A thermal transfer sheet capable of transferring high-resolution patterns and resistant to friction and a preparation method thereof

By using a specific ratio of release layer, ink layer and adhesive layer in the thermal transfer ribbon, the problem in the existing technology that the pattern is easily damaged on the surface of the smooth substrate is solved, and the friction resistance of the high-resolution pattern is achieved. and clarity, enhanced adhesion and wear resistance.

CN115610132BActive Publication Date: 2024-10-25HUNAN DINGYIYUAN TECH DEV CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211280386.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-10-19
Publication Date
2024-10-25
Estimated Expiration
2042-10-19

AI Technical Summary

Technical Problem

Existing thermal transfer ribbons transfer patterns easily to damage or disappear on the surface of smooth substrates. This is mainly due to poor material adhesion of the release coating and poor ink coating performance, resulting in pattern damage during friction.

Method used

Using a release layer, ink layer and adhesive layer composed of solvent, polystyrene resin, adhesive resin and thermoplastic elastomer materials, the scratch resistance and clarity of the pattern are improved through a specific layer structure and material ratio. , enhance adhesion to smooth substrates.

Benefits of technology

It significantly improves the scratch resistance and abrasion resistance of thermal transfer ribbon patterns on smooth substrate surfaces, reduces pattern blockage and trailing defects, and ensures the integrity and clarity of high-resolution patterns.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115610132B_ABST
    Figure CN115610132B_ABST
Patent Text Reader

Abstract

The present invention relates to a thermal transfer sheet capable of transferring high-resolution patterns and being resistant to friction and a preparation method, belonging to the field of thermal printing technology. The thermal transfer sheet capable of transferring high-resolution patterns and being resistant to friction comprises a back coating layer, a substrate, a release layer, an ink layer and an adhesive layer which are sequentially laminated from top to bottom; the release layer is formed by mixing the following raw materials in parts by weight and then coating: a solvent part, 30-90 parts of a polystyrene resin, 20-30 parts of an adhesive resin and 1.5-15 parts of a thermoplastic elastomer material. The present invention also discloses a preparation method for the thermal transfer sheet capable of transferring high-resolution patterns and being resistant to friction. Beneficial effect: The scratch resistance and alcohol resistance of the pattern transferred by the carbon ribbon on the surface of a smooth substrate can be greatly reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of thermal printing, and in particular relates to a thermal transfer sheet capable of transferring high-resolution patterns and being resistant to friction, and a preparation method thereof. Background Art

[0002] Thermal transfer printing refers to a printing method in which a carbon ribbon with a transferable ink layer is heated by a print head through a thermal transfer printer, and the ink layer is transferred to a substrate. The image formed by hot melt transfer is suitable for printing images such as text and barcodes because of its high concentration and high definition. At present, the resin-based carbon ribbons on the market are transferred to smooth substrates such as PET and PP material label surfaces. Due to the frequent friction required for packaging, mechanical processing, etc., the pattern of the label is damaged or disappears after a period of use. The main problem is that the release coating has poor performance in isolating the base film and the ink coating. The existing release coating is mostly prepared by a single or several polyester resins to obtain a coating liquid coated on the back of the base film. The material used has poor adhesion to the transferred substrate, resulting in problems such as damage to the transfer pattern on the label.

[0003] Therefore, a thermal transfer sheet capable of transferring high-resolution patterns and being friction-resistant and a preparation method thereof are proposed to solve the deficiencies in the prior art. Summary of the invention

[0004] In order to solve the above technical problems, the present invention provides a thermal transfer sheet capable of transferring high-resolution patterns and being resistant to friction, which can significantly reduce the scratch resistance and alcohol resistance of the pattern transferred by the carbon ribbon on the surface of a smooth substrate.

[0005] The technical solution of the present invention to solve the above technical problems is as follows: a thermal transfer sheet capable of transferring high-resolution patterns and resistant to friction comprises a back coating layer, a substrate, a release layer, an ink layer and an adhesive layer which are sequentially laminated from top to bottom;

[0006] The release layer is formed by mixing the following raw materials in parts by weight and then coating: 70-90 parts of solvent, 30-90 parts of polystyrene resin, 20-30 parts of adhesive resin and 1.5-15 parts of thermoplastic elastomer material;

[0007] The ink layer is formed by mixing the following raw materials in parts by weight and then coating: 70-80 parts of solvent, 10-20 parts of polyester resin, 10-15 parts of coloring pigment and 0-5 parts of dispersant;

[0008] The adhesive layer is formed by coating after mixing the following raw materials in parts by weight: 40-60 parts of solvent, 10-20 parts of polyester resin, and 20-40 parts of adhesive resin.

[0009] Beneficial effect: The carbon ribbon can significantly reduce the scratch resistance and alcohol resistance of the pattern transferred by the carbon ribbon on the surface of a smooth substrate.

[0010] Principle description: The release layer is between the substrate and the ink before printing, and is located on the side of the ink layer away from the transferred substrate after printing. It mainly helps the ink layer to separate from the substrate. The polystyrene resin can improve the clarity of the image of the thermal transfer sheet of the present invention for the smooth surface of the transferred body. From the perspective of image transfer integrity and clarity, the selection and dosage of polystyrene resin are critical, especially the molecular weight and glass transition temperature (TG value) have a greater impact on it; the average molecular weight of the polystyrene resin selected in this application is 600-3000, preferably 1000-1800. Too low or too high molecular weight may cause uneven distribution of the coating liquid on the surface of the substrate. Selecting this molecular weight range can take into account the transfer effect while reducing the transfer problem caused by too high molecular weight. The TG (melting point) value of the styrene resin selected in this application is 35℃-100℃, preferably 65℃-85℃. The higher TG value can ensure that the tailing problem is not generated after the resin melts when the print head is heated. It can further improve the clarity of the image on the uneven transfer object and reduce transfer defects such as block drop and tailing. The thermoplastic elastomer material in the release layer can improve the flexibility of the thermal transfer carbon ribbon and improve the scratch resistance of the transfer pattern.

[0011] Based on the above technical solution, the present invention can also be improved as follows.

[0012] Furthermore, the matrix is ​​any one of polypropylene, polyethylene naphthalate, polyethylene terephthalate, polyethylene, polyvinyl alcohol, and polymethyl methacrylate.

[0013] Beneficial effect: Using the above film as a substrate can better ensure that the back coating layer, release layer, ink layer and adhesive layer can be effectively coated on the surface of the substrate.

[0014] Furthermore, the adhesive resin is one of ethylene-vinyl acetate resin and vinyl chloride-vinyl acetate resin or a mixture of both.

[0015] Beneficial effects: It can improve the closing effect between the release layer and the ink layer; at the same time, the adhesive resin improves the film-forming performance and flowability of the acrylic resin, which can further improve the clarity of the image on the uneven transfer body and reduce transfer defects such as falling blocks and tailing.

[0016] Furthermore, the thermoplastic elastomer material is a styrene-butadiene block copolymer.

[0017] Beneficial effects: It can improve the flexibility of the thermal transfer ribbon and improve the scratch resistance of the transferred pattern.

[0018] Furthermore, the solvent is one or a mixture of 2-butanone and toluene.

[0019] Beneficial effect: Using 2-butanone and / or toluene as a solvent can ensure that the components in the back coating layer, the release layer, the ink layer and the adhesive layer are fully dispersed and mixed.

[0020] Furthermore, the thickness of the substrate is 2-15 μm, the thickness of the back coating is 0.2-1.0 μm, the thickness of the release layer is 0.1-0.4 μm, the thickness of the ink layer is 0.3-0.5 μm, and the thickness of the adhesive layer is 0.1-0.3 μm.

[0021] Beneficial effect: The thickness of the thermal transfer ribbon can be guaranteed within this thickness range, and at the same time, the adhesion and wear resistance to the substrate are good.

[0022] Furthermore, the back coating layer is any one of polyurethane-modified silicone resin, acrylic-modified silicone resin, polyvinyl acetal resin, and polyvinyl butyral resin, or a combination of two or more thereof.

[0023] Beneficial effects: heat transfer and anti-friction, protection of print head and printing substrate.

[0024] Furthermore, the coloring pigment is carbon black.

[0025] Beneficial effects: Good coloring effect.

[0026] To achieve the second objective of the present invention, a method for preparing a thermal transfer sheet capable of transferring high-resolution patterns and being friction-resistant is provided, comprising the following steps:

[0027] S1: Prepare solution:

[0028] Back coating liquid: 40-100 parts of the back coating material are added to 40-60 parts of the solvent to dissolve to prepare the back coating liquid for standby use;

[0029] Release liquid: add 30-90 parts of polystyrene resin and 20-30 parts of adhesive resin into 70-90 parts of solvent to dissolve, then add 1.5-15 parts of thermoplastic elastomer material and stir and mix to make release liquid for standby use;

[0030] Ink liquid: add 10-20 parts of polyester resin to 70-80 parts of solvent to dissolve, then add 10-15 parts of coloring pigment and 0-5 parts of dispersant, stir and mix, to prepare ink liquid for standby use;

[0031] Adhesive liquid: add 10-20 parts of polyester resin and 20-40 parts of adhesive resin into 40-60 parts of solvent to dissolve and prepare adhesive liquid for use;

[0032] S2: stunning;

[0033] Providing a substrate, and applying corona on both sides of the substrate;

[0034] S3: coating;

[0035] The back coating liquid prepared in step S1 is coated on the side of the substrate subjected to corona treatment in step S2, and then dried to form a back coating layer for standby use;

[0036] Then, the release liquid prepared in step S1 is coated on the side of the substrate away from the back coating layer in step S2, and then dried to form a release layer;

[0037] Then, the ink prepared in step S1 is coated on the side of the release layer in step S3 away from the substrate, and then dried to form an ink layer;

[0038] Finally, the adhesive solution prepared in step S1 is coated on the side of the ink layer in step S3 away from the release layer, so as to obtain a thermal transfer sheet capable of transferring high-resolution patterns and being friction-resistant.

[0039] Further, in step S3, a ceramic anilox roller with 200 to 250 lines is used to coat the back coating liquid, the coating speed is 60-100 m / min, the drying temperature is 50-100°C, and the drying time is 40-60s; a ceramic anilox roller with 200 to 250 lines is used to coat the release liquid, the coating speed is 60-100 m / min, the drying temperature is 50-100°C, and the drying time is 40-60s; a ceramic anilox roller with 200 to 250 lines is used to coat the ink liquid, the coating speed is 60-100 m / min, the drying temperature is 40-100°C, and the drying time is 40-60s; a ceramic anilox roller with 200 to 250 lines is used to coat the adhesive liquid, the coating speed is 60-100 m / min, the drying temperature is 80-100°C, and the drying time is 60-120s.

[0040] Beneficial effects: The thermal transfer sheet prepared by the above preparation method can greatly reduce the scratch resistance and alcohol resistance of the pattern transferred by the carbon ribbon on the surface of the smooth substrate, is adaptable to different substrates, has low production cost, and is simple and feasible in process. BRIEF DESCRIPTION OF THE DRAWINGS

[0041] Figure 1 Schematic diagram of the layer structure of the carbon ribbon of the present invention;

[0042] Figure 2 A sample diagram for the printing test of the present invention; DETAILED DESCRIPTION

[0043] The principles and features of the present invention are described below in conjunction with the accompanying drawings. The examples given are only used to explain the present invention and are not used to limit the scope of the present invention.

[0044] Embodiment 1:

[0045] The present embodiment provides a thermal transfer sheet capable of transferring high-resolution patterns and being resistant to friction, comprising a back coating layer, a substrate, a release layer, an ink layer and an adhesive layer which are sequentially laminated from top to bottom.

[0046] Wherein, the substrate is polyethylene terephthalate with a thickness of 4.3 μm;

[0047] The back coating layer is coated with the following raw materials in parts by weight: 30 parts of 2-butanone, 30 parts of toluene, 10 parts of polyurethane modified silicone resin, 10 parts of acrylic modified silicone resin, 30 parts of polyvinyl acetal resin, and 30 parts of polyvinyl butyral resin, with a coating thickness of 0.2-1.0 μm;

[0048] The release layer is coated with the following raw materials in parts by weight: 90 parts of toluene, 4 parts of polystyrene resin (Tg is 65° C.), 5.75 parts of ethylene-vinyl acetate resin and 0.25 parts of styrene-butadiene rubber, with a coating thickness of 1 μm;

[0049] The ink layer is coated with the following raw materials in parts by weight: 40 parts of 2-butanone, 40 parts of toluene, 10 parts of polyester resin, 9 parts of carbon black and 1 part of dispersant;

[0050] The adhesive layer is formed by coating the following raw materials in parts by weight: 30 parts of 2-butanone, 30 parts of toluene, 10 parts of polyester resin, and 30 parts of adhesive resin.

[0051] Preparation of thermal transfer sheets capable of transferring high-resolution patterns and resistant to friction:

[0052] Apply corona to both sides of the polyethylene terephthalate;

[0053] According to the weight proportions of each component of the back coating layer, materials are taken and mixed to form a back coating liquid;

[0054] Use a 230-line ceramic anilox roller to apply the back coating liquid on the corona-charged side of the PET substrate, and dry it at 100°C for 60 seconds for later use;

[0055] According to the weight proportions of each component of the release layer, materials are taken and mixed to form a receiving liquid;

[0056] Use a 230-line ceramic anilox roller to coat the receiving liquid on the side of the substrate away from the back coating, and dry it at 100° C. for 60 seconds for standby use;

[0057] According to the weight proportions of each component of the ink layer, materials are taken and mixed to form ink liquid;

[0058] Use a 230-line ceramic anilox roller to apply the ink on the side of the release layer away from the substrate, and dry it at 60° C. for 60 seconds for later use;

[0059] According to the weight proportions of each component of the bonding layer, materials are taken and mixed to form a bonding liquid;

[0060] The adhesive liquid was coated on the side of the ink layer away from the release layer using a 230-line ceramic anilox roller, and dried at 60° C. for 60 seconds to obtain a thermal transfer sheet that can transfer high-resolution patterns and is resistant to friction.

[0061] Embodiment 2:

[0062] The difference between this embodiment and embodiment 1 is that:

[0063] The release layer is coated with the following raw materials in parts by weight: 90 parts of toluene, 5 parts of polystyrene resin (Tg is 85° C.), 4.75 parts of ethylene-vinyl acetate resin and 0.25 parts of styrene-butadiene rubber, and the coating thickness is 1 μm.

[0064] Embodiment 3:

[0065] The difference between this embodiment and embodiment 1 is that:

[0066] The release layer is coated with the following raw materials in parts by weight: 90 parts of toluene, 6 parts of polystyrene resin (Tg is 100° C.), 3.75 parts of ethylene-vinyl acetate resin and 0.25 parts of styrene-butadiene rubber, and the coating thickness is 1 μm.

[0067] Embodiment 4:

[0068] The difference between this embodiment and embodiment 1 is that:

[0069] The release layer is coated with the following raw materials in parts by weight: 90 parts of toluene, 7 parts of polystyrene resin (Tg is 120° C.), 2.75 parts of ethylene-vinyl acetate resin and 0.25 parts of styrene-butadiene rubber, and the coating thickness is 0.6 μm.

[0070] Embodiment 5:

[0071] The difference between this embodiment and embodiment 1 is that:

[0072] The release layer is coated with the following raw materials in parts by weight: 90 parts of toluene, 8 parts of polystyrene resin (Tg is 130° C.), 1.75 parts of ethylene-vinyl acetate resin and 0.25 parts of styrene-butadiene rubber, and the coating thickness is 1 μm.

[0073] It should be noted that, except for the release layer, as long as the type and content of the materials in the other layers are within the aforementioned range, the properties of the obtained products are similar.

[0074] Comparative Example 1:

[0075] The same ink layer, adhesive layer and back coating formulation, coating thickness, coating method and printing method as in Example 1-5 were used, but the resin in the release layer was replaced with a common polyester resin.

[0076] Comparative Example 2:

[0077] The same ink layer, adhesive layer and back coating formulations, coating thickness, coating method and printing method as those in Examples 1-5 were used, but the resin in the release layer was replaced with polyethylene wax.

[0078] Comparative Example 3:

[0079] The same ink layer, adhesive layer and back coating formulation, coating thickness, coating method and printing method as in Examples 1-5 were used, but no release layer was applied.

[0080] Comparative Example 4:

[0081] The same ink layer, adhesive layer and back coating formulation, coating thickness, coating method and printing method as in Examples 1-5 were used, but the release layer did not contain a thermoplastic elastomer material.

[0082] Comparative Example 5:

[0083] The same ink layer, adhesive layer and back coating formulations, coating thickness, coating method and printing method as in Example 1-5 were used, but the polystyrene resin in the release layer was replaced with acrylic resin.

[0084] Performance testing of printed samples of Examples 1-5 and Comparative Examples 1-5.

[0085] Using a label printer (manufactured by Zebra, model 105SLPlus), the resin ribbon prepared in this embodiment was transferred onto coated paper. Figure 2 Lines shown (0.6pt thick); print speed set to 12.7cm / s, print density set to 25.

[0086] The formed image was visually confirmed, and then a 500 g weight was wrapped with a dust-free cloth and scraped 100 times with alcohol, and the evaluation was performed according to the following evaluation criteria:

[0087] A: No obvious loss was observed in the image after alcohol scratching;

[0088] B: Slightly observed missing in the image;

[0089] NG: A large number of deletions are observed in the image.

[0090] Test results:

[0091] project Example 1 Example 2 Example 3 Example 4 Example 5 Print Test NG B A A NG project Comparative Example 1 Comparative Example 2 Comparative Example 3 Comparative Example 4 Comparative Example 5 Print Test B B NG NG NG

[0092] In summary, the above printing test results, Examples 1-5 are compared with Comparative Examples 1-5. Polystyrene resin is added to the release layer, and an acrylic resin with a molecular weight of 1000-1800 is selected. Too low or too high a molecular weight may cause uneven distribution of the coating liquid on the surface of the substrate. Selecting this molecular weight range can reduce the poor transfer problem caused by too high a molecular weight while taking into account the transfer effect; the TG (melting point) value of the acrylic resin is 35°C-100°C, preferably 65°C-85°C. A higher TG value can ensure that the tailing problem is not generated after the resin melts when the print head is heated, and can further improve the clarity of the image of the uneven transfer body, and reduce transfer defects such as falling blocks and tailing; the thermoplastic elastomer material in the release layer can improve the flexibility of the thermal transfer carbon ribbon and improve the scratch resistance of the transfer pattern; Examples 1-5 are selected to compare with Comparative Example 3. Setting a release layer can improve the integrity of the transfer pattern.

[0093] In the description of this specification, the description with reference to the terms "one embodiment", "some embodiments", "example", "specific example", or "some examples" etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representations of the above terms do not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described may be combined in any one or more embodiments or examples in a suitable manner. In addition, those skilled in the art may combine and combine the different embodiments or examples described in this specification and the features of the different embodiments or examples, without contradiction.

[0094] The above are only preferred embodiments of the present invention and are not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. A thermal transfer sheet that can transfer high-resolution patterns and is friction-resistant. It is characterized in that It includes a back coating layer, a substrate, a release layer, an ink layer and an adhesive layer which are sequentially laminated from top to bottom; The release layer is formed by mixing the following raw materials in parts by weight and then coating: 90 parts of toluene, 5 parts of polystyrene resin with a Tg of 85° C., 4.75 parts of ethylene-vinyl acetate resin and 0.25 parts of styrene-butadiene rubber; Or the release layer is formed by mixing the following raw materials in parts by weight and then coating: 90 parts of toluene, 6 parts of polystyrene resin with a Tg of 100° C., 3.75 parts of ethylene-vinyl acetate resin and 0.25 parts of styrene-butadiene rubber; Or the release layer is formed by mixing the following raw materials in parts by weight and then coating: 90 parts of toluene, 7 parts of polystyrene resin with a Tg of 120° C., 2.75 parts of ethylene-vinyl acetate resin and 0.25 parts of styrene-butadiene rubber; The ink layer is formed by mixing the following raw materials in parts by weight and then coating: 70-80 parts of solvent, 10-20 parts of polyester resin, 10-15 parts of coloring pigment and 0-5 parts of dispersant; The adhesive layer is formed by mixing the following raw materials in parts by weight and then coating: 40-60 parts of solvent, 10-20 parts of polyester resin, and 20-40 parts of adhesive resin; The bonding resin is ethylene-vinyl acetate resin; The average molecular weight of the polystyrene resin is 1000-1800.

2. The thermal transfer sheet capable of transferring high-resolution patterns and resistant to friction according to claim 1, It is characterized in that The matrix is ​​any one of polypropylene, polyethylene naphthalate, polyethylene terephthalate, polyethylene, polyvinyl alcohol, and polymethyl methacrylate.

3. The thermal transfer sheet capable of transferring high-resolution patterns and resistant to friction according to claim 1, It is characterized in that The thickness of the substrate is 2-15 μm, the thickness of the back coating is 0.2-1.0 μm, the thickness of the release layer is 0.1-1.0 μm, the thickness of the ink layer is 0.3-0.5 μm, and the thickness of the adhesive layer is 0.1-0.3 μm.

4. The thermal transfer sheet capable of transferring high-resolution patterns and resistant to friction according to claim 1, It is characterized in that The back coating layer is any one of polyurethane modified silicone resin, acrylic modified silicone resin, polyvinyl acetal resin, polyvinyl butyral resin, or a combination of two or more thereof.

5. The thermal transfer sheet capable of transferring high-resolution patterns and resistant to friction according to claim 1, It is characterized in that The coloring pigment is carbon black.

6. A method for preparing a thermal transfer sheet capable of transferring high-resolution patterns and resistant to friction according to any one of claims 1 to 5, It is characterized in that The following steps are involved: S1: Prepare solution: Back coating liquid: 40-100 parts of the back coating material are added to 40-60 parts of the solvent to dissolve to prepare the back coating liquid for standby use; Release liquid: add polystyrene resin and ethylene-vinyl acetate resin into toluene to dissolve, then add styrene-butadiene rubber and stir to mix to prepare release liquid for later use; Ink liquid: add 10-20 parts of polyester resin to 70-80 parts of solvent to dissolve, then add 10-15 parts of coloring pigment and 0-5 parts of dispersant, stir and mix, to prepare ink liquid for standby use; Adhesive liquid: add 10-20 parts of polyester resin and 20-40 parts of adhesive resin into 40-60 parts of solvent to dissolve and prepare adhesive liquid for use; S2: stunning; Providing a substrate, and applying corona on both sides of the substrate; S3: coating; The back coating liquid prepared in step S1 is coated on the side of the substrate subjected to corona treatment in step S2, and then dried to form a back coating layer for standby use; Then, the release liquid prepared in step S1 is coated on the side of the substrate away from the back coating layer in step S2, and then dried to form a release layer; Then, the ink prepared in step S1 is coated on the side of the release layer in step S3 away from the substrate, and then dried to form an ink layer; Finally, the adhesive solution prepared in step S1 is coated on the side of the ink layer in step S3 away from the release layer, so as to obtain a thermal transfer sheet capable of transferring high-resolution patterns and being friction-resistant.

7. The method for preparing the thermal transfer sheet capable of transferring high-resolution patterns and being friction-resistant according to claim 6, It is characterized in that In step S3, a ceramic anilox roller with 200 to 250 lines is used to apply the back coating liquid, the coating speed is 60-100 m / min, the drying temperature is 50-100° C., and the drying time is 40-60 s; A ceramic anilox roller with 200 to 250 lines is used to apply the release liquid, the coating speed is 60-100 m / min, the drying temperature is 50-100° C., and the drying time is 40-60 s; The ink is coated with a ceramic anilox roller with 200 to 250 lines, the coating speed is 60-100 m / min, the drying temperature is 40-100° C., and the drying time is 40-60 s; A ceramic anilox roller with 200 to 250 lines is used to coat the adhesive liquid. The coating speed is 60-100 m / min, the drying temperature is 80-100° C., and the drying time is 60-120 s.