A clear-background-color blue-light-proof and infrared-proof resin lens and a preparation method thereof
By adopting a multi-layer film structure and specific processes on the resin lens, combining silicone and oxide materials, the problem of insufficient high temperature resistance and durability of the resin lens is solved, and the low reflectivity, infrared and clear background effect is achieved. Comprehensive improvement.
Patent Information
- Application Number
- CN202211343744.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-10-31
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2042-10-31
AI Technical Summary
While existing resin lenses meet anti-reflection, infrared and blue light resistance, they have insufficient high temperature resistance and durability. In particular, the film layer with clear base color function has a significant impact on the lens stress and affects its normal use.
Using specific UV405 resin lens substrates and multi-layer film structures, including silicone hardened layer, silicon-aluminum composite oxide layer, titanium-niobium composite oxide layer, titanium-niobium composite oxide layer, titanium nitride layer, silicon oxide layer and ITO layer, combined with specific The process and material ratio form a clear base color anti-infrared film layer, and add a waterproof layer to the surface to improve the high temperature and durability of the lens.
It achieves low reflectivity, good anti-infrared effect and clear background color visual effect, and significantly improves the high-temperature resistance and durability of the lens, ensuring the stability and mass production of the lens in high temperature and high humidity environments.
Smart Images

Figure CN115616797B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of resin lens preparation, and in particular to a clear-bottom-color, blue-light-proof, infrared-proof, and high-temperature-resistant resin lens and a preparation method thereof. Background Art
[0002] In recent years, the demand for optical resin lenses in the domestic and international eyewear markets has been growing. Compared with glass lenses, resin lenses have the advantages of light weight, good dyeing performance, and easy processing. Medium and high refractive index optical resin lenses are favored by users for their unique advantages such as high light transmittance, UV protection, and ultra-thinness.
[0003] In order to meet the requirements of the optical performance of resin lenses, a film is generally coated on the surface of the resin lens to reduce the reflection of light and enhance the transmission of light, which is an optical anti-reflection film. Near-infrared is not sensitive to the human eye and is mainly absorbed by the cornea, which has potential damage to the human eye. This requires that the optical film layer has the characteristics of anti-reflection and infrared protection. Such an optical film layer is much thicker than a general conventional film layer. In addition, since the main material of the optical film is an inorganic material, and the polymer resin lens substrate is an organic material, the difference in the physical and chemical properties of the two leads to higher stress in the lens after coating, which in turn leads to poor temperature resistance and durability. In particular, the film layer with clear background color and infrared protection function is generally thicker, which has a particularly significant effect on the stress of the lens after coating, affecting its normal use. Therefore, how to provide a low-reflection, infrared-proof, high-temperature-resistant and durable resin lens has become an urgent problem to be solved in this field.
[0004] Blue light protection can effectively protect consumers from the demands of electronic use environments. The new national blue light protection standard also distinguishes between harmful blue light and beneficial blue light. However, blue light protection usually makes the lenses more yellow and less bright. In order to meet the new demands of consumers in the new electronic environment, we urgently need to provide a blue light protection resin lens with a clear base color.
[0005] Therefore, we need to provide new resin lens products that comprehensively meet the performance and protection requirements of anti-reflection, blue light protection, infrared protection, and the aesthetic requirements of clear background color. Summary of the invention
[0006] In order to overcome the defects of the prior art, the present invention aims to provide a clear background color, blue light protection, infrared protection and high temperature resistant resin lens and a preparation method thereof, which can effectively meet the anti-reflection requirements, achieve good infrared protection effect, improve the high temperature resistance and durability of the resin lens by reducing stress, and use special processes to plate special materials to meet the national blue light protection standards and clear background color visual effects.
[0007] The present invention is achieved through the following technical solutions:
[0008] The first aspect of the present invention provides a clear base color, blue light proof, infrared proof and high temperature resistant resin lens, comprising: a resin lens substrate, a hardened layer and a clear base color infrared proof layer; wherein the resin lens substrate, the hardened layer and the clear base color infrared proof film layer are arranged in sequence, the hardened layer is located on the surface of the resin lens substrate, and the clear base color infrared proof film layer is located on the surface of the hardened layer;
[0009] The UV cutoff wavelength of the resin lens substrate is 405-407nm;
[0010] Furthermore, the clear base color infrared-proof and high temperature-resistant resin lens further comprises a waterproof layer, and the waterproof layer is located on the surface of the clear base color infrared-proof film layer;
[0011] Furthermore, the material of the hardened layer is organic silicon; further preferably, the organic silicon contains at least Ti element;
[0012] Further, the clear background color anti-infrared film layer includes a silicon-aluminum composite oxide layer, a titanium-niobium composite oxide layer, a tin-doped indium oxide (i.e., ITO) layer, and a titanium nitride (TiN) layer; further, the clear background color anti-infrared film layer includes three layers of silicon-aluminum composite oxide layers, three layers of titanium-niobium composite oxide layers, a layer of tin-doped indium oxide (i.e., ITO) layer, a layer of silicon dioxide, and a layer of titanium nitride (TiN);
[0013] Further, the silicon-aluminum composite oxide layer is composed of a composite material of SiO2 and Al2O3, wherein the molar fraction of SiO2 in the composite material is 70% to 95%; further preferably, wherein the molar fraction of SiO2 in the composite material is 92%;
[0014] Further, the titanium-niobium composite oxide layer is composed of a composite material of TiO2 and Nb2O5, wherein TiO2 accounts for 10% to 90% of the molar fraction of the composite material; preferably, TiO2 accounts for 80% of the molar fraction of the composite material;
[0015] Furthermore, the purity of TiN in the titanium nitride layer is greater than 99.9%;
[0016] Furthermore, the thickness of the hardened layer is 1 to 5 μm;
[0017] Furthermore, the thickness of the clear base color anti-infrared film layer is 290 to 950 nm;
[0018] Furthermore, the thickness of the waterproof layer is 4 to 20 nm;
[0019] Furthermore, the average reflectivity of the clear-base-color blue-light-proof and infrared-proof resin high-temperature-resistant lens is ≤1.5%;
[0020] Furthermore, the near infrared blocking rate of the clear base color anti-blue light and anti-infrared resin high temperature resistant lens is greater than 55%;
[0021] Furthermore, the yellow index of the clear base color blue light and infrared resistant resin high temperature resistant lens is ≤4.5%;
[0022] The second aspect of the present invention provides a method for preparing the above-mentioned clear base color blue light and infrared resistant resin high temperature resistant lens, comprising the following steps:
[0023] S1: preparing a hard layer: forming a hard layer on the surface of a resin lens substrate, i.e. obtaining a resin lens containing a hard layer;
[0024] S2 preparing a clear base color anti-infrared film layer: forming the clear base color anti-infrared film layer on the surface of the resin lens obtained in S1, that is, obtaining a resin lens containing a clear base color anti-infrared film layer, specifically comprising:
[0025] S21: forming a resin lens having a first silicon-aluminum composite oxide layer and a second titanium-niobium composite oxide layer on the surface of the resin lens obtained in step S1;
[0026] S22: forming a third layer of a resin lens containing a titanium nitride layer on the surface of the resin lens obtained in step S21;
[0027] S23: forming a fourth SiO2 layer-containing resin lens on the surface of the resin lens obtained in step S22;
[0028] S24: forming a fifth titanium-niobium composite oxide layer, a sixth silicon-aluminum composite oxide layer, and a seventh titanium-niobium composite oxide layer on the surface of the resin lens obtained in step S23;
[0029] S25: forming an eighth ITO-containing resin lens on the surface of the resin lens obtained in step S24;
[0030] S26: forming a ninth layer of a resin lens containing a silicon-aluminum composite oxide layer on the surface of the resin lens obtained in step S25;
[0031] S3: preparing a waterproof layer: forming a waterproof layer on the surface of the resin lens obtained in step S2.
[0032] Beneficial Effects
[0033] 1. The present invention adopts a specific UV405 resin lens substrate to make the lens close to the blue light protection standard and maintain a low yellow index;
[0034] 2. The present invention adopts a specific film layer to make the lens have the effects of infrared protection, blue light protection and clear background color, which specifically includes: (1) using titanium niobium composite oxide material to prepare the film layer so that it has infrared protection effect, improves the temperature resistance and durability of the product, and improves the repeatability and mass production of the product, and significantly improves the temperature resistance and durability of the lens: a. TiO2 is doped with a certain molar ratio of Nb2O5 to effectively avoid the easy crystallization characteristics of the TiO2 film layer, and can also effectively avoid the defect of the dense Nb2O5 film layer being easy to crack on the resin lens. In the case of low ion source energy for coating resin glasses, the film layer is ensured to be in an amorphous state to prevent the film layer from cracking due to crystallization, thereby improving the high temperature and high humidity resistance of the film layer and the lens, and further improving the heat resistance and durability of the lens. And improve the durability of the product; b. In addition, when preparing the low-reflection titanium-niobium composite oxide film layer, since the film material is doped with TiO2 and Nb2O5, the sensitivity of TiO2 to the O2 flow in the IAD auxiliary process is reduced, the process difficulty is reduced and the repeatability and mass production of the product are effectively improved: c. The film material adopts a composite material of TiO2 and Nb2O5, and the optical refractive index is close to that of TiO2, which is higher than the refractive index of materials such as Nb2O5, so that the anti-infrared cutoff effect is better, the reflectivity of the anti-reflection film is lower, and the infrared cutoff is deeper than other existing products, and the light transmittance of the resin lens is improved, so that the lens prepared by the present invention has a good visual effect while protecting the human eye and reducing near-infrared radiation;
[0035] (2) The TiN layer prepared by a specific process can supplement the anti-blue light standard, enhance infrared blocking, and reduce the yellow index to increase the effect of clearing the background color. The film layer produces 2% absorption on one side of the 415-445nm band, which is important for the anti-blue light standard, to ensure that the lens meets the anti-blue light standard and protects the human eye from blue light damage; the absorption of yellow light is about 0.6% higher than that of blue light, thereby effectively reducing the yellow index and ensuring that the lens is clear and white; the absorption of near-infrared is above 3%, which effectively increases the infrared blocking rate and reduces the damage of infrared to the human eye;
[0036] (3) Improving the high temperature resistance of the product: The present invention uses a silicon-aluminum composite oxide layer and a SiO2 layer in combination, which effectively avoids the high stress of the film layer caused by the easy formation of long columns by SiO2, maintains the glassy structure of the film layer, and improves the high temperature resistance of the film layer. BRIEF DESCRIPTION OF THE DRAWINGS
[0037] Figure 1Schematic diagram of the layers of a clear base color infrared-proof resin lens prepared by embodiments 1 to 4 of the present invention; resin lens substrate 1, hardened layer 2, clear base color infrared-proof film layer 3, waterproof layer 4; wherein the clear base color infrared-proof film layer 3 includes: a silicon-aluminum composite oxide layer 3-1, a titanium-niobium composite oxide layer 3-2, a titanium nitride layer 3-3 plated by a special process, a silicon dioxide layer 3-4, a titanium-niobium composite oxide layer 3-5, a silicon-aluminum composite oxide layer 3-6, a titanium-niobium composite oxide layer 3-7, an ITO layer 3-8, and a silicon-aluminum composite oxide layer 3-9 DETAILED DESCRIPTION
[0038] In a specific embodiment, the clear background color infrared protection film layer includes three silicon-aluminum composite oxide layers, three titanium-niobium composite oxide layers, a titanium nitride layer, a silicon dioxide layer, and a tin-doped indium oxide (i.e., ITO) layer, wherein the clear background color infrared protection film layer comprises the following layers in order: (1) silicon-aluminum composite oxide layer, (2) titanium-niobium composite oxide layer, (3) titanium nitride layer, (4) silicon dioxide layer, (5) titanium-niobium composite oxide layer, (6) silicon-aluminum composite oxide layer, (7) titanium-niobium composite oxide layer, (8) tin-doped indium oxide (i.e., ITO) layer, and (9) silicon-aluminum composite oxide layer; and the first silicon-aluminum composite oxide layer is located on the surface of the hardened layer;
[0039] Furthermore, in a specific embodiment, the thickness of each layer of the clear base color anti-infrared film layer is:
[0040] The thickness of the first silicon-aluminum composite oxide layer is 0 to 180 nm, preferably 5 to 30 nm;
[0041] The thickness of the second titanium-niobium composite oxide layer is 10 to 40 nm, preferably 10 to 20 nm;
[0042] The thickness of the third titanium nitride layer is 0.5 to 2 nm, preferably 0.7 to 1.2 nm;
[0043] The thickness of the fourth silicon dioxide layer is 20 to 60 nm, preferably 30 to 50 nm;
[0044] The thickness of the fifth titanium-niobium composite oxide layer is 80 to 150 nm, preferably 100 to 120 nm;
[0045] The thickness of the sixth silicon-aluminum composite oxide layer is 90 to 250 nm, preferably 140 to 200 nm;
[0046] The thickness of the seventh titanium-niobium composite oxide layer is 80 to 150 nm, preferably 90 to 110 nm;
[0047] The thickness of the eighth ITO layer is 2 to 10 nm, preferably 5 nm;
[0048] The thickness of the ninth silicon-aluminum composite oxide layer is 60 to 130 nm, preferably 65 to 90 nm;
[0049] In a specific embodiment, the step of preparing the hardened layer in S1 comprises: immersing the ultrasonically cleaned resin lens substrate in a 25-30% by weight hardening solution aqueous solution at a dipping temperature of 10-20° C., dipping for 4-8 seconds and then pulling out the solution at a speed of 1.0-3.0 mm / s, and then drying it at 70-90° C. for 2-5 hours, then taking out the substrate and sending it to a drying oven for drying and curing, the curing temperature is 100-150° C., and the curing time is 120-180 min, so as to obtain a resin lens containing a hardened layer;
[0050] In a specific embodiment, the process of preparing the clear base color infrared protection film layer in step S2 comprises:
[0051] In a vacuum coating machine, a vacuum coating process is adopted to evaporate silicon-aluminum composite oxide layer, titanium-niobium composite oxide, titanium nitride, silicon dioxide and ITO solid film layer materials, and then transmit them through the gas phase to deposit them into a thin film on the surface of the resin lens obtained in step S1 to form a clear base color anti-infrared film layer, which specifically includes the following steps:
[0052] S21: forming a first layer of silicon-aluminum composite oxide layer on the surface of the resin lens obtained in step S1, and the background vacuum degree is ≤3×10 -3 Pa, and the temperature in the coating chamber is 50-70°C, and an ion source is used to assist the process, a high-energy electron beam is used to heat the silicon-aluminum composite oxide at a rate of Depositing the evaporated silicon-aluminum composite oxide in the form of nano-scale molecules to obtain a resin lens containing a first silicon-aluminum composite oxide layer;
[0053] S22: forming a titanium-niobium composite oxide layer on the surface of the resin lens obtained in step S21; the surface of the resin lens obtained in step S21 has a background vacuum degree of ≤3×10 -3 Pa, and the temperature in the coating chamber is 50-70°C, and an ion source is used to assist the process, a high-energy electron beam is used to heat the titanium-niobium composite oxide at a rate of Depositing the evaporated titanium-niobium composite oxide in the form of nano-scale molecules to obtain a resin lens containing a second titanium-niobium composite oxide layer;
[0054] S23: forming a titanium nitride layer on the surface of the resin lens obtained in step S22, specifically comprising:
[0055] S231: First evacuate to the background vacuum degree ≤8×10 -4Pa, and then bombarded with an ion source Hall source for 50 to 80 seconds, the ion source bombardment parameters are: anode voltage: 90 to 140 V, anode current: 2.5 to 5 A, auxiliary gas is Ar, and the flow rate is 5 to 20 sccm; preferably, the ion source Hall source bombardment time is 60 seconds, and the ion source bombardment parameters are: anode voltage: 110 V, anode current: 3 A, auxiliary gas is Ar, and the flow rate is 10 sccm;
[0056] S232: Deposition in an ion source assisted process, using a high energy electron beam to heat TiN at a rate The evaporated TiN is deposited in the form of nano-scale molecules, and the auxiliary parameters of the ion source are: anode voltage: 90-140V, anode current: 2.5-5A, auxiliary gas is Ar and N2, Ar flow rate is 5-15sccm, N2 flow rate is: 3-15sccm; preferably, under the assistance of the ion source, at a rate The evaporated TiN is deposited in the form of nano-scale molecules, and the auxiliary parameters of the ion source are: anode voltage: 110V, anode current: 3A, auxiliary gas is Ar and N2, Ar flow rate is 10sccm, N2 flow rate is: 5sccm;
[0057] S233: continue to bombard the TiN film surface with the ion source Hall source for 20 to 40 seconds, the bombardment parameters are: anode voltage: 90 to 140 V, anode current: 2.5 to 5 A, auxiliary gas is Ar and N2, Ar flow rate is 5 to 15 sccm, N2 flow rate is: 3 to 15 sccm; preferably, the bombardment time is 30 seconds, the bombardment parameters are: anode voltage: 110 V, anode current: 3 A, auxiliary gas is Ar and N2, Ar flow rate is 10 sccm, N2 flow rate is: 5 sccm;
[0058] S24: The surface of the resin lens obtained in S23 has a background vacuum of ≤3×10 -3 Pa, and the temperature in the coating chamber is 50-70℃, and there is an ion source assisted process, high-energy electron beam is used to heat SiO2 at a rate of The evaporated SiO2 is deposited in the form of nano-scale molecules to obtain a resin lens containing a SiO2 layer; the ion source auxiliary parameters are: anode voltage: 90-140V, anode current: 2.5-5A, auxiliary gas is Ar, and the flow rate is 5-20sccm; preferably, the rate is 100% under the assistance of the ion source. The evaporated SiO2 was deposited in the form of nano-scale molecules, and the ion source bombardment auxiliary parameters were: anode voltage: 110V, anode current: 3A, auxiliary gas was Ar, and the flow rate was 10sccm;
[0059] S25: repeating step S22 to form a titanium-niobium composite oxide layer on the surface of the resin lens obtained in step S24;
[0060] S26: repeat step S21 to form a silicon-aluminum composite oxide layer on the surface of the resin lens obtained in step S25;
[0061] S27: repeat step S22 to form a titanium-niobium composite oxide layer on the surface of the resin lens obtained in step S26;
[0062] S28: The surface of the resin lens obtained in S27 has a background vacuum of ≤3×10 -3 Pa, and the temperature in the coating chamber is 50-70℃, and there is an ion source assisted process, high-energy electron beam is used to heat ITO at a rate of Depositing the evaporated ITO in the form of nano-scale molecules to obtain a resin lens containing an ITO layer;
[0063] S29: continuing to use the vacuum coating process on the surface of the resin lens obtained in S28, repeating the process steps of S21, and then forming a layer of resin lens containing a silicon-aluminum composite oxide layer;
[0064] In steps S21, S22, S25 to S29, the ion source assisted deposition process parameters are: the ion source is a Hall source, the anode voltage is 90 to 140 V, the anode current is 2.5 to 5 A, the auxiliary gas is O2, and the flow rate is 10 to 30 sccm; preferably, the ion source assisted deposition process parameters are: the ion source is a Hall source, the anode voltage is 110 V, the anode current is 3 A, the auxiliary gas is O2, and the flow rate is 15 sccm;
[0065] In a specific embodiment, the step S3: forming a waterproof layer on the surface of the resin lens obtained in step S2 comprises the following steps: continuing to use the vacuum coating process on the surface of the lens obtained in step S29, and the vacuum degree of the background is ≤3×10 - 3 Pa, and the temperature in the coating chamber is 50-70℃, high-energy electron beam is used to heat the material at a rate of The evaporated fluorine-containing waterproof material (preferably containing perfluoroalkane (C 12 F 27 The waterproof material N) is deposited in the form of nano-scale molecules to obtain a resin lens containing a waterproof layer;
[0066] In a specific embodiment, the titanium nitride material has a molecular formula of TiN and a purity of 99.9%, and is made by sintering titanium nitride powder using a conventional process, and is specifically commissioned to Changzhou Zhanchi Optoelectronics Technology Co., Ltd. for development and production;
[0067] In a specific embodiment, the silicon-aluminum composite oxide is developed and produced by Changzhou Zhanchi Optoelectronics Technology Co., Ltd. The silicon-aluminum composite oxide layer is composed of a composite material of SiO2 and Al2O3, and the molar fraction of SiO2 in the composite material is 70% to 95%. For specific models, please refer to the embodiments and comparative examples;
[0068] In a specific embodiment, the titanium-niobium composite oxide is developed and produced by Changzhou Zhanchi Optoelectronics Technology Co., Ltd. The titanium-niobium composite oxide is composed of TiO2 and Nb2O5, wherein the molar fraction of TiO2 is 10% to 90%. For specific models, see the examples and comparative examples.
[0069] The resin lens substrate selected in the present invention is a conventional lens in the art, and the content of the UV powder is adjusted so that the UV cut-off wavelength is 405-407 nm. The definition of the UV cut-off wavelength refers to 5.4.2.4.4 of the optical resin lens standard QB / T 2506-2017;
[0070] For example, in a specific embodiment, a resin lens substrate with model MR-8 (refractive index 1.60) or MR-7 (refractive index 1.67) and a UV cutoff wavelength of 405 to 407 nm is purchased from Mitsui Chemicals, Inc. of Japan, hereinafter referred to as "MR-8-UV405" or "MR-7-UV405"; or in a specific embodiment, a resin lens substrate with a refractive index of 1.56 and a UV cutoff wavelength of 405 to 407 nm developed and produced by Jiangsu Shike New Materials Co., Ltd. is purchased, hereinafter referred to as "SK1.56-UV405". For the specific preparation method of the resin lens substrate, refer to the patent of Shike Optics Co., Ltd.: CN201410245692.6.
[0071] The present invention can select a conventional hardening liquid. For example, in a specific embodiment, the hardening liquid model Z117 or Z118 (hereinafter referred to as "Z117" or "Z118") of Ito Optical Industry Co., Ltd. is selected; or in a specific embodiment, the hardening liquid model VH56 (hereinafter referred to as "VH56") of Dun Optics (Changshu) Co., Ltd. is selected. Selecting the hardening liquid for coating greatly improves the dense connection between the film layers.
[0072] (I) Embodiment
[0073] Example 1
[0074] A clear base color infrared-proof resin lens, which comprises, in order: a resin lens substrate 1 (MR-8-UV405); a hardening layer 2 (Z117) / 2.6-3 μm; a clear base color infrared-proof film layer comprising: a silicon-aluminum composite oxide layer 3-1 (wherein the molar percentage of SiO2 and Al2O3 is: 92% SiO2: 8% Al2O3; commissioned by Changzhou Zhanchi Optoelectronics Technology Co., Ltd. to develop and produce, the material model is SA56) / 26 nm, a titanium-niobium composite oxide layer 3-2 (wherein the molar percentage of TiO2 and Nb2O5 is: 80% TiO2: 20% Nb2O5; commissioned by Changzhou Zhanchi Optoelectronics Technology Co., Ltd. to develop and produce, the material model is PTN28) / 12. 48nm, titanium nitride layer 3-3 (molecular formula TiN, purity above 99.9%, sintered by Changzhou Zhanchi Optoelectronics Technology Co., Ltd.) / 1.0nm, silicon dioxide layer 3-4 / 34.5nm (molecular formula SiO2, purity 99.99%, sintered by Danyang Keda Coating Materials Co., Ltd.), titanium niobium composite oxide layer 3-5 (material is the same as 3-2) / 114.5nm, silicon aluminum composite oxide layer 3-101.66 / 160.4nm (material is the same as 3-1); titanium niobium composite oxide layer 3-7 (material is the same as 3-2) / 101.6nm; ITO layer 3-8 / 5nm; silicon aluminum composite oxide layer 3-9 / 71.0nm (material is the same as 3-1); waterproof layer 4 (using C-containing 12 F 27 N waterproof material / 10nm);
[0075] The method for preparing the resin lens comprises the following steps:
[0076] S1: Making a hard layer: immerse the resin lens substrate cleaned by ultrasonic wave into a 27% by weight hardening liquid aqueous solution of model Z117 at a dipping temperature of 15°C, and pull out the solution at a speed of 2.0 mm / s after dipping for 5 seconds; after drying at 80°C for 3 hours, take out the substrate and send it to a drying oven for drying and curing at a curing temperature of 120°C for 150 minutes, thereby obtaining a resin lens with a hardening layer;
[0077] S2: preparing a clear background color infrared-proof film layer: in a vacuum coating machine, using a vacuum coating process, evaporating the solid film material and then transmitting it through the gas phase, and depositing it into a thin film on the surface of the resin lens obtained in step S1 to form a clear background color infrared-proof film layer, specifically comprising the following steps:
[0078] S21: forming a silicon-aluminum composite oxide layer on the surface of the resin lens obtained in step S1. -3 Pa, and the temperature in the coating chamber is 50-70°C, and an ion source is used to assist the process, a high-energy electron beam is used to heat the silicon-aluminum composite oxide at a rate of Depositing the evaporated silicon-aluminum composite oxide in the form of nano-scale molecules to obtain a resin lens containing a first silicon-aluminum composite oxide layer;
[0079] S22: forming a titanium-niobium composite oxide layer on the surface of the resin lens obtained in step S21. The surface of the resin lens obtained in step S21 has a background vacuum degree of ≤3×10 -3 Pa, and the temperature in the coating chamber is 50-70°C, and an ion source is used to assist the process, a high-energy electron beam is used to heat the titanium-niobium composite oxide at a rate of Depositing the evaporated titanium-niobium composite oxide in the form of nano-scale molecules to obtain a resin lens containing a second titanium-niobium composite oxide layer;
[0080] S23: forming a titanium nitride layer on the surface of the resin lens obtained in step S22, specifically comprising the following steps: S231: first evacuating to a background vacuum degree of ≤8×10 -4 Pa, and then bombarded with an ion source Hall source for 60 seconds. The ion source bombardment parameters are: anode voltage: 110V, anode current: 3A, auxiliary gas is Ar, and the flow rate is 10sccm; S232: Deposition under the ion source assisted process, using a high-energy electron beam to heat TiN at a rate The evaporated TiN is deposited in the form of nanoscale molecules, and the auxiliary parameters of the ion source are: anode voltage: 110V, anode current: 3A, auxiliary gases are Ar and N2, Ar flow rate is 10sccm, N2 flow rate is: 5sccm; S233: continue to bombard the TiN film surface with the ion source Hall source for 30 seconds, and the bombardment parameters are: anode voltage: 110V, anode current: 3A, auxiliary gases are Ar and N2, Ar flow rate is 10sccm, N2 flow rate is: 5sccm.
[0081] S24: The surface of the resin lens obtained in S23 has a background vacuum of ≤3×10 -3 Pa, and the temperature in the coating chamber is 50-70℃, and there is an ion source assisted process, high-energy electron beam is used to heat SiO2 at a rate of The evaporated SiO2 is deposited in the form of nano-scale molecules to obtain a resin lens containing a SiO2 layer; the auxiliary parameters of the ion source are: anode voltage: 110V, anode current: 3A, auxiliary gas is Ar, and the flow rate is 10sccm.
[0082] S25: repeating step S22 to form a titanium-niobium composite oxide layer on the surface of the resin lens obtained in step S24;
[0083] S26: repeat step S21 to form a silicon-aluminum composite oxide layer on the surface of the resin lens obtained in step S25;
[0084] S27: repeat step S22 to form a titanium-niobium composite oxide layer on the surface of the resin lens obtained in step S26;
[0085] S28: The surface of the resin lens obtained in S27 has a background vacuum of ≤3×10 -3 Pa, and the temperature in the coating chamber is 50-70℃, and there is an ion source assisted process, high-energy electron beam is used to heat ITO at a rate of Depositing the evaporated ITO in the form of nano-scale molecules to obtain a resin lens containing an ITO layer;
[0086] S29: continuing to use the vacuum coating process on the surface of the resin lens obtained in S28, repeating the process steps of S21, and then forming a layer of resin lens containing a silicon-aluminum composite oxide layer;
[0087] S3: preparing a waterproof layer: forming a waterproof layer on the surface of the resin lens obtained in step S29: continuing to use the vacuum coating process on the surface of the lens obtained in step S29, with a background vacuum degree of ≤3×10 -3 Pa, and the temperature in the coating chamber is 60℃, a high-energy electron beam is used to heat the material at a rate of The evaporated C 12 F 27 The waterproof material of N is deposited on the surface of the resin lens obtained in S24 in the form of nano-scale molecules.
[0088] Example 2
[0089] A clear-base-color infrared-proof resin lens, which comprises, in order: a resin lens substrate 1 (SK1.56-UV405); a hardened layer 2 (VH56) / 1-2.6 μm; a clear-base-color infrared-proof film layer comprising: a silicon-aluminum composite oxide layer 3-1 (wherein the molar percentage of SiO2 and Al2O3 is: 92% SiO2: 8% Al2O3; commissioned by Changzhou Zhanchi Optoelectronics Technology Co., Ltd. to develop and produce, the material model is SA56) / 26 nm, a titanium-niobium composite oxide layer 3-2 (wherein the molar percentage of TiO2 and Nb2O5 is: 80% TiO2: 20% Nb2O5; commissioned by Changzhou Zhanchi Optoelectronics Technology Co., Ltd. to develop and produce, the material model is PTN28) / 11.8nm, titanium nitride layer 3-3 (molecular formula TiN, purity above 99.9%, sintered by Changzhou Zhanchi Optoelectronics Technology Co., Ltd.) / 1.0nm, silicon dioxide layer 3-4 / 35.26nm (molecular formula SiO2, purity 99.99%, sintered by Danyang Keda Coating Materials Co., Ltd.), titanium niobium composite oxide layer 3-5 (material is the same as 3-2) / 114.2nm, silicon aluminum composite oxide layer 3-6 / 160.4nm (material is the same as 3-1); titanium niobium composite oxide layer 3-7 (material is the same as 3-2) / 101.7nm; ITO layer 3-8 / 5nm; silicon aluminum composite oxide layer 3-9 / 70.83nm (material is the same as 3-1); waterproof layer 4 (using C-containing 12 F 27 N waterproof material / 10nm).
[0090] The method for preparing the resin lens comprises the following steps:
[0091] S1: Making a hard layer: immerse the resin lens substrate cleaned by ultrasonic wave into a 30% by weight hardening liquid aqueous solution of model VH56 at a dipping temperature of 15°C, and pull out the solution at a speed of 2.0 mm / s after dipping for 5 seconds; after drying at 80°C for 3 hours, take out the substrate and send it to a drying oven for drying and curing at a curing temperature of 120°C and a curing time of 150 minutes, thereby obtaining a resin lens with a hard layer;
[0092] The remaining steps are the same as in Example 1.
[0093] Example 3
[0094] A clear-base-color infrared-proof resin lens, which comprises, in order: a resin lens substrate 1 (MR-7-UV405); a hardened layer 2 (Z118) / 1-2.6 μm; a clear-base-color infrared-proof film layer comprising: a silicon-aluminum composite oxide layer 3-1 (wherein the molar percentage of SiO2 and Al2O3 is: 92% SiO2: 8% Al2O3; commissioned by Changzhou Zhanchi Optoelectronics Technology Co., Ltd. to develop and produce, the material model is SA56) / 26 nm, a titanium-niobium composite oxide layer 3-2 (wherein the molar percentage of TiO2 and Nb2O5 is: 80% TiO2: 20% Nb2O5; commissioned by Changzhou Zhanchi Optoelectronics Technology Co., Ltd. to develop and produce, the material model is PTN28) / 14 .34nm, titanium nitride layer 3-3 (molecular formula TiN, purity above 99.9%, sintered by Changzhou Zhanchi Optoelectronics Technology Co., Ltd.) / 1.0nm, silicon dioxide layer 3-4 / 34.1nm (molecular formula SiO2, purity 99.99%, sintered by Danyang Keda Coating Materials Co., Ltd.), titanium niobium composite oxide layer 3-5 (material is the same as 3-2) / 116.05nm, silicon aluminum composite oxide layer 3-6 / 160.78nm (material is the same as 3-1); titanium niobium composite oxide layer 3-7 (material is the same as 3-2) / 101.34nm; ITO layer 3-8 / 5nm; silicon aluminum composite oxide layer 3-9 / 70.0nm (material is the same as 3-1); waterproof layer 4 (using C-containing 12 F 27 N waterproof material / 10nm).
[0095] The method for preparing the resin lens comprises the following steps:
[0096] S1: Making a hard layer: immerse the resin lens substrate cleaned by ultrasonic wave into a 27% by weight hardening liquid aqueous solution of model Z118 at a temperature of 15°C, and pull out the solution at a speed of 2.0 mm / s after immersion for 5 seconds; after drying at 80°C for 3 hours, take out the substrate and send it to a drying oven for drying and curing at a temperature of 120°C for 150 minutes, thereby obtaining a resin lens with a hard layer;
[0097] The remaining steps are the same as in Example 1.
[0098] Example 4
[0099] A clear-base-color infrared-proof resin lens, which comprises, in order: a resin lens substrate 1 (MR-8-UV405); a hardened layer 2 (Z117) / 2.6-3 μm; a clear-base-color infrared-proof film layer comprising: a silicon-aluminum composite oxide layer 3-1 (wherein the molar percentage of SiO2 and Al2O3 is: 92% SiO2: 8% Al2O3; commissioned by Changzhou Zhanchi Optoelectronics Technology Co., Ltd. to develop and produce, the material model is SA56) / 26 nm, a titanium-niobium composite oxide layer 3-2 (wherein the molar percentage of TiO2 and Nb2O5 is: 80% TiO2: 20% Nb2O5; commissioned by Changzhou Zhanchi Optoelectronics Technology Co., Ltd. to develop and produce, the material model is PTN28) / 1 2.48nm, titanium nitride layer 3-3 (molecular formula TiN, purity above 99.9%, sintered by Changzhou Zhanchi Optoelectronics Technology Co., Ltd.) / 0.75nm, silicon dioxide layer 3-4 / 34.5nm (molecular formula SiO2, purity 99.99%, sintered by Danyang Keda Coating Materials Co., Ltd.), titanium niobium composite oxide layer 3-5 (material is the same as 3-2) / 114.5nm, silicon aluminum composite oxide layer 3-6 / 160.4nm (material is the same as 3-1); titanium niobium composite oxide layer 3-7 (material is the same as 3-2) / 101.6nm; ITO layer 3-8 / 5nm; silicon aluminum composite oxide layer 3-9 / 71.0nm (material is the same as 3-1); waterproof layer 4 (using C-containing 12 F 27 N waterproof material / 10nm);
[0100] The preparation method is the same as that of Example 1.
[0101] (II) Comparative Example
[0102] Comparative Example 1
[0103] A clear bottom color infrared-proof resin lens, which comprises, in order: a resin lens substrate 1 (MR-8-UV405); a hardened layer 2 (Z117) / 2.6-3 μm; a light green infrared-proof film layer comprising: a SiO2 layer 3-1 / 24.6 nm, a ZrO2 layer 3-2 / 8.42 nm, a SiO2 layer 3-3 / 51.42 nm, a ZrO2 layer 3-4 / 118.72 nm, a SiO2 layer 3-5 / 160.59 nm, a ZrO2 layer 3-6 / 80.64 nm, an ITO layer 3-7 / 5 nm; a SiO2 layer 3-8 / 66.3 nm; a waterproof layer 4 (using a C-containing 12 F 27 N waterproof material / 10nm);
[0104] The preparation method comprises the following steps:
[0105] S1: Making a hard layer: immerse the resin lens substrate cleaned by ultrasonic wave into a 27% by weight hardening liquid aqueous solution of model Z117 at a dipping temperature of 15°C, and pull out the solution at a speed of 2.0 mm / s after dipping for 5 seconds; after drying at 80°C for 3 hours, take out the substrate and send it to a drying oven for drying and curing at a curing temperature of 120°C for 150 minutes, thereby obtaining a resin lens with a hardening layer;
[0106] S2: preparing a clear background color infrared-proof film layer: in a vacuum coating machine, using a vacuum coating process, evaporating the solid film material and then transmitting it through the gas phase, and depositing it into a thin film on the surface of the resin lens obtained in step S1 to form a clear background color infrared-proof film layer, specifically comprising the following steps:
[0107] S21: comprising the following steps:
[0108] S211: The surface of the resin lens obtained in S1 has a background vacuum of ≤3×10 -3 Pa, and the temperature in the coating chamber is 60℃, without ion source auxiliary process, high energy electron beam is used to heat SiO2 at a rate of The evaporated SiO2 is deposited in the form of nano-scale molecules to obtain a resin lens containing a first SiO2 layer;
[0109] S212: The surface of the resin lens obtained in S211 has a background vacuum of ≤3×10 -3 Pa, the temperature in the coating chamber is 60℃, and there is no ion source auxiliary process. High-energy electron beam is used to heat ZrO2 at a rate of The evaporated ZrO2 is deposited in the form of nano-scale molecules to obtain a resin lens containing a second ZrO2 layer;
[0110] S213: repeating steps S211 and S212 to alternately form a third SiO2 layer, a fourth ZrO2 layer, a fifth SiO2 layer, and a sixth ZrO2 layer, respectively, to form a resin lens including a third SiO2 layer, a fourth ZrO2 layer, a fifth SiO2 layer, and a sixth ZrO2 layer;
[0111] S22: The surface of the resin lens obtained in S21 has a background vacuum of ≤3×10 -3 Pa, and the temperature in the coating chamber is 60℃, and under the conditions of ion source auxiliary process, high-energy electron beam is used to heat ITO at a rate of Depositing the evaporated ITO in the form of nano-scale molecules to obtain a resin lens containing a seventh ITO layer;
[0112] S23: continuing to use the vacuum coating process on the surface of the resin lens obtained in S22, repeating the process steps of S211, and then forming a resin lens containing an eighth SiO2 layer;
[0113] S3: preparing a waterproof layer: forming a waterproof layer on the surface of the resin lens obtained in S23: continuing to use the vacuum coating process on the surface of the lens obtained in step S2, with a background vacuum degree of ≤3×10 -3 Pa, and the temperature in the coating chamber is 60℃, a high-energy electron beam is used to heat the material at a rate of The evaporated C 12 F 27 The waterproof material of N is deposited on the surface of the resin lens obtained in S24 in the form of nano-scale molecules.
[0114] Comparative Example 2
[0115] A blue anti-reflection and infrared-proof resin lens, which comprises, in order: a resin lens substrate 1 (MR-8-UV405); a hardening layer 2 (Z117) / 2.6-3μm; an anti-reflection layer comprising: a silicon-aluminum composite oxide layer 3-1 (wherein the molar percentage of SiO2 and Al2O3 is: 92% SiO2: 8% Al2O3; commissioned by Changzhou Zhanchi Optoelectronics Technology Co., Ltd. to develop and produce, the material model is SA56) / 27.6nm, a titanium-niobium composite oxide layer 3-2 (wherein the molar percentage of TiO2 and Nb2O5 is: 80% TiO2: 20% Nb2O5 ; Entrusted to Changzhou Zhanchi Optoelectronics Technology Co., Ltd. to develop and produce, the material model is PTN28) / 15.45nm, silicon aluminum composite oxide layer 3-3 / 31.42nm (material is the same as 3-1), titanium niobium composite oxide layer 3-4 (material is the same as 3-2) / 98.9nm, silicon aluminum composite oxide layer 3-5 / 171.92nm (material is the same as 3-1), titanium niobium composite oxide layer 3-6 (material is the same as 3-2) / 91.96nm, ITO layer 3-7 / 5nm; silicon aluminum composite oxide layer 3-8 / 75.8nm (material is the same as 3-1); waterproof layer 4 (using C 12 F 27 N waterproof material / 10nm);
[0116] The method for preparing the resin lens comprises the following steps:
[0117] S1: Making a hard layer: immerse the resin lens substrate cleaned by ultrasonic wave into a 27% by weight hardening liquid aqueous solution of model Z117 at a dipping temperature of 15°C, and pull out the solution at a speed of 2.0 mm / s after dipping for 5 seconds; after drying at 80°C for 3 hours, take out the substrate and send it to a drying oven for drying and curing at a curing temperature of 120°C for 150 minutes, thereby obtaining a resin lens with a hardening layer;
[0118] S2: Preparation of anti-reflection and infrared protection layer: In a vacuum coating machine, a vacuum coating process is adopted to evaporate the solid film material and then transmit it through the gas phase, and then deposit it into a thin film on the surface of the resin lens obtained in step S1 to form an anti-reflection and infrared protection layer, which specifically includes the following steps:
[0119] S21: comprising the following steps:
[0120] S211: The surface of the resin lens obtained in S1 has a background vacuum of ≤3×10 -3 Pa, and the temperature in the coating chamber is 60 ° C, with an ion source assisted process, a high-energy electron beam is used to heat the silicon-aluminum composite oxide at a rate of Depositing the evaporated silicon-aluminum composite oxide in the form of nano-scale molecules to obtain a resin lens containing a first silicon-aluminum composite oxide layer;
[0121] S212: The surface of the resin lens obtained in S211 has a background vacuum of ≤3×10 -3 Pa, the temperature in the coating chamber is 60℃, and there is an ion source assisted process. High-energy electron beam is used to heat the titanium-niobium composite oxide at a rate of Depositing the evaporated titanium-niobium composite oxide in the form of nano-scale molecules to obtain a resin lens containing a second titanium-niobium composite oxide layer;
[0122] S213: repeating steps S211 and S212 to alternately form a third silicon-aluminum composite oxide layer, a fourth titanium-niobium composite oxide layer, a fifth silicon-aluminum composite oxide layer, and a sixth titanium-niobium composite oxide layer, respectively, that is, forming a resin lens including a third silicon-aluminum composite oxide layer, a fourth titanium-niobium composite oxide layer, a fifth silicon-aluminum composite oxide layer, and a sixth titanium-niobium composite oxide layer;
[0123] S22: The surface of the resin lens obtained in S21 has a background vacuum of ≤3×10 -3 Pa, and the temperature in the coating chamber is 60℃, and under the conditions of ion source auxiliary process, high-energy electron beam is used to heat ITO at a rate of Depositing the evaporated ITO in the form of nano-scale molecules to obtain a resin lens containing a seventh ITO layer;
[0124] S23: continuing to use the vacuum coating process on the surface of the resin lens obtained in S22, repeating the process steps of S211, and then forming a resin lens containing an eighth silicon-aluminum composite oxide layer;
[0125] S3: preparing a waterproof layer: forming a waterproof layer on the surface of the resin lens obtained in S23: continuing to use the vacuum coating process on the surface of the lens obtained in step S2, with a background vacuum degree of ≤3×10-3 Pa, and the temperature in the coating chamber is 60℃, a high-energy electron beam is used to heat the material at a rate of The evaporated C 12 F 27 The waterproof material of N is deposited on the surface of the resin lens obtained in S24 in the form of nano-scale molecules.
[0126] Comparative Example 3
[0127] A clear-bottom-color infrared-proof resin lens, which comprises, in order: a resin lens substrate 1 (MR-8-UV405); a hardening layer 2 (Z117) / 2.6-3μm; an anti-reflection layer comprising: a silicon-aluminum composite oxide layer 3-1 (wherein the molar percentage of SiO2 and Al2O3 is: 92% SiO2: 8% Al2O3; commissioned by Changzhou Zhanchi Optoelectronics Technology Co., Ltd. to develop and produce, the material model is SA56) / 26nm, a titanium-niobium composite oxide layer 3-2 (wherein the molar percentage of TiO2 and Nb2O5 is: 80% TiO2: 20% Nb2O5; Entrusted to Changzhou Zhanchi Optoelectronics Technology Co., Ltd. for development and production, the material model is PTN28) / 13.48nm, silicon aluminum composite oxide layer 3-3 / 34.5nm (material is the same as 3-1), titanium niobium composite oxide layer 3-4 (material is the same as 3-2) / 114.5nm, silicon aluminum composite oxide layer 3-5 / 160.4nm (material is the same as 3-1), titanium niobium composite oxide layer 3-6 (material is the same as 3-2) / 101.62nm, ITO layer 3-7 / 5nm; silicon aluminum composite oxide layer 3-8 / 73nm (material is the same as 3-1); waterproof layer 4 (using C 12 F 27 N waterproof material / 10nm);
[0128] Its preparation process and method are the same as those of Comparative Example 2.
[0129] Comparative Example 4
[0130] A clear bottom color infrared-proof resin lens, which comprises, in order: a resin lens substrate 1 (MR-8-UV405); a hardening layer 2 (Z117) / 2.6-3 μm; an anti-reflection layer comprising: a SiO2 layer 3-1 / 26.6 nm, a TiO2 layer 3-2 / 13.35 nm, a SiO2 layer 3-3 / 34.8 nm, a TiO2 layer 3-4 / 113.81 nm, a SiO2 layer 3-5 / 161.65 nm, a TiO2 layer 3-6 / 101.11 nm, an ITO layer 3-7 / 5 nm; a SiO2 layer 3-8 / 73.6 nm; a waterproof layer 4 (using a C-containing 12 F 27 N waterproof material / 10nm); its preparation method comprises the following steps:
[0131] S1: Making a hard layer: immerse the resin lens substrate cleaned by ultrasonic wave into a 27% by weight hardening liquid aqueous solution of model Z117 at a dipping temperature of 15°C, and pull out the solution at a speed of 2.0 mm / s after dipping for 5 seconds; after drying at 80°C for 3 hours, take out the substrate and send it to a drying oven for drying and curing at a curing temperature of 120°C for 150 minutes, thereby obtaining a resin lens with a hardening layer;
[0132] S2: preparing a clear background color infrared-proof film layer: in a vacuum coating machine, using a vacuum coating process, evaporating the solid film material and then transmitting it through the gas phase, and depositing it into a thin film on the surface of the resin lens obtained in step S1 to form a clear background color infrared-proof film layer, specifically comprising the following steps:
[0133] S21: comprising the following steps:
[0134] S211: The surface of the resin lens obtained in S1 has a background vacuum of ≤3×10 -3 Pa, and the temperature in the coating chamber is 60℃, with ion source assisted process, high energy electron beam is used to heat SiO2 at a rate of The evaporated SiO2 is deposited in the form of nano-scale molecules to obtain a resin lens containing a first SiO2 layer;
[0135] S212: The surface of the resin lens obtained in S211 has a background vacuum of ≤3×10 -3 Pa, the temperature in the coating chamber is 60℃, and there is an ion source assisted process. High-energy electron beam is used to heat TiO2 at a rate of The evaporated TiO2 is deposited in the form of nano-scale molecules to obtain a resin lens containing a second TiO2 layer;
[0136] S213: repeating steps S211 and S212 to alternately form a third SiO2 layer, a fourth TiO2 layer, a fifth SiO2 layer, and a sixth TiO2 layer, respectively, to form a resin lens including a third SiO2 layer, a fourth TiO2 layer, a fifth SiO2 layer, and a sixth TiO2 layer;
[0137] S22: The surface of the resin lens obtained in S21 has a background vacuum of ≤3×10 -3 Pa, and the temperature in the coating chamber is 60℃, and under the conditions of ion source auxiliary process, high-energy electron beam is used to heat ITO at a rate of Depositing the evaporated ITO in the form of nano-scale molecules to obtain a resin lens containing a seventh ITO layer;
[0138] S23: continuing to use the vacuum coating process on the surface of the resin lens obtained in S22, repeating the process steps of S211, and then forming a resin lens containing an eighth SiO2 layer;
[0139] S3: preparing a waterproof layer: forming a waterproof layer on the surface of the resin lens obtained in S23: continuing to use the vacuum coating process on the surface of the lens obtained in step S2, with a background vacuum degree of ≤3×10 -3 Pa, and the temperature in the coating chamber is 60℃, a high-energy electron beam is used to heat the material at a rate of The evaporated C 12 F 27 The waterproof material of N is deposited on the surface of the resin lens obtained in S24 in the form of nano-scale molecules.
[0140] Comparative Example 5
[0141] A clear base color infrared-proof resin lens, which comprises, in order: a resin lens substrate 1 (MR-8-UV405); a hardened layer 2 (Z117) / 2.6-3μm; a clear base color infrared-proof film layer 3 comprising: a silicon-aluminum composite oxide layer 3-1 (wherein the molar percentage of SiO2 and Al2O3 is: 92% SiO2: 8% Al2O3; commissioned by Changzhou Zhanchi Optoelectronics Technology Co., Ltd. to develop and produce, the material model is SA56) / 26nm, a titanium-niobium composite oxide layer 3-2 (wherein the molar percentage of TiO2 and Nb2O5 is: 80% TiO2: 20% Nb2O5; commissioned by Changzhou Zhanchi Optoelectronics Technology Co., Ltd. to develop and produce, the material model is PTN28) / 12.48nm, SiO-Cr absorption layer 3-3 (SiO:Cr molar ratio is 1:1, sintered by Danyang Keda Coating Material Co., Ltd.) / 1.2nm, silicon dioxide layer 3-4 / 34.5nm (molecular formula SiO2, purity 99.99%, sintered by Danyang Keda Coating Material Co., Ltd.), titanium niobium composite oxide layer 3-5 (material is the same as 3-2) / 114.5nm, silicon aluminum composite oxide layer 3-6 / 160.4nm (material is the same as 3-1); titanium niobium composite oxide layer 3-7 (material is the same as 3-2) / 101.6nm; ITO layer 3-8 / 5nm; silicon aluminum composite oxide layer 3-9 / 71.0nm (material is the same as 3-1); waterproof layer 4 (using C-containing 12 F 27 N waterproof material / 10nm);
[0142] The preparation method thereof is the same as that of Example 1 except for the 3-3 SiO-Cr absorption layer.
[0143] The preparation process of the SiO-Cr absorption layer is as follows: a SiO-Cr layer is formed on the surface of the resin lens obtained in step S22. First, vacuum is drawn to a background vacuum degree of ≤1.2×10-4 Pa. Then, SiO-Cr is deposited in an ion source Hall source assisted process, using a high energy electron beam to heat the SiO-Cr at a rate of The evaporated SiO-Cr is deposited in the form of nano-scale molecules to obtain a resin lens containing a SiO-Cr layer. The auxiliary parameters of the ion source here are: anode voltage: 110V, anode current: 3A, and Ar flow rate of 12sccm.
[0144] Comparative Example 6
[0145] A clear base color infrared-proof resin lens, which comprises, in order: a resin lens substrate 1 (MR-8-UV405); a hardened layer 2 (Z117) / 2.6-3μm; a clear base color infrared-proof film layer 3 comprising: a silicon-aluminum composite oxide layer 3-1 (wherein the molar percentage of SiO2 and Al2O3 is: 92% SiO2: 8% Al2O3; commissioned by Changzhou Zhanchi Optoelectronics Technology Co., Ltd. to develop and produce, the material model is SA56) / 26nm, a titanium-niobium composite oxide layer 3-2 (wherein the molar percentage of TiO2 and Nb2O5 is: 80% TiO2: 20% Nb2O5; commissioned by Changzhou Zhanchi Optoelectronics Technology Co., Ltd. to develop and produce, the material model is PTN28) / 12.48nm, titanium nitride layer 3-3 (molecular formula TiN, purity above 99.9%, sintered by Changzhou Zhanchi Optoelectronics Technology Co., Ltd.) / 1.0nm, silicon dioxide layer 3-4 / 34.5nm (molecular formula SiO2, purity 99.99%, sintered by Danyang Keda Coating Materials Co., Ltd.), titanium niobium composite oxide layer 3-5 (material is the same as 3-2) / 114.5nm, silicon aluminum composite oxide layer 3-6 / 160.4nm (material is the same as 3-1); titanium niobium composite oxide layer 3-7 (material is the same as 3-2) / 101.6nm; ITO layer 3-8 / 5nm; silicon aluminum composite oxide layer 3-9 / 71.0nm (material is the same as 3-1); waterproof layer 4 (using C-containing 12 F 27 N waterproof material / 10nm);
[0146] The preparation method thereof is the same as that of Example 1 except for the 3-3 layers of titanium nitride.
[0147] The preparation process of titanium nitride is as follows: a titanium nitride layer is formed on the surface of the resin lens obtained in step S22. First, vacuum is drawn to a background vacuum degree of ≤8×10 -4 Pa. Then bombard with ion source Hall source for 60 seconds, the ion source bombardment parameters are: anode voltage: 110V, anode current: 3A, auxiliary gas is Ar, flow rate is 10sccm. Then deposit under ion source Hall source assisted process, use high energy electron beam to heat TiN, at a rate The evaporated TiN is deposited in the form of nano-scale molecules to obtain a resin lens containing a TiN layer. The ion source auxiliary parameters here are: anode voltage: 110V, anode current: 3A, Ar flow rate is 12sccm, and there is no nitrogen flow rate. After obtaining a resin lens containing a TiN layer, the TiN surface is bombarded with an ion source for 30 seconds, and its ion source parameters are the same as the ion source auxiliary parameters of this layer.
[0148] Comparative Example 7
[0149] A clear base color infrared-proof resin lens, which comprises, in order: a resin lens substrate 1 (MR-8-UV405); a hardened layer 2 (Z117) / 2.6-3μm; a clear base color infrared-proof film layer 3 comprising: a silicon-aluminum composite oxide layer 3-1 (wherein the molar percentage of SiO2 and Al2O3 is: 92% SiO2: 8% Al2O3; commissioned by Changzhou Zhanchi Optoelectronics Technology Co., Ltd. to develop and produce, the material model is SA56) / 26nm, a titanium-niobium composite oxide layer 3-2 (wherein the molar percentage of TiO2 and Nb2O5 is: 80% TiO2: 20% Nb2O5; commissioned by Changzhou Zhanchi Optoelectronics Technology Co., Ltd. to develop and produce, the material model is PTN28) / 12.48nm, titanium nitride layer 3-3 (molecular formula TiN, purity above 99.9%, sintered by Changzhou Zhanchi Optoelectronics Technology Co., Ltd.) / 1.0nm, silicon dioxide layer 3-4 / 34.5nm (molecular formula SiO2, purity 99.99%, sintered by Danyang Keda Coating Materials Co., Ltd.), titanium niobium composite oxide layer 3-5 (material is the same as 3-2) / 114.5nm, silicon aluminum composite oxide layer 3-6 / 160.4nm (material is the same as 3-1); titanium niobium composite oxide layer 3-7 (material is the same as 3-2) / 101.6nm; ITO layer 3-8 / 5nm; silicon aluminum composite oxide layer 3-9 / 71.0nm (material is the same as 3-1); waterproof layer 4 (using C-containing 12 F 27 N waterproof material / 10nm);
[0150] The preparation method is the same as that of Example 1 except for the 3-3 layer of titanium nitride. The preparation process of titanium nitride is as follows: S23: forming a titanium nitride layer on the surface of the resin lens obtained in step S22. First, evacuate to a background vacuum degree of ≤8×10 - 4 Pa. No ion source Hall source pre-bombardment. Directly deposited under the ion source Hall source assisted process, using high energy electron beam to heat TiN at a rate The evaporated TiN is deposited in the form of nano-scale molecules to obtain a resin lens containing a TiN layer. Here, the ion source auxiliary parameters are: anode voltage: 110V, anode current: 3A, Ar flow rate: 10sccm, nitrogen flow rate: 5sccm. After obtaining a resin lens containing a TiN layer, continue to bombard the TiN surface with an ion source for 30 seconds. The ion source parameters are the same as the ion source auxiliary parameters of this layer.
[0151] Comparative Example 8
[0152] A clear base color infrared-proof resin lens, which comprises, in order: a resin lens substrate 1 (MR-8-UV405); a hardened layer 2 (Z117) / 2.6-3μm; a clear base color infrared-proof film layer 3 comprising: a silicon-aluminum composite oxide layer 3-1 (wherein the molar percentage of SiO2 and Al2O3 is: 92% SiO2: 8% Al2O3; commissioned by Changzhou Zhanchi Optoelectronics Technology Co., Ltd. to develop and produce, the material model is SA56) / 26nm, a titanium-niobium composite oxide layer 3-2 (wherein the molar percentage of TiO2 and Nb2O5 is: 80% TiO2: 20% Nb2O5; commissioned by Changzhou Zhanchi Optoelectronics Technology Co., Ltd. to develop and produce, the material model is PTN28) / 12.48nm, titanium nitride layer 3-3 (molecular formula TiN, purity above 99.9%, sintered by Changzhou Zhanchi Optoelectronics Technology Co., Ltd.) / 1.0nm, silicon dioxide layer 3-4 / 34.5nm (molecular formula SiO2, purity 99.99%, sintered by Danyang Keda Coating Materials Co., Ltd.), titanium niobium composite oxide layer 3-5 (material is the same as 3-2) / 114.5nm, silicon aluminum composite oxide layer 3-6 / 160.4nm (material is the same as 3-1); titanium niobium composite oxide layer 3-7 (material is the same as 3-2) / 101.6nm; ITO layer 3-8 / 5nm; silicon aluminum composite oxide layer 3-9 / 71.0nm (material is the same as 3-1); waterproof layer 4 (using C-containing 12 F 27 N waterproof material / 10nm);
[0153] The preparation method thereof is the same as that of Example 1 except for the 3-3 layers of titanium nitride.
[0154] The preparation process of titanium nitride is as follows: S23: forming a titanium nitride layer on the surface of the resin lens obtained in step S22. First, evacuate to a background vacuum degree of ≤3×10 -3 Pa (vacuum is not specifically controlled). Then bombard with ion source Hall source for 60 seconds. The ion source bombardment parameters are: anode voltage: 110V, anode current: 3A, auxiliary gas is Ar, and the flow rate is 10sccm. Then deposit under ion source Hall source assisted process, use high energy electron beam to heat TiN, and the rate is The evaporated TiN is deposited in the form of nano-scale molecules to obtain a resin lens containing a TiN layer. Here, the ion source auxiliary parameters are: anode voltage: 110V, anode current: 3A, Ar flow rate: 10sccm, nitrogen flow rate: 5sccm. After obtaining a resin lens containing a TiN layer, the TiN surface is bombarded with an ion source for 30 seconds, and its ion source parameters are the same as the ion source auxiliary parameters of this layer.
[0155] 2. Experimental Examples
[0156] The list of materials for the main embodiments and comparative examples is as follows: the one containing TiN or SiO-Cr is a 9-layer anti-infrared film structure, and the one not containing TiN or SiO-Cr is an 8-layer anti-infrared film system.
[0157] Table 1. Comparison of materials in Examples and Comparative Examples
[0158]
[0159] 1. Determine the average reflectivity, transmittance, yellow index and infrared protection effect of the lens
[0160] 1.1 Determination of the average reflectivity, transmittance and infrared protection effect of Examples 1 to 4 and Comparative Examples 1 to 8
[0161] For the lenses prepared in Examples 1 to 4 and Comparative Examples 1 to 8, the average reflectivity (average reflectivity: refers to the visual average reflectivity under C light (a light source with a color temperature of 6774K defined in CIE) illumination, here refers to the reflectivity of a single side), the average transmittance (average transmittance: refers to the visual average transmittance under C light (a light source with a color temperature of 6774K defined in CIE) illumination, here refers to the transmittance of the same film system coated on both sides), the yellow index (refers to the yellow index of the lens calculated with reference to QB-T-2506-2001 after coating on both sides) and the near-infrared transmittance (near-infrared average transmittance: here refers to the near-infrared cutoff rate of the lens calculated with reference to QB-T-2506-2017 after coating on both sides) were measured, and the measurement results are recorded in Table 2 below:
[0162] Table 2. Comparison of reflectivity, infrared rejection and yellowness index
[0163] Film color Contains TiN Single-sided visible light reflectivity Average visible light transmittance Near infrared average blocking rate Yellow Index Example 1 green yes 1.23% 90.5% 59.3% 3.6% Example 2 green yes 1.21% 90.8% 58.9% 3.7% Example 3 green yes 1.29% 90.2% 59.4% 3.8% Example 4 green yes 1.26% 91.8% 58.5% 4.1% Comparative Example 1 green no 1.26% 95.1% 38.4% 5.2% Comparative Example 2 blue no 0.73% 95.7% 52.1% 13.4% Comparative Example 3 green no 1.21% 95.3% 56.4% 4.8% Comparative Example 4 green no 1.20% 95.4% 56.9% 5.0% Comparative Example 5 green no 1.27% 92.9% 57.1% 5.4% Comparative Example 6 green yes 1.26% 93.1% 57.4% 5.4% Comparative Example 7 green yes 1.29% 89.2% 59.5% 5.0% Comparative Example 8 green yes 1.25% 92.6% 57.9% 5.1%
[0164] From Comparative Examples 2 and 3, it can be seen that the infrared blocking rate of the green film is higher and the yellow index is lower. The TiN layer with a special process is used, and the infrared blocking rate is further improved and the yellow index is further reduced. The visual effect of the lens is clearer.
[0165] 1.2 Determining the blue light protection effect of lenses
[0166] Refer to the national standard GB / T38120-2019 to check whether the lenses meet the standards.
[0167] Table 3. Comparison of blue light protection index and yellow index
[0168]
[0169]
[0170] 1.3 Comparison of the impact of TiN process on anti-blue light standards and yellow index
[0171] Test the transmission and reflection of a single surface and calculate the absorption results as follows:
[0172] Table 4. Effect of TiN process on anti-blue light index and yellow index
[0173]
[0174] The general process uses SiO-Cr as the absorption layer, which can effectively meet the needs of blue light protection. However, its yellow-green light absorption is low, which will lead to an increase in the yellow index. Most weak absorption materials have this characteristic.
[0175] Strictly controlling the preparation process of the TiN film layer helps to achieve the expected technical effect of the film layer.
[0176] (1) When TiN is not strictly controlled in vacuum, it tends to oxidize, thereby reducing the absorption of the film layer, and the absorption of yellow-green light and infrared light decreases faster, resulting in an increase in the yellow index, and the lens appears yellow and unclear; (2) When TiN is not assisted by an ion source, the film layer is loose and the nitrogen content is reduced during the evaporation process. It will be oxidized when other layers are plated. As a result, there is a tendency to oxidize, thereby reducing the absorption of the film layer, and the absorption of yellow-green light and infrared light decreases faster, resulting in an increase in the yellow index, and the lens appears yellow and unclear; (3) When TiN is assisted by an ion source but not assisted by nitrogen, it will lead to metallization of the film layer (insufficient nitridation) and a sharp increase in absorption. The absorption of blue light increases much faster than that of yellow-green light and infrared, resulting in an increase in the yellow index, and the lens appears yellow and gray and unclear. The specific process of the present invention is used to prepare the TiN layer, which can effectively increase the blocking absorption of near-infrared, control the absorption of blue light, and increase the absorption of yellow light, thereby reducing the yellow index and making the lens clearer and more beautiful.
[0177] 2. High temperature resistance, durability and high temperature adhesion test
[0178] 2.1 Temperature resistance test:
[0179] After the samples (Examples 1 to 4 and Comparative Examples 1 to 8) were completed, the heat resistance of the samples was tested after being stored for one week. The test method for heat resistance is based on Article 5.8 of the National Heat Resistance Standard for Resin Lenses (GB 10810.4-2012): pass the baking test at 55°C for 30 minutes. After passing the test, the same method is used to increase the baking time by 5°C for 30 minutes each time until the lens shows failure phenomena such as film cracking or orange peel, and the highest qualified temperature is recorded. The results are recorded in Table 5 below.
[0180] 2.2 High temperature adhesion test:
[0181] Adhesion test refers to the film adhesion test in accordance with Article 5.9 of GB10810.4-2012. High temperature film adhesion test refers to the test conducted by Wanxin Company in accordance with Article 5.9 of GB10810.4-2012, with the boiling conditions changed to 90±2℃ for 60 minutes. Other test methods are the same. Adhesion and high temperature adhesion test results: Grade A refers to no film removal or the film removal area is less than 5%, Grade B refers to the film removal area between 5% and 15%, and Grade C (unqualified) refers to the film removal area significantly greater than 15%. In order to verify the product adhesion distribution, high temperature adhesion tests were performed at 5 different locations in the coating room.
[0182] The test results of Examples 1 to 4 and Comparative Examples 1 to 8 are recorded in Table 5 below.
[0183] 2.3 High temperature and high humidity test
[0184] The photovoltaic industry and the optical communication industry use high temperature and high humidity to evaluate the durability of products. Referring to the test standards of the photovoltaic industry (GB / T 18911-2002, IEC61646:1996, Article 10.13) and the test methods of the optical communication industry (Ballcore Test, GR-1221-Core, Article 6.2.5), the high temperature and high humidity test and debugging of the resin lens is defined as: storage at 85°C and 85% humidity for 12 hours, and checking whether the prepared lens has obvious failure phenomena such as film cracks or orange peel; each high temperature and high humidity test is performed with 3 resin lenses placed in different positions. The test results of Examples 1 to 4 and Comparative Examples 1 to 8 are recorded in Table 5 below.
[0185] Table 5 High temperature resistance, durability and high temperature adhesion test results
[0186]
[0187]
[0188] It can be seen that, under the condition that other conditions remain unchanged, the high-refractive index material of the lens made of titanium-niobium composite oxide has better high-temperature resistance, high-temperature adhesion and durability than other conventional materials; the low-refractive index material made of silicon-aluminum composite oxide has better high-temperature resistance, high-temperature adhesion and durability than other conventional materials; we use these two specific ratios of materials to prepare the film system and its appropriate process to ensure the high-temperature resistance and durability of the clear base color anti-infrared products.
Claims
1. A clear background color, blue light proof, infrared proof, and high temperature resistant resin lens, characterized in that: include: A resin lens substrate, a hardened layer and a clear bottom color infrared-proof film layer; wherein the resin lens substrate, the hardened layer and the clear bottom color infrared-proof film layer are arranged in sequence, the hardened layer is located on the surface of the resin lens substrate, and the clear bottom color infrared-proof film layer is located on the surface of the hardened layer; the clear bottom color infrared-proof and high temperature-resistant resin lens also includes a waterproof layer, and the waterproof layer is located on the surface of the clear bottom color infrared-proof film layer; The clear background color infrared-proof film layer comprises three silicon-aluminum composite oxide layers, three titanium-niobium composite oxide layers, a titanium nitride layer, a silicon dioxide layer and a tin-doped indium oxide layer, namely, an ITO layer. In the clear background color infrared-proof film layer, the layers are: (1) silicon-aluminum composite oxide layer, (2) titanium-niobium composite oxide layer, (3) titanium nitride layer, (4) silicon dioxide layer, (5) titanium-niobium composite oxide layer, (6) silicon-aluminum composite oxide layer, (7) titanium-niobium composite oxide layer, (8) tin-doped indium oxide layer, namely, an ITO layer, and (9) silicon-aluminum composite oxide layer; and the first silicon-aluminum composite oxide layer is located on the surface of the hardened layer; The preparation method of the clear base color blue light proof infrared proof high temperature resistant resin lens comprises the following steps: S1: preparing a hard layer: forming a hard layer on the surface of a resin lens substrate, i.e. obtaining a resin lens containing a hard layer; the step of preparing the hard layer comprises: immersing the resin lens substrate cleaned by ultrasonic wave into a hardening liquid aqueous solution with a mass percentage of 25-30%, the immersion temperature being 10-20°C, and pulling out the solution at a speed of 1.0-3.0 mm / s after immersion for 4-8 seconds, and then drying it at 70-90°C for 2-5 hours, then taking out the substrate and sending it to a drying oven for drying and curing, the curing temperature being 100-150°C, and the curing time being 120-180min, to obtain a resin lens containing a hard layer; S2: preparing a clear background color infrared-proof film layer: forming the clear background color infrared-proof film layer on the surface of the resin lens obtained in S1, that is, obtaining a resin lens containing a clear background color infrared-proof film layer, specifically comprising: in a vacuum coating machine, using a vacuum coating process, evaporating a silicon-aluminum composite oxide layer, a titanium-niobium composite oxide, titanium nitride, silicon dioxide and an ITO solid film layer material, and then transmitting the evaporated film through the gas phase, and depositing the evaporated film on the surface of the resin lens obtained in step S1 to form a clear background color infrared-proof film layer, specifically comprising the following steps: S21: forming a first layer of silicon-aluminum composite oxide layer on the surface of the resin lens obtained in step S1, and the background vacuum degree is ≤3×10 -3 Pa, the temperature in the coating chamber is 50-70°C, and an ion source-assisted process is used, a high-energy electron beam is used to heat the silicon-aluminum composite oxide, and the evaporated silicon-aluminum composite oxide is deposited in the form of nano-scale molecules at a rate of 5-7Å / S to obtain a resin lens containing a first silicon-aluminum composite oxide layer; S22: forming a titanium-niobium composite oxide layer on the surface of the resin lens obtained in step S21; the surface of the resin lens obtained in step S21 has a background vacuum degree of ≤3×10 -3 Pa, and the temperature in the coating chamber is 50-70° C., and an ion source-assisted process is provided, using a high-energy electron beam to heat the titanium-niobium composite oxide, and depositing the evaporated titanium-niobium composite oxide in the form of nano-scale molecules at a rate of 2-4Å / S to obtain a resin lens containing a second titanium-niobium composite oxide layer; S23: forming a titanium nitride layer on the surface of the resin lens obtained in step S22, specifically comprising: S231: First evacuate to the background vacuum degree ≤8×10 -4 Pa, and then bombarded with an ion source Hall source for 50-80 seconds. The ion source bombardment parameters are: anode voltage: 90-140 V, anode current: 2.5-5 A, auxiliary gas is Ar, and the flow rate is 5-20 sccm; S232: Deposition under ion source assisted process, using high energy electron beam to heat TiN, and depositing evaporated TiN in the form of nano-scale molecules at a rate of 0.8~1.5Å / S. The ion source assisted parameters are: anode voltage: 90~140V, anode current: 2.5~5A, auxiliary gas is Ar and N2, Ar flow rate is 5~15sccm, N2 flow rate is: 3~15sccm; S233: continue to bombard the TiN film surface with the ion source Hall source for 20 to 40 seconds, the bombardment parameters are: anode voltage: 90 to 140 V, anode current: 2.5 to 5 A, auxiliary gas is Ar and N2, Ar flow rate is 5 to 15 sccm, N2 flow rate is: 3 to 15 sccm; S24: The surface of the resin lens obtained in S23 has a background vacuum of ≤3×10 -3 Pa, and the temperature in the coating chamber is 50~70℃, and under the conditions of ion source auxiliary process, high-energy electron beam is used to heat SiO2, and the evaporated SiO2 is deposited in the form of nano-scale molecules at a rate of 5~20Å / S to obtain a resin lens containing a SiO2 layer; S25: repeating step S22 to form a titanium-niobium composite oxide layer on the surface of the resin lens obtained in step S24; S26: repeat step S21 to form a silicon-aluminum composite oxide layer on the surface of the resin lens obtained in step S25; S27: repeat step S22 to form a titanium-niobium composite oxide layer on the surface of the resin lens obtained in step S26; S28: The surface of the resin lens obtained in S27 has a background vacuum of ≤3×10 -3 Under the conditions of 1000 Pa, 50-70°C temperature in the coating chamber and ion source assisted process, a high-energy electron beam is used to heat ITO, and the evaporated ITO is deposited in the form of nano-scale molecules at a rate of 1-3Å / S to obtain a resin lens containing an ITO layer; S29: continuing to use the vacuum coating process on the surface of the resin lens obtained in S28, repeating the process steps of S21, and then forming a layer of resin lens containing a silicon-aluminum composite oxide layer; S3: preparing a waterproof layer: forming a waterproof layer on the surface of the resin lens obtained in step S2, including the following steps: continuing to use a vacuum coating process on the surface of the lens obtained in step S29, with a background vacuum degree of ≤3×10 -3 Under the conditions of Pa and the temperature in the coating chamber being 50~70℃, a high-energy electron beam is used to heat the material, and the evaporated fluorine-containing waterproof material is deposited in the form of nano-scale molecules at a rate of 5~8Å / S to obtain a resin lens with a waterproof layer.
2. The clear base color blue light proof infrared proof high temperature resistant resin lens according to claim 1, characterized in that: The material of the hardening layer is silicone.
3. The clear base color blue light proof infrared proof high temperature resistant resin lens according to claim 2, characterized in that: The organic silicon contains at least Ti element.
4. The clear base color, blue light proof, infrared proof and high temperature resistant resin lens according to any one of claims 1 to 3, characterized in that: The silicon-aluminum composite oxide layer is composed of a composite material of SiO2 and Al2O3, wherein the molar fraction of SiO2 in the composite material is 70% to 95%.
5. The clear base color, blue light proof, infrared proof and high temperature resistant resin lens according to claim 4, characterized in that: The silicon-aluminum composite oxide layer is composed of a composite material of SiO2 and Al2O3, wherein SiO2 accounts for 92% of the molar fraction of the composite material.
6. The clear base color, blue light proof, infrared proof and high temperature resistant resin lens according to any one of claims 1 to 3, characterized in that: The titanium-niobium composite oxide layer is composed of a composite material of TiO2 and Nb2O5, wherein TiO2 accounts for 10% to 90% of the molar fraction of the composite material.
7. The clear base color, blue light proof, infrared proof and high temperature resistant resin lens according to claim 6, characterized in that: The titanium-niobium composite oxide layer is composed of a composite material of TiO2 and Nb2O5, wherein TiO2 accounts for 80% of the molar fraction of the composite material.
8. The clear base color, blue light proof, infrared proof and high temperature resistant resin lens according to any one of claims 1 to 3, characterized in that: The purity of TiN in the titanium nitride layer is greater than 99.9 wt %.
9. The clear base color, blue light proof, infrared proof and high temperature resistant resin lens according to claim 2 or 3, characterized in that:The thickness of the hardened layer is 1 to 5 μ m.
10. The clear base color, blue light proof, infrared proof and high temperature resistant resin lens according to claim 1, characterized in that: The thickness of the clear base color anti-infrared film layer is 290-950nm.
11. The clear base color, blue light proof, infrared proof and high temperature resistant resin lens according to claim 1, characterized in that: The thickness of the waterproof layer is 4-20 nm.
12. The clear-bottom-color, blue-light-proof, infrared-proof, and high-temperature-resistant resin lens according to any one of claims 1 to 3, 5, 7, and 10 to 11, characterized in that: The average reflectivity of the clear-base-color blue-light-proof, infrared-proof, and high-temperature-resistant resin lens is ≤1.5%.
13. According to any one of claims 1 to 3, 5, 7, 10 to 11, the clear-bottom-color, blue-light-proof, infrared-proof and high-temperature-resistant resin lens has a near-infrared blocking rate of >55%.
14. The clear-base-color, blue-light-proof, infrared-proof, and high-temperature-resistant resin lens according to any one of claims 1 to 3, 5, 7, and 10 to 11, wherein the yellow index of the clear-base-color, blue-light-proof, infrared-proof, and high-temperature-resistant resin lens is ≤4.5%.
15. A method for preparing the clear base color blue light proof infrared proof high temperature resistant resin lens according to any one of claims 1 to 14, characterized in that: The following steps are involved: S1: preparing a hard layer: forming a hard layer on the surface of a resin lens substrate, i.e. obtaining a resin lens containing a hard layer; S2 preparing a clear base color anti-infrared film layer: forming the clear base color anti-infrared film layer on the surface of the resin lens obtained in S1, that is, obtaining a resin lens containing a clear base color anti-infrared film layer, specifically comprising: S21: forming a resin lens having a first silicon-aluminum composite oxide layer and a second titanium-niobium composite oxide layer on the surface of the resin lens obtained in step S1; S22: forming a third layer of a resin lens containing a titanium nitride layer on the surface of the resin lens obtained in step S21; S23: forming a fourth SiO2 layer-containing resin lens on the surface of the resin lens obtained in step S22; S24: forming a fifth titanium-niobium composite oxide layer, a sixth silicon-aluminum composite oxide layer, and a seventh titanium-niobium composite oxide layer on the surface of the resin lens obtained in step S23; S25: forming an eighth ITO-containing resin lens on the surface of the resin lens obtained in step S24; S26: forming a ninth layer of a resin lens containing a silicon-aluminum composite oxide layer on the surface of the resin lens obtained in step S25; S3: preparing a waterproof layer: forming a waterproof layer on the surface of the resin lens obtained in step S2.
Citation Information
Patent Citations
Anti-blue light nanometer composite monomer material and anti-blue light optical resin prepared from same
CN103992422A
Blue ray radiation preventing and achromatism spectacle lens, and method of producing the same
CN101216611A
Low-reflection anti-infrared high-temperature-resistant resin lens and preparation method thereof
CN112415639A