for calcination for 5 hours. Finally, the calcined powder is dispersed in a mixed solution of water and ethanol with a mass ratio of 7:3 to obtain a porous titanium dioxide microsphere dispersion;
[0071] (2) adding γ-methacryloxypropyltrimethoxysilane as a silane coupling agent to the titanium dioxide microsphere dispersion obtained in (1), grafting and modifying the porous titanium dioxide microspheres at 70° C. to obtain a titanium dioxide microsphere dispersion with double bonds, which is set aside for later use;
[0072] (3) dissolving a photoinitiator, diphenyl-(2,4,6-trimethylbenzoyl)phosphine oxide (1.3% by mass of the organic monomer) in an organic monomer, hydroxyethyl acrylate, to obtain a mixed solution, and then spraying the mixed solution on a polyester needle-punched felt, and rolling it with a rolling mill to obtain a needle-punched polyester filter felt for standby use;
[0073] (4) Spraying the titanium dioxide microsphere dispersion with double bonds obtained in step 2 onto the polyester needle-punched filter felt obtained in step (3), and rolling it with a rolling mill, and then irradiating the needle-punched felt with ultraviolet light with a central wavelength of 365 nm. After drying, an antibacterial polyester needle-punched filter felt with dye adsorption effect can be obtained.
[0074] The test showed that the particle size of the titanium dioxide microspheres obtained in (1) was 600 nm, and the removal rate of the polyester needle-punched felt obtained by UV curing for 10 mg / L Sudan red dye solution was as high as 90%. The antibacterial test showed that the antibacterial rate for Staphylococcus aureus reached 87%.
[0075] The above description is only a specific implementation mode of the present invention, but the protection scope of the present invention is not limited thereto. Any modifications, equivalent substitutions and improvements made by any technician familiar with the technical field within the technical scope disclosed by the present invention and within the spirit and principle of the present invention should be covered by the protection scope of the present invention.
Claims
1. A method for preparing an antibacterial needle-punched filter felt having dye adsorption efficacy, characterized in that: The method for preparing the antibacterial needle-punched filter felt having dye adsorption efficacy comprises: Step 1, using water and hexadecyltrimethylammonium bromide as phase A, and using ethanol, butyl titanate, cyclohexane and n-pentanol as phase B, mixing phase A and phase B evenly, placing in a high shear homogenizer and stirring at high speed for 20 minutes, then taking out and placing in a hydrothermal reactor, reacting for 7 hours, taking out and centrifuging and washing, then placing the obtained powder in a muffle furnace at 600° C. and calcining for 5 hours, and finally dispersing the calcined powder in a mixed solution of water and ethanol to obtain a porous titanium dioxide microsphere dispersion; Step 2: Add a silane coupling agent with double bonds to the titanium dioxide microsphere dispersion obtained in step 1, and graft-modify the porous titanium dioxide microspheres at 70° C. to obtain a titanium dioxide microsphere dispersion with double bonds, which is set aside; Step 3, dissolving the photoinitiator in the organic monomer to obtain a mixed solution, then spraying the mixed solution on the needle-punched felt, and pressing it with a rolling mill to obtain a needle-punched filter felt for standby use; Step 4, spraying the titanium dioxide microsphere dispersion with double bonds obtained in step 2 onto the needle-punched filter felt obtained in step 3, and rolling it with a rolling car, and then irradiating the needle-punched filter felt with ultraviolet light, and after drying, an antibacterial needle-punched filter felt with dye adsorption effect can be obtained; The organic monomer in step three is one of hydroxyethyl acrylate and hydroxypropyl acrylate.
2. The method for preparing the antibacterial needle-punched filter felt with dye adsorption efficacy according to claim 1, characterized in that: In step 1, the speed of the high shear homogenizer is 3500 r / min; after being placed in the hydrothermal reactor, the stirring rate is controlled to be 150 r / min, and the timing is started when the temperature rises to 120°C.
3. The method for preparing the antibacterial needle-punched filter felt with dye adsorption efficacy according to claim 1, characterized in that: The particle size of the titanium dioxide microspheres in step 1 is 300-600 nm.
4. The method for preparing the antibacterial needle-punched filter felt with dye adsorption efficacy according to claim 1, characterized in that: Step 1: The calcined powder is dispersed in a mixture of water and ethanol, wherein the mass ratio of water to ethanol is 7:
3.
5. The method for preparing the antibacterial needle-punched filter felt with dye adsorption efficacy according to claim 1, characterized in that: The silane coupling agent in step 2 is γ-methacryloxypropyltrimethoxysilane.
6. The method for preparing the antibacterial needle-punched filter felt with dye adsorption efficacy according to claim 1, characterized in that: The photoinitiator in step three is one of diphenyl-(2,4,6-trimethylbenzoyl)phosphine oxide and 2-hydroxy-2-methyl-1-phenylacetone.
7. The method for preparing the antibacterial needle-punched filter felt with dye adsorption efficacy according to claim 1, characterized in that: The mass proportion of the photoinitiator used in step 3 is 1%-1.5% of the organic monomer.
8. The method for preparing the antibacterial needle-punched filter felt with dye adsorption efficacy according to claim 1, characterized in that: The needle-punched felt in step three is one of polyester and polypropylene.