A method and system for detecting electrochemical properties of easily passivated bare metals

Through the detection system and method, the electrochemical properties of easily passivated metals are measured, which solves the problem of the passivation layer affecting the electrochemical properties, provides experimental support for the optimization of the electrochemical cleaning and grinding process, and improves the grinding performance of the grinding wheel.

CN115609095BActive Publication Date: 2024-10-29湖南工商大学
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202211159614.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-09-22
Publication Date
2024-10-29
Estimated Expiration
2042-09-22

AI Technical Summary

Technical Problem

During the electrochemical cleaning and grinding process, the passivation layer of easily passivated metal hinders the transmission of reactive substances, resulting in a reduction of the active reaction area on the electrode surface, affecting the electrochemical characteristics, and it is difficult for the existing technology to effectively detect the newly scratched surface. Electrochemical properties of easily passivated metals.

Method used

A system and method for detecting the electrochemical properties of bare metals that are easily passivated are adopted. The passivation layer on the surface of easily passivated metals is cut with a diamond pen, and the current density-time relationship curves under different operating voltages are measured using cutting fluid and electrolyte. Exclude the influence of passivation effect and measure the voltage-current density relationship when easily passivable metal is used as anode.

Benefits of technology

The electrochemical characteristics of easily passivated metals in the bare metal state were successfully measured and analyzed, providing experimental support for studying the cleaning rules of adhered metals during electrochemical cleaning and grinding, helping to optimize the electrochemical cleaning and grinding process and improve grinding wheel grinding. performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115609095B_ABST
    Figure CN115609095B_ABST
Patent Text Reader

Abstract

The present invention provides a method and system for detecting the electrochemical characteristics of bare metal of easily passivated metal, wherein the easily passivated metal wheel is connected to the positive electrode of a DC power supply through a grinder spindle, an anode brush, a wire, and a digital multimeter, and a copper cathode is connected to the negative electrode of a DC power supply through a wire. During the experiment, a diamond pen is used to cut the passivation film on the surface of the easily passivated metal wheel to obtain a film-free substrate to eliminate the influence of the passivation effect, and the idling electrolysis current and the working electrolysis current under different working voltages are measured. Based on the passivation mechanism and cutting geometry analysis, the current density-time relationship curve under different working voltages and the working voltage-current density relationship curve at any time are obtained when the bare metal of the easily passivated metal is used as an anode. The present invention can provide experimental support for the study of the cleaning mechanism of adhered metal during electrochemical cleaning and grinding.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of electrochemical cleaning and grinding of ductile metal parts, and in particular to a technology for detecting electrochemical properties of easily passivated bare metals. Background Art

[0002] Composite machining technology is an important means to achieve high-performance machining of parts made of difficult-to-machine materials by coupling advanced technologies in disciplines such as mechanics, electromagnetism, fluid, optics and acoustics. It is the future development direction of mechanical machining.

[0003] Electrochemical Cleaning Grinding (ECCG) is a grinding-electrochemical composite processing technology developed in recent years. It can be used to solve the problem of grinding wheel adhesion during grinding of ductile metals (including aluminum alloys, titanium alloys, titanium-aluminum alloys and high-temperature alloys). In the electrochemical cleaning grinding process, grinding is the main process to complete the removal of workpiece material; electrochemical cleaning is an auxiliary process to electrolytically remove the metal adhering to the surface of the grinding wheel to restore the grinding performance of the grinding wheel. The key to electrochemical grinding technology is to match the formation rate and electrolysis rate of the metal adhering to the surface of the grinding wheel. When the formation rate is greater than the electrolysis rate, the cleaning effect is not significant and the grinding performance of the grinding wheel cannot be fully restored; when the formation rate is less than the electrolysis rate, the over-electrolysis effect is significant, which will cause grinding wheel damage and energy waste.

[0004] For easily passivated metals (such as aluminum alloy, titanium alloy and titanium aluminum alloy), when used as electrode materials, the passivation layer will hinder the transmission of reactants, reduce the active reaction area on the electrode surface, and easily cause changes in the electrochemical properties of the electrode material itself.

[0005] In the process of electrochemical cleaning and grinding of easily passivated metals, the grinding wheel rotates at high speed, and the time for the newly formed adhered metal to reach the relative position of the cathode is extremely short (about 0.01s), which is less than the net passivation time of the easily passivated metal. Therefore, at the moment when the adhesion area reaches the corresponding position of the cathode, the adhered metal should be regarded as a film-free substrate surface that has just been scratched from the workpiece surface and has not been affected by oxidation or environmental corrosion. In order to study the electrochemical characteristics of the adhered metal in the ECCG system, the influence of the passivation effect must be excluded. Therefore, the analysis of the bare metal electrochemical characteristics of easily passivated metals (especially the determination of the voltage-current density relationship curve) is an important part of the research on electrochemical cleaning and grinding technology. Summary of the invention

[0006] In order to solve the above technical problems, the present invention proposes a method and system for detecting the electrochemical properties of bare metal of easily passivated metal, so as to quantitatively detect the voltage-current density relationship curve of a bare metal of easily passivated metal that has just been scratched and not affected by oxidation or environmental medium corrosion (i.e., bare metal of easily passivated metal) when used as an anode.

[0007] The purpose of the present invention is achieved through the following technical solutions:

[0008] The present invention provides a bare metal electrochemical property detection system for easily passivated metals, comprising:

[0009] Grinding machine spindle, anode brush, digital multimeter, wires, DC power supply, copper cathode, diamond pen, cutting fluid nozzle, wheel and electrolyte nozzle;

[0010] The wheel comprises: an easily passivated metal wheel and an insulating resin layer covering the outside of the easily passivated metal wheel;

[0011] The wheel can be rotated at a set speed along with the main shaft of the grinder; the diamond pen is placed on the working platform of the grinder, and can drive the wheel to cut at a set feed speed and cutting depth through the working platform of the grinder and scrape off the passivation layer on the end face of the easily passivated metal wheel; the cutting fluid nozzle can continuously spray cutting fluid to the cutting area between the wheel and the diamond pen;

[0012] The wheel serves as an anode and is connected to the positive electrode of a DC power supply through a grinder spindle, an anode brush, a digital multimeter and a wire; the copper cathode serves as a cathode and is connected to the negative electrode of the DC power supply through a wire; and the electrolyte nozzle can spray electrolyte into the electrode gap between the wheel and the copper cathode.

[0013] The present invention also provides a method for detecting the electrochemical properties of easily passivated bare metals, which comprises:

[0014] Step S01: Use the grinding machine spindle to drive the wheel at a speed n s Rotate; use the cutting fluid nozzle to spray cutting fluid to the cutting area; use the electrolyte nozzle to spray electrolyte to the electrode gap formed by the copper cathode and the easily passivated metal wheel;

[0015] Step S02: Turn on the digital multimeter; turn on the DC power supply;

[0016] Step S03: Setting the working voltage E app And turn on the circuit, use a digital multimeter to measure the idling electrolysis current I b , using formula (1) to solve the average current density i on the surface of the easily passivated metal wheel under idling conditions b ;

[0017]

[0018] In the formula, I b is the idling electrolysis current; S 0 is the effective working area of ​​the copper cathode;

[0019] Step S04: Start the CNC grinding machine table and make the diamond pen move at a feed speed v d , cutting depth is dc Cutting wheel, and use a digital multimeter to measure the working electrolysis current I w , the working voltage is E app The working electrolysis current-time relationship curve is denoted as I w -t curve; Based on the passivation mechanism of easily passivated metals and the cutting geometry, the working voltage is obtained as E app When the unknown electrolysis coefficient k is included a and k b Working electrolysis current I w Relationship function I with time t w =F(k a ,k b ,t);

[0020] Step S05: According to function I w =F(k a ,k b ,t) Based on the I obtained in step S04 w -t curve is fitted to obtain the electrolysis coefficient k a and k b ;

[0021] Step S06: The average current density i on the surface of the easily passivated metal wheel under idling condition obtained in step S03 is b and the electrolysis coefficient k obtained in step S05 a and k b , substituting into formula (3), the working voltage is obtained as E app The current density-time relationship of bare metal that is easy to passivate;

[0022] i=k a exp(-k b t)+i b Formula (3)

[0023] Where i is the current density when the easily passivated metal is used as the anode; k a and k b is the electrolysis coefficient related to material properties, working voltage, electrode gap and electrolyte properties; t is time; i b is the average current density on the surface of the easily passivated metal wheel under idling conditions;

[0024] Step S07: Setting different working voltages E app , and repeating steps S03 to S06 to obtain the current density-time relationship of the easily passivated metal bare metal corresponding to different working voltages;

[0025] Step S08: Let t=t 0 , according to different working voltage E appThe corresponding current density-time relationship of the easily passivated metal bare metal is obtained at any time t 0 The corresponding working voltage-current density curve of the easily passivated bare metal.

[0026] More preferably, in step S04, based on the passivation mechanism of the easily passivated metal and the cutting geometry, the working voltage is E app When the unknown electrolysis coefficient k is included a and k b Working electrolysis current I w Relationship function I with time t w =F(k a ,k b ,t) process, including:

[0027] When t=[2π(J-1)+π+θ c ] / ω, the current I of the latest cutting circle 1 :

[0028]

[0029] When t=[2π(J-1)+π+θ c ] / ω, the current I of the remaining cutting circles j :

[0030]

[0031] When t=[2π(J-1)+π+θ c ] / ω, the working electrolysis current I w It can be expressed as:

[0032]

[0033] Combining equations (4) and (8), and substituting J = (ωt + π - θ c ) / (2π) is substituted into formula (9), and the working electrolysis current I can be obtained. w Relationship function I with time t w =F(k a ,k b ,t):

[0034] I w =F(k a ,k b ,t) Formula (10)

[0035] In the above formula, θ c k is the half top angle of the copper cathode working surface; a and k b is the electrolysis coefficient related to material properties, working voltage, electrode gap and electrolyte properties; ib is the average current density on the surface of the easily passivated metal wheel under idling conditions; R in and R out are the inner and outer diameters of the easily passivated metal wheel; f r is the feed rate of the diamond pen; l c is the projected length of the contact surface between the diamond pen and the easily passivated metal wheel in the cutting direction; J is the number of cutting circles completely covered by the copper cathode working surface, and the maximum value is (R out -R in ) / f r ;ω is the angular velocity of the grinding machine spindle; I j represents the current of the jth cutting circle completely covered by the copper cathode working surface;

[0036] More preferably, the electrolyte is tap water.

[0037] More preferably, the cutting fluid is tap water.

[0038] It can be seen from the above technical solutions of the present invention that the present invention has the following technical effects:

[0039] The present invention uses a diamond pen to cut the passivation layer on the surface of an easily passivated metal to obtain a film-free substrate, so as to eliminate the influence of the passivation effect, and measures the idling electrolysis current and the working electrolysis current under different working voltages; based on the passivation mechanism and cutting geometry analysis, the current density-time relationship curves under different working voltages and the working voltage-current density relationship curves at any time when the easily passivated metal film-free substrate (that is, the easily passivated metal bare metal) that has just been scratched and not affected by oxidation or environmental medium corrosion is used as an anode are obtained, which can provide experimental support for studying the cleaning law of adhered metal during electrochemical cleaning and grinding. BRIEF DESCRIPTION OF THE DRAWINGS

[0040] Figure 1 This is a working principle diagram of a bare metal electrochemical property detection system for easily passivated metals in the present invention;

[0041] Figure 2 This is a flow chart of a method for detecting the electrochemical properties of bare metals that are easily passivated in the present invention;

[0042] Figure 3 It is a schematic diagram of the working principle of the diamond pen cutting the easily passivated metal wheel in the present invention;

[0043] Figure 4 The current density-time relationship curve of the easily passivated metal bare metal corresponding to different working voltages in the present invention;

[0044] Figure 5 is any time t in the present invention 0Corresponding working voltage-current density curve of easily passivated bare metal.

[0045] Description of reference numerals:

[0046] Grinding machine spindle 1, anode brush 2, digital multimeter 3, wire 4, DC power supply 5, copper cathode 6, diamond pen 7, cutting fluid nozzle 8, wheel 9, electrolyte nozzle 10;

[0047] The metal wheel 92 and the insulating resin layer 91 are easily passivated. DETAILED DESCRIPTION

[0048] The present invention is described in detail below with reference to the accompanying drawings and embodiments.

[0049] Embodiment 1:

[0050] The present invention proposes a system for detecting the electrochemical properties of easily passivated metal bare metal. The working principle of the detection system is as follows: Figure 1 As shown, it includes a grinding machine spindle 1, an anode brush 2, a digital multimeter 3, a wire 4, a DC power supply 5, a copper cathode 6, a diamond pen 7, a cutting fluid nozzle 8, a wheel 9 and an electrolyte nozzle 10.

[0051] The wheel 9 includes: an easily passivated metal wheel 92 and an insulating resin layer 91 covering the outside of the easily passivated metal wheel 92. The insulating resin layer 91 is used to isolate the electrolyte from contacting the circumference of the easily passivated metal wheel 92, thereby preventing the circumference of the easily passivated metal wheel 92 from participating in electrolysis.

[0052] n s is the speed of the grinding machine spindle 1 or wheel 9, v d is the feeding speed of the diamond pen 7.

[0053] The connection relationship or position relationship between the above components is as follows:

[0054] The wheel 9 can run at a set speed along with the grinder spindle 1; the diamond pen 7 is placed on the grinder work platform, and can be driven by the grinder work platform to cut the wheel 9 at a set feed speed and cutting depth and scrape off the passivation layer on the end face of the easily passivated metal wheel 92; the cutting fluid nozzle 8 can continuously spray cutting fluid into the cutting area between the wheel 9 and the diamond pen 7; the cutting fluid can be tap water.

[0055] The wheel 9 is used as an anode and is connected to the positive electrode of the DC power supply 5 through the grinder spindle 1, the anode brush 2, the digital multimeter 3 and the wire 4; the copper cathode 6 is used as a cathode and is connected to the negative electrode of the DC power supply 5 through the wire 4; the electrolyte nozzle 10 can spray the electrolyte into the gap between the positive and negative electrodes between the wheel 9 and the copper cathode 6. The electrolyte can be tap water. The digital multimeter 3 is used to measure the idling electrolysis current I b and working electrolysis current Iw .

[0056] The working principle of the bare metal electrochemical property detection system for easily passivated metals is as follows:

[0057] The wheel 9 rotates driven by the grinder spindle 1. The DC power supply 5 remains on to provide electrical energy. The digital multimeter 3 remains on to measure the circuit current. The wheel 9 is connected to the positive pole of the DC power supply 5 through the grinder spindle 1, the anode brush 2, the digital multimeter 3, and the wire 4 as an anode; the copper cathode 6 is connected to the negative pole of the DC power supply 5 through the wire 4 as a cathode. At the same time, the electrolyte is supplied to the electrode gap formed by the wheel 9 and the copper cathode 5 through the electrolyte nozzle 10; and the cutting fluid is supplied to the cutting area through the cutting fluid nozzle 8. At the same time, the digital multimeter 3 is used to record the idling electrolysis current I b and working electrolysis current I w .

[0058] Embodiment 2:

[0059] The present invention also provides a method for detecting the electrochemical properties of easily passivated metal bare metal, which is implemented based on the above detection system. Before implementing the detection method, according to Figure 1 The detection system is built as shown.

[0060] The implementation process of this detection method is as follows Figure 2 As shown, the following steps are included:

[0061] Step S01: Turn on the CNC grinding machine, and the grinding machine spindle 1 drives the wheel 9 at a speed n s Rotate; open the cutting fluid nozzle 8 to spray the cutting fluid into the cutting area; open the electrolyte nozzle 10 to spray the electrolyte into the electrode gap formed by the copper cathode 6 and the wheel 9;

[0062] Step S02: Turn on the digital multimeter 3; turn on the DC power supply 5;

[0063] Step S03: Setting the working voltage E app And turn on the circuit, use the digital multimeter 3 to measure the idling electrolysis current I b , using equation (1) to solve the average current density i on the surface of the easily passivated metal wheel 92 under idling conditions b ;

[0064]

[0065] In the formula, I b is the idling electrolysis current; S 0 is the effective working area of ​​the copper cathode, which can be expressed as:

[0066] S 0 =θ c (Rout 2 -R in 2 ) Formula (2)

[0067] In the formula, θ c R is the half top angle of the copper cathode working surface; in and R out are the inner diameter and outer diameter of the easily passivated metal wheel 92 respectively.

[0068] Step S04: Start the CNC grinding machine table and make the diamond pen 7 move at a feed speed v d , cutting depth is d c Cutting wheel 9, while using a digital multimeter (3) to measure the working electrolysis current I w , the working voltage is E app Working electrolysis current-time relationship curve (I w -t curve); Based on the passivation mechanism of easily passivated metals and the cutting geometry, the working voltage is obtained as E app When the unknown electrolysis coefficient k is included a and k b Working electrolysis current I w Relationship function I with time t w =F(k a ,k b ,t);

[0069] Figure 3 A working principle diagram of the diamond pen 7 cutting wheel 9 is given, in which: d c is the cutting depth; l c f is the projected length of the contact surface between the diamond pen 7 and the easily passivated metal wheel 92 in the cutting direction; r is the feed rate of the diamond pen 7; θ p R is the half apex angle of the diamond pen 7; in and R out are the inner diameter and outer diameter of the easily passivated metal wheel 92 respectively.

[0070] Due to the existence of the passivation effect, for a specific working voltage, the current density i and time t when the easily passivated metal is used as the anode exist in the following relationship:

[0071] i=k a exp(-k b t)+i b Formula (3)

[0072] In the formula, k a and k b is the electrolysis coefficient related to material properties, working voltage, electrode gap and electrolyte properties; i bis the average current density on the surface of the easily passivated metal wheel 92 under idling conditions (calculated using formula (1));

[0073] When t=[2π(J-1)+π+θ c ] / ω, the current I of the latest cutting circle (i.e., the cutting circle that has been cut by the diamond pen and completely covered by the copper cathode working surface) 1 :

[0074]

[0075] In formula (4), θ c k is the half top angle of the copper cathode working surface; a and k b is the electrolysis coefficient related to material properties, working voltage, electrode gap and electrolyte properties; i b is the average current density on the surface of the easily passivated metal wheel 92 under idling conditions (calculated using formula (1)); R in and R out are the inner diameter and outer diameter of the easily passivated metal wheel 92 respectively;

[0076] f in formula (4) r is the feed rate of the diamond pen 7, which is calculated using formula (5):

[0077]

[0078] In formula (5), v d is the feeding speed of the diamond pen 7; n s is the speed of the grinding machine spindle 1;

[0079] In formula (4), c is the projected length of the contact surface between the diamond pen 7 and the easily passivated metal wheel 92 in the cutting direction, which is calculated using formula (6):

[0080]

[0081] In formula (6), d c is the cutting depth; θ p f is the half apex angle of the diamond pen 7; r is the feed rate of the diamond pen 7, calculated using formula (5);

[0082] J in formula (4) is the number of cutting circles completely covered by the copper cathode working surface, and its maximum value is (R out -R in ) / f r (where f r R is the feed rate of the diamond pen 7; in and R outare the inner diameter and outer diameter of the easily passivated metal wheel 92 respectively);

[0083] The ω in formula (4) is the rotational angular velocity of the grinding machine spindle 1, which can be expressed as:

[0084] ω=πn s / 30 Formula (7)

[0085] In formula (7), n s is the rotation speed of the grinding machine spindle 1 or wheel 9.

[0086] When t=[2π(J-1)+π+θ c ] / ω, the current of the remaining cutting circles is expressed by formula (8):

[0087]

[0088] In formula (8), I j represents the current of the jth cutting circle completely covered by the copper cathode working surface; the meanings of the other parameters are the same as those of the corresponding parameters in formula (4) and are not described in detail here.

[0089] When t=[2π(J-1)+π+θ c ] / ω, the working electrolysis current I w It can be expressed as:

[0090]

[0091] The meanings of the parameters in formula (9) are the same as those of the corresponding parameters in formula (4), and will not be described in detail here.

[0092] Combining equations (4) and (8), and substituting J = (ωt + π - θ c ) / (2π) is substituted into formula (9), and the working voltage is equal to E app Working electrolysis current I w Function I with respect to time t w =F(k a ,k b ,t):

[0093] I w =F(k a ,k b ,t) Formula (10)

[0094] In formula (10), k a and k b is the unknown electrolysis coefficient related to material properties, working voltage, electrode gap and electrolyte properties; t is time; I w is the working electrolysis current.

[0095] Step S05: According to the function I shown in formula (10) w =F(k a ,k b ,t) Based on the I obtained in step S04 w -t curve is fitted to obtain the electrolysis coefficient k a and k b ;

[0096] Step S06: The average current density i on the surface of the easily passivated metal wheel 92 under the idling condition obtained in step S03 is b and the electrolysis coefficient k obtained in step S05 a and k b , substituting into formula (3), the working voltage is obtained as E app The current density-time relationship of bare metal that is easy to passivate;

[0097] Step S07: Setting different working voltages E app , and repeat steps S03 to S06 to obtain the current density-time relationship of the easily passivated metal bare metal corresponding to different working voltages, which can be used as follows Figure 4 The it curve shown represents;

[0098] Step S08: Let t=t 0 , according to different working voltage E app The corresponding bare metal current density-time curve of the easily passivated metal (represented by the it curve) can be obtained at any time t 0 The corresponding working voltage-current density curve of the easily passivated metal bare metal (ie: Figure 5 E shown app -i curve).

[0099] Although the present invention has been disclosed as above with preferred embodiments, the embodiments are not intended to limit the present invention. Any equivalent changes or modifications made without departing from the spirit and scope of the present invention also belong to the protection scope of the present invention. Therefore, the protection scope of the present invention should be based on the content defined by the claims of this application.

Claims

1. A method for detecting the electrochemical properties of easily passivated bare metals, characterized in that: The detection method comprises: Step S01: Use the grinding machine spindle (1) to drive the wheel (9) at a speed n s Rotate; use a cutting fluid nozzle (8) to spray cutting fluid to the cutting area; use an electrolyte nozzle (10) to spray electrolyte to the electrode gap formed by the copper cathode (6) and the easily passivated metal wheel (92); Step S02: Turn on the digital multimeter (3); turn on the DC power supply (5); Step S03: Setting the working voltage E app Then connect the circuit and use a digital multimeter (3) to measure the idling electrolysis current I b , using equation (1) to solve the average current density i on the surface of the easily passivated metal wheel (92) under idling conditions b ; In the formula, I b is the idling electrolysis current; S0 is the effective working area of ​​the copper cathode; Step S04: Start the CNC grinding machine table to make the diamond pen (7) move at a feed speed v d , cutting depth is d c The cutting wheel (9) is used to measure the working electrolysis current I using a digital multimeter (3) w , the working voltage is E app The working electrolysis current-time relationship curve is denoted as I w -t curve; Based on the passivation mechanism of easily passivated metals and the cutting geometry, the working voltage is obtained as E app When the unknown electrolysis coefficient k is included a and k b Working electrolysis current I w Relationship function I with time t w =F(k a ,k b ,t); Step S05: According to function I w =F(k a ,k b ,t) Based on the I obtained in step S04 w -t curve is fitted to obtain the electrolysis coefficient k a and k b ; Step S06: The average current density i on the surface of the easily passivated metal wheel (92) under the idling condition obtained in step S03 is b and the electrolysis coefficient k obtained in step S05 a and k b , substituting into formula (3), the working voltage is obtained as E app The current density-time relationship of bare metal that is easy to passivate; i = k a exp(-k b t) + i b Equation (3) Where i is the current density when the easily passivated metal is used as the anode; k a and k b is the electrolysis coefficient related to material properties, working voltage, electrode gap and electrolyte properties; t is time; i b is the average current density on the surface of the easily passivated metal wheel (92) under idling conditions; Step S07: Setting different working voltages E app , and repeat steps S03 to S06 to obtain different working voltages E app The corresponding current density-time relationship of the easily passivated bare metal; Step S08: Let t = t0, according to different working voltages E app The corresponding current density-time relationship of the easily passivated metal bare metal is obtained, and the working voltage-current density curve of the easily passivated metal bare metal corresponding to any time t0 is obtained.

2. According to the method for detecting electrochemical properties of easily passivated metal bare metal according to claim 1, in step S04, based on the passivation mechanism of easily passivated metal and the cutting geometry relationship, the working voltage E is obtained. app When the unknown electrolysis coefficient k is included a and k b Working electrolysis current I w Relationship function I with time t w =F(k a ,k b ,t) process, including: When t=[2π(J-1)+π+θ c ] / ω, the current I1 of the latest cutting circle: When t=[2π(J-1)+π+θ c ] / ω, the current I of the remaining cutting circles j : When t=[2π(J-1)+π+θ c ] / ω, the working electrolysis current I w It can be expressed as: Combining equations (4) and (8), and substituting J = (ωt + π - θ c ) / (2π) is substituted into formula (9), and the working electrolysis current I can be obtained. w Relationship function I with time t w =F(k a ,k b ,t): I w =F(k a ,k b ,t) Formula (10) In the above formula, θ c k is the half top angle of the copper cathode working surface; a and k b is the electrolysis coefficient related to material properties, working voltage, electrode gap and electrolyte properties; i b is the average current density on the surface of the easily passivated metal wheel (92) under idling conditions; R in and R out are respectively the inner diameter and outer diameter of the easily passivated metal wheel (92); r is the feed rate of the diamond pen (7); l c is the projected length of the contact surface between the diamond pen (7) and the easily passivated metal wheel (92) in the cutting direction; J is the number of cutting circles completely covered by the copper cathode working surface, and the maximum value is (R out -R in ) / f r ; ω is the rotational angular velocity of the grinding machine spindle (1); I j Represents the current of the jth cutting circle which is completely covered by the copper cathode working surface.

3. The method for detecting the electrochemical properties of bare metals that are easily passivated according to claim 1, characterized in that: The electrolyte is tap water.

4. The method for detecting electrochemical properties of bare metals that are easily passivated according to claim 1, characterized in that: The cutting fluid is tap water.

Citation Information

Patent Citations

  • Grinding wheel adhesion rate detection method and system based on electrochemical principle

    CN114965612A