A method for preparing battery-grade lithium iron phosphate from waste lithium iron phosphate powder
Through hydrochloric acid solution dissolution and evaporation concentration and dilution technology, combined with iron powder and lithium fluoride to remove impurities, the efficient recycling of lithium iron phosphate is achieved, solving the problems of high costs and complex processes in the existing technology, and improving recycling efficiency and product performance.
Patent Information
- Application Number
- CN202211327306.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-10-26
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2042-10-26
AI Technical Summary
The existing lithium iron phosphate battery recycling technology has problems of high cost, complex processes and high energy consumption. Especially in the low-energy-consuming one-step method, the method of directly recycling battery-grade lithium iron phosphate waste powder is missing, and pH is in common methods. The regulation requires a large amount of alkaline materials to produce wastewater, and the product performance is affected.
Hydrochloric acid solution is used to dissolve lithium iron phosphate waste powder, adjust the pH through two evaporation and concentration and then dilution, and remove copper and aluminum impurities through iron powder and lithium fluoride. Finally, battery-grade lithium iron phosphate is prepared by baking at normal pressure, without using alkaline reagents , reduce wastewater treatment and costs.
The lithium-ion-only direct recovery rate is >99.5%, reducing recycling costs, reducing wastewater treatment pressure, improving the high purity and performance of the product, and simplifying the recycling process.
Smart Images

Figure CN115626624B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of recycling waste lithium iron phosphate powder, and in particular to a method for preparing battery-grade lithium iron phosphate from waste lithium iron phosphate powder. Background Art
[0002] As new energy vehicles continue to gain attention and development, replacing traditional vehicles has become an inevitable trend. While new energy vehicles create green travel, they also bring corresponding problems. The life of lithium-ion power batteries, which are the "heart" of new energy vehicles, is only 5 years on average, resulting in an increase in the cumulative scrapping of electric vehicle power batteries. However, due to the complex structure of lithium-ion power batteries, the high cost of recycling, and the imperfect process, recycling and utilization has been in a downturn. Among them, lithium iron phosphate batteries have been widely used in recent years due to their low preparation cost and high safety performance. Its usage has a tendency to surpass the usage of ternary batteries, and the scrap volume of lithium iron phosphate has shown a trend of multiple growth in recent years. Therefore, the recycling of waste lithium iron phosphate batteries is imminent. At present, the industrial recycling method for waste lithium iron phosphate is to recover lithium carbonate from the positive electrode sheet by selective lithium extraction, and the phosphorus iron slag after selective lithium extraction is recovered by the iron phosphate method. A large amount of sulfuric acid needs to be added in the whole process, the wastewater treatment pressure is high, and the recycling cost is high. However, there is a serious lack of methods and technologies for directly recovering battery-grade lithium iron phosphate from lithium iron phosphate waste powder at room temperature and pressure with low energy consumption in one step.
[0003] In recent years, Japanese, Korean and Chinese companies have conducted a lot of research on waste lithium iron phosphate powder, but they mainly use the step-by-step recovery method to generate iron phosphate and lithium carbonate for recycling. Although this method can recover iron, phosphorus and lithium elements in waste lithium iron phosphate positive electrode materials at a high recovery rate, the recycling process is complicated and the comprehensive recovery rate of lithium ions is low.
[0004] In addition, some companies use acid leaching, pH adjustment, addition of surfactants and antioxidants to treat battery powder, and then add lithium source, phosphorus source and / or iron source, adjust the pH of the system, seal the high pressure insulation reaction, obtain lithium iron phosphate precursor, and then make lithium iron phosphate from the lithium iron phosphate precursor. Although this method has a simple process, low acid consumption, low energy consumption, and high recovery rates of lithium, iron, and phosphorus, there are two pH adjustment processes in this method, which requires a large amount of alkaline materials and produces a large amount of wastewater. In addition, hydrothermal synthesis of lithium iron phosphate requires high temperature and high pressure to react, with high equipment requirements, long production cycle, and great difficulty in industrialization. In addition, the reaction process has strict requirements on the reagents for adjusting the pH of the solution. Sodium hydroxide or ammonia-based adjusting reagents will make the sodium and ammonia nitrogen content in the generated lithium iron phosphate product too high, and the product cannot show good performance, and the lithium-containing adjusting reagents greatly increase the cost.
[0005] In view of this, the present invention is proposed. Summary of the invention
[0006] The object of the present invention is to provide a method for preparing battery-grade lithium iron phosphate from waste lithium iron phosphate powder, which can shorten the lithium iron phosphate recovery process while reducing the amount of reagents used and the amount of wastewater treated.
[0007] The present invention is achieved in that:
[0008] In a first aspect, the present invention provides a method for preparing battery-grade lithium iron phosphate from waste lithium iron phosphate powder, comprising:
[0009] Dissolution step: dissolving the waste lithium iron phosphate powder in a hydrochloric acid solution and then separating the solid and the liquid to obtain a lithium iron phosphate solution;
[0010] The impurity removal step: the lithium iron phosphate solution is concentrated and evaporated without adding alkali, and then diluted to adjust the pH, iron powder is added to remove copper impurities, and then lithium fluoride is added to remove aluminum impurities, and solid-liquid separation is performed to obtain a copper-aluminum removal solution; the copper-aluminum removal solution is concentrated and evaporated without adding alkali, and then diluted to adjust the pH, and insoluble matter is separated to obtain a calcium-magnesium removal solution;
[0011] Calcination step: drying the calcium and magnesium removal solution and then calcining it to obtain battery-grade lithium iron phosphate powder.
[0012] In an optional embodiment, the impurity removal step includes at least one of the following features (1) to (4):
[0013] Feature (1): The lithium iron phosphate solution is concentrated and evaporated to 10-25% of the initial volume of the lithium iron phosphate solution, and then diluted with water to the initial volume of the lithium iron phosphate solution;
[0014] Feature (2): The amount of the iron powder added is 1.2-2.0 times the amount of copper impurities in the lithium iron phosphate solution;
[0015] Feature (3): The amount of lithium fluoride added is 6-10 times the amount of aluminum element in the lithium iron phosphate solution;
[0016] Feature (4): After adding the lithium fluoride, react at 30-70°C for 1-3 hours.
[0017] In an optional embodiment, the copper-aluminum removal solution is concentrated and evaporated to 10-25% of the initial volume of the copper-aluminum removal solution, and then diluted with water to the initial volume of the copper-aluminum removal solution.
[0018] In an optional embodiment, the mass concentration of the hydrochloric acid solution is 15-40%.
[0019] In an optional embodiment, the dissolving step includes at least one of the following features (5) to (7):
[0020] Feature (5): The mass ratio of the lithium iron phosphate waste powder to the hydrochloric acid solution is 1:1.4-1:3.5.
[0021] Feature (6): The iron content in the lithium iron phosphate waste powder is 25-33%.
[0022] Feature (7): The reaction temperature in the dissolution step is 20-100°C and the reaction time is 1-4h.
[0023] In an optional embodiment, the calcination temperature is 500-850° C. and the calcination time is 1-7 hours.
[0024] In an optional embodiment, before drying the decalcified and magnesium-containing solution, the process further comprises evaporating and concentrating the decalcified and magnesium-containing solution to 1 / 20-1 / 12 of the initial volume of the decalcified and magnesium-containing solution;
[0025] Preferably, the drying is spray drying.
[0026] In an optional embodiment, a carbon source is added as an additive during the calcination process, and the amount of the carbon source added is 5-10% of the solid content of the lithium iron phosphate;
[0027] Preferably, the carbon source is carbon black.
[0028] In an optional embodiment, the method for preparing battery-grade lithium iron phosphate from waste lithium iron phosphate powder further includes a hydrochloric acid recovery step: condensing and recovering the steam generated when the lithium iron phosphate solution and the copper-aluminum removal solution are concentrated and evaporated.
[0029] In an optional embodiment, the recovery rate of the hydrochloric acid is greater than 96%.
[0030] The present invention has the following beneficial effects:
[0031] The method for preparing battery-grade lithium iron phosphate from waste lithium iron phosphate powder provided by the present invention adopts hydrochloric acid solution to dissolve the waste lithium iron phosphate powder, and through two evaporation concentration and dilution, not only can the pH be adjusted, but also the hydrochloric acid solution can be recovered, the recovery ratio exceeds 96%, the direct recovery rate of lithium is greater than 99.5%, the recovery cost is low, and the hydrochloric acid solution used for dissolving the waste lithium iron phosphate powder can be recycled; in the process of removing impurities and adjusting the pH of the solution, the present invention does not add any alkaline solution, and only adjusts the pH of the solution through concentration, evaporation and dilution in an operation mode, which reduces the wastewater treatment pressure while ensuring the high purity of the prepared lithium iron phosphate material, and the product performance is more superior; in addition, in the present application, copper impurities and aluminum impurities are removed by introducing iron powder and lithium fluoride, and excess fluorine can also remove calcium and magnesium in the second evaporation concentration and dilution process, and the entire impurity removal process does not introduce other impurity components, so that the lithium iron phosphate prepared by the present application has a low impurity content, a large first discharge capacity and a high first efficiency. The invention removes impurities from waste lithium iron powder, concentrates and dries the slurry, and then calcines the slurry at normal pressure to prepare battery-grade lithium iron phosphate, and the recycling process is short. BRIEF DESCRIPTION OF THE DRAWINGS
[0032] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the drawings required for use in the embodiments are briefly introduced below. It should be understood that the following drawings only show certain embodiments of the present invention and therefore should not be regarded as limiting the scope. For ordinary technicians in this field, other related drawings can be obtained based on these drawings without creative work.
[0033] Figure 1 A process flow chart of a method for preparing battery-grade lithium iron phosphate from waste lithium iron phosphate powder provided by the present invention;
[0034] Figure 2 This is an electron microscope image of the lithium iron phosphate prepared in Example 1 of the present invention. DETAILED DESCRIPTION
[0035] In order to make the purpose, technical scheme and advantages of the embodiments of the present invention clearer, the technical scheme in the embodiments of the present invention will be described clearly and completely below. If the specific conditions are not specified in the embodiments, they are carried out according to conventional conditions or conditions recommended by the manufacturer. If the manufacturer of the reagents or instruments used is not specified, they are all conventional products that can be purchased commercially.
[0036] See also Figure 1 The present invention provides a method for preparing battery-grade lithium iron phosphate from waste lithium iron phosphate powder, which comprises the following steps:
[0037] (1) Dissolution step
[0038] The lithium iron phosphate waste powder is dissolved in a hydrochloric acid solution and then the solid and liquid are separated to obtain a lithium iron phosphate solution.
[0039] In some embodiments, the mass concentration of the hydrochloric acid solution is 15-40%; the mass ratio of the lithium iron phosphate waste powder to the hydrochloric acid solution is 1:1.4-1:3.5; the iron content of the lithium iron phosphate waste powder is 25-33%, and the lithium content is 3-5%; the reaction temperature in the dissolving step is 20-100°C, and the reaction time is 1-4h. The solid-liquid separation in the present application can be performed by at least one of filtration, filter pressing, or centrifugation.
[0040] (2) Impurity removal step
[0041] The lithium iron phosphate solution is concentrated and evaporated without adding alkali, and then diluted to adjust the pH. In some embodiments, the lithium iron phosphate solution is concentrated and evaporated to 10-25% of the initial volume of the lithium iron phosphate solution, and then water is added to dilute it to the initial volume of the lithium iron phosphate solution, and then iron powder is added. The amount of iron powder added is 1.2-2.0 times the mass of copper impurities in the lithium iron phosphate solution to remove copper impurities;
[0042] Then, lithium fluoride is added, and the amount of lithium fluoride added is 6-10 times the amount of aluminum element in the lithium iron phosphate solution. The reaction is carried out at 30-70° C. for 1-3 hours to remove aluminum impurities, and a copper-aluminum removal solution is obtained by separation;
[0043] Since the pH values required for removing Al, Ca and Mg differ greatly, when lithium fluoride is added, only aluminum impurities in the lithium iron phosphate solution can be removed. Then, in the present application, the copper-aluminum removal solution is concentrated and evaporated without adding alkali and then diluted to adjust the pH. In some embodiments, the copper-aluminum removal solution is concentrated and evaporated to 10-25% of the initial volume of the copper-aluminum removal solution, and then water is added to dilute it to the initial volume of the copper-aluminum removal solution. During the concentration and dilution process, the pH can be adjusted, so that the insoluble matter is separated after a period of reaction to obtain a calcium-magnesium removal solution.
[0044] The impurity removal principle is as follows: in the present invention, the lithium iron phosphate solution is concentrated and evaporated, and the steam generated by evaporation can be condensed to recover part of the hydrochloric acid, and then diluted with water to adjust the pH value of the system, and only water dilution is used for adjustment, without adding any reagent for adjusting the pH of the solution, and the iron powder can react with the copper ions in the lithium iron phosphate solution to replace the copper (Fe+Cu 2+ →Cu↓+Fe 2+ ), thereby achieving the removal of copper impurities. In the present invention, by adding lithium fluoride, lithium fluoride can react with aluminum ions to generate lithium hexafluoroaluminate (6LiF+Al 3+ →Li3AlF6+3Li +), Li3AlF6 is insoluble in water and can be removed by filtration. In addition, since in some embodiments of the present application, the amount of lithium fluoride added is excessive, the excess lithium fluoride can also react with dilute hydrochloric acid to generate hydrofluoric acid (LiF+HCl→LiCl+HF), and hydrofluoric acid can react with calcium ions to generate calcium fluoride (2F + +Ca 2+ →CaF2↓), which is white crystal or white powder, insoluble in water, soluble in hydrochloric acid and hydrofluoric acid, and hydrofluoric acid can also react with magnesium ions to form magnesium fluoride (2F + +Mg 2+ →MgF2↓), magnesium fluoride is insoluble in water and slightly soluble in dilute acid, so this application can remove most of the calcium and part of the magnesium. However, after removing aluminum, HF exists in the reaction system. At this time, the system is acidic, and calcium fluoride and calcium fluoride are difficult to precipitate. Therefore, this application is concentrated and evaporated again, and the hydrochloric acid in the system is further recovered. During the dilution process, the pH of the system increases, and calcium fluoride and calcium fluoride are precipitated and removed.
[0045] The present application only uses hydrochloric acid to dissolve the waste lithium iron phosphate powder, and then adjusts the pH value of the solution through two evaporation concentration and dilution operations. The proportion of hydrochloric acid solution that can be recovered exceeds 96%, and the one-time direct recovery rate of lithium is >99.5%. The recovery cost is low, and the hydrochloric acid solution used to dissolve the waste lithium iron phosphate powder can be recycled. No alkaline solution is added during the process of removing impurities and adjusting the pH value of the solution, which reduces the pressure of wastewater treatment while ensuring the high purity of the prepared lithium iron phosphate material, and the product performance is more superior.
[0046] (3) Calcination step
[0047] The calcium and magnesium removal solution is evaporated and concentrated and then dried, and the dried product is roasted to obtain battery-grade lithium iron phosphate powder.
[0048] In some embodiments of the present application, evaporation concentration is performed to 1 / 20-1 / 12 of the initial volume of the calcium and magnesium removal solution. The subsequent drying can be hot air drying, oven drying or spray drying, preferably spray drying. After the drying is completed, roasting is performed. A carbon source is added as an additive during the roasting process. The amount of carbon source added is 5-10% of the solid content of lithium iron phosphate. The carbon source can be, for example, carbon black. The temperature during roasting is 500-850°C and the time is 1-7h.
[0049] (4) Hydrochloric acid recovery step
[0050] The steam generated when the lithium iron phosphate solution and the copper-aluminum removal solution are concentrated and evaporated is condensed and recovered, and the recovery rate of hydrochloric acid is greater than 96%. The recovery cost is low, and the hydrochloric acid solution used to dissolve the lithium iron phosphate waste powder can be recycled.
[0051] The features and performance of the present invention are further described in detail below in conjunction with the embodiments.
[0052] Example 1
[0053] This embodiment provides a method for preparing battery-grade lithium iron phosphate from waste lithium iron phosphate powder, comprising the following steps:
[0054] (1) Take 500 g of lithium iron phosphate waste powder (iron content 27%, lithium content 3.365%), add 1000 g of 25% hydrochloric acid solution, react at 50° C. for 3 h, and filter to obtain a lithium iron phosphate solution.
[0055] (2) The volume of the lithium iron phosphate solution in step (1) is evaporated until the residual volume is 20% of the initial volume of the lithium iron phosphate solution, the steam generated by evaporation can be recovered as hydrochloric acid after condensation, the residue after evaporation is diluted with water to the original volume, iron powder is added for reaction (the amount of iron powder added is 1.3 times the mass of copper impurities), and the copper removal solution is obtained after reaction at room temperature for 2 hours. Lithium fluoride (the amount of lithium fluoride added is 7 times the mass of aluminum element) is added to the copper removal solution, and the copper removal aluminum solution is filtered after reaction at 30° C. for 2 hours to obtain a copper removal aluminum solution, and the copper removal aluminum solution is evaporated again until the residual volume is 20% of the initial volume of the copper removal aluminum solution, the steam generated by evaporation can be recovered as hydrochloric acid after condensation, and the residue after evaporation is diluted with water to the original volume of the solution, and the insoluble matter is filtered to obtain a calcium and magnesium removal solution.
[0056] (3) The decalcified and magnesium-free solution in step (2) was evaporated and concentrated to a residual volume of 1 / 15 of the initial volume of the decalcified and magnesium-free solution, and then spray-dried, carbon black was added as a carbon source (the amount of carbon black added was 8% of the solid content of lithium iron phosphate), and calcined at 750° C. for 4 h to obtain 381 g of battery-grade lithium iron phosphate positive electrode material, wherein the lithium content was 4.41% (such as Figure 2 shown).
[0057] (4) The steam generated by the two evaporation and concentration processes is collected and recovered as hydrochloric acid after condensation. When the lithium iron phosphate solution is evaporated, about 800 g of a hydrochloric acid solution with a mass fraction of 27% is condensed, and when the copper-aluminum removal solution is evaporated, about 500 g of a hydrochloric acid solution with a mass fraction of 5% is condensed.
[0058] Among them, hydrochloric acid recovery rate = amount of hydrochloric acid recovered by condensation / amount of hydrochloric acid added = (800 × 27% + 500 × 5%) / (1000 × 25%) = 241 / 250 = 96.4%;
[0059] The recovery rate of lithium = the lithium content in the iron-lithium product / the lithium content in the raw material = (381×4.41%) / (500×3.365%)=16.8021 / 16.825=99.86%.
[0060] Example 2
[0061] The present invention discloses a method for preparing battery-grade lithium iron phosphate from waste lithium iron phosphate powder, which specifically comprises the following steps:
[0062] (1) Take 500 g of lithium iron phosphate waste powder (iron content 33%), add 800 g of 37% hydrochloric acid solution by mass, react at 70° C. for 3 h, and filter to obtain a lithium iron phosphate solution.
[0063] (2) The volume of the lithium iron phosphate solution in step (1) is evaporated to a residual volume of 15% of the initial volume of the lithium iron phosphate solution, the steam generated by evaporation can be recovered as hydrochloric acid after condensation, the residue after evaporation is diluted with water to the original volume, iron powder is added to react (the amount of iron powder added is 1.5 times the mass of copper impurities), and the reaction is carried out at room temperature for 3 hours to obtain a copper removal solution, lithium fluoride is added to the copper removal solution (the amount of lithium fluoride added is 8 times the mass of aluminum elements), the reaction is carried out at 50° C. for 2 hours, and then filtered to obtain a copper removal aluminum solution, and the copper removal aluminum solution is evaporated again to a residual volume of 15% of the initial volume of the copper removal aluminum solution, the steam generated by evaporation can be recovered as hydrochloric acid after condensation, the residue after evaporation is diluted with water to the original volume of the solution, and the insoluble matter is filtered to obtain a calcium and magnesium removal solution.
[0064] (3) The calcium-magnesium-removing solution in step (2) is evaporated and concentrated to a residual volume of 1 / 20 of the initial volume of the calcium-magnesium-removing solution, followed by spray drying and calcination to obtain a lithium iron phosphate positive electrode material, wherein the carbon source is carbon black, the amount of carbon black added is 8% of the solid content of the lithium iron phosphate, the calcination temperature is 650° C., and the calcination time is 6 h.
[0065] (4) The steam generated by the two evaporation and concentration steps is collected and condensed to be recovered as hydrochloric acid.
[0066] Example 3
[0067] The present invention discloses a method for preparing battery-grade lithium iron phosphate from waste lithium iron phosphate powder, which specifically comprises the following steps:
[0068] (1) Take 500 g of lithium iron phosphate waste powder (iron content 29%), add 850 g of 32% hydrochloric acid solution by mass, react at 95° C. for 3 h, and filter to obtain a lithium iron phosphate solution.
[0069] (2) The volume of the lithium iron phosphate solution in step (1) is evaporated until the residual volume is 25% of the initial volume of the lithium iron phosphate solution, the steam generated by evaporation can be recovered as hydrochloric acid after condensation, the residue after evaporation is diluted with water to the original volume, iron powder is added to react (the amount of iron powder added is 1.6 times the mass of copper impurities), and the copper removal solution is obtained after reacting at room temperature for 3 hours, lithium fluoride is added to the copper removal solution (the amount of lithium fluoride added is 10 times the mass of aluminum element), the copper removal solution is reacted at 70° C. for 2 hours, and then filtered to obtain a copper removal aluminum solution, and the copper removal aluminum solution is evaporated again until the residual volume is 25% of the initial volume of the copper removal aluminum solution, the steam generated by evaporation can be recovered as hydrochloric acid after condensation, the residue after evaporation is diluted with water to the original volume of the solution, and the insoluble matter is filtered to obtain a calcium and magnesium removal solution.
[0070] (3) The calcium-magnesium-removing solution in step (2) is evaporated and concentrated to a residual volume of 1 / 17 of the initial volume of the calcium-magnesium-removing solution, followed by spray drying and calcination to obtain a lithium iron phosphate positive electrode material, wherein the carbon source is carbon black, the amount of carbon black added is 8% of the solid content of the lithium iron phosphate, the calcination temperature is 800° C., and the calcination time is 3 h.
[0071] (4) The steam generated by the two evaporation and concentration steps is collected and condensed to be recovered as hydrochloric acid.
[0072] Example 4
[0073] The present invention discloses a method for preparing battery-grade lithium iron phosphate from waste lithium iron phosphate powder, which specifically comprises the following steps:
[0074] (1) Take 500 g of lithium iron phosphate waste powder (iron content 31%), add 880 g of 28% hydrochloric acid solution by mass, react at 74° C. for 3 h, and filter to obtain a lithium iron phosphate solution.
[0075] (2) The volume of the lithium iron phosphate solution in step (1) is evaporated until the residual volume is 20% of the initial volume of the lithium iron phosphate solution, the steam generated by evaporation can be recovered as hydrochloric acid after condensation, the residue after evaporation is diluted with water to the original volume, iron powder is added to react (the amount of iron powder added is 1.7 times the mass of copper impurities), and the copper removal solution is obtained after reacting at room temperature for 3 hours, lithium fluoride is added to the copper removal solution (the amount of lithium fluoride added is 9 times the mass of aluminum element), and the copper removal aluminum solution is filtered after reacting at 60° C. for 2 hours to obtain a copper removal aluminum solution, and the copper removal aluminum solution is evaporated again until the residual volume is 25% of the initial volume of the copper removal aluminum solution, the steam generated by evaporation can be recovered as hydrochloric acid after condensation, and the residue after evaporation is diluted with water to the original volume of the solution, and the insoluble matter is filtered to obtain a calcium and magnesium removal solution.
[0076] (3) The calcium-magnesium-removing solution in step (2) is evaporated and concentrated to a residual volume of 1 / 13 of the initial volume of the calcium-magnesium-removing solution, followed by spray drying and calcination to obtain a lithium iron phosphate positive electrode material, wherein the carbon source is carbon black, the amount of carbon black added is 10% of the solid content of the lithium iron phosphate, the calcination temperature is 783° C., and the calcination time is 4 h.
[0077] (4) The steam generated by the two evaporation and concentration steps is collected and condensed to be recovered as hydrochloric acid.
[0078] Example 5
[0079] The present invention discloses a method for preparing battery-grade lithium iron phosphate from waste lithium iron phosphate powder, which specifically comprises the following steps:
[0080] (1) Take 700 g of lithium iron phosphate waste powder (iron content 31%), add 1000 g of 31% hydrochloric acid solution by mass, react at 54° C. for 3 h, and filter to obtain a lithium iron phosphate solution.
[0081] (2) The volume of the lithium iron phosphate solution in step (1) is evaporated to a residual volume of 18% of the initial volume of the lithium iron phosphate solution, the steam generated by evaporation can be recovered as hydrochloric acid after condensation, the residue after evaporation is diluted with water to the original volume, iron powder is added to react (the amount of iron powder added is 1.5 times the mass of copper impurities), and the copper removal solution is obtained after reacting at room temperature for 3 hours, lithium fluoride is added to the copper removal solution (the amount of lithium fluoride added is 8 times the mass of aluminum element), and the copper removal aluminum solution is filtered after reacting at 70° C. for 2 hours to obtain a copper removal aluminum solution, and the copper removal aluminum solution is evaporated again to a residual volume of 25% of the initial volume of the copper removal aluminum solution, the steam generated by evaporation can be recovered as hydrochloric acid after condensation, and the residue after evaporation is diluted with water to the original volume of the solution, and the insoluble matter is filtered to obtain a calcium and magnesium removal solution.
[0082] (3) The calcium-magnesium-removing solution in step (2) is evaporated and concentrated to a residual volume of 1 / 12 of the initial volume of the calcium-magnesium-removing solution, followed by spray drying and calcination to obtain a lithium iron phosphate positive electrode material, wherein the carbon source is carbon black, the amount of carbon black added is 7% of the solid content of the lithium iron phosphate, the calcination temperature is 779° C., and the calcination time is 4.3 h.
[0083] (4) The steam generated by the two evaporation and concentration steps is collected and condensed to be recovered as hydrochloric acid.
[0084] Example 6
[0085] This embodiment is basically the same as Embodiment 1, except that the concentration multiples of evaporation and concentration of the lithium iron phosphate solution are different. In Embodiment 1, the volume of the lithium iron phosphate solution in step (1) is evaporated until the remaining volume is 20% of the initial volume of the lithium iron phosphate solution; while in this embodiment, the volume of the lithium iron phosphate solution in step (1) is evaporated until the remaining volume is 70% of the initial volume of the lithium iron phosphate solution.
[0086] Specifically, this embodiment provides a method for preparing battery-grade lithium iron phosphate from waste lithium iron phosphate powder, which specifically includes the following steps:
[0087] (1) Take 500 g of lithium iron phosphate waste powder (iron content 27%), add 1000 g of 25% hydrochloric acid solution by mass, react at 50° C. for 3 h, and filter to obtain a lithium iron phosphate solution.
[0088] (2) The volume of the lithium iron phosphate solution in step (1) is evaporated until the residual volume is 70% of the initial volume of the lithium iron phosphate solution, the steam generated by evaporation can be recovered as hydrochloric acid after condensation, the residue after evaporation is diluted with water to the original volume, iron powder is added to react (the amount of iron powder added is 1.3 times the mass of copper impurities), and the copper removal solution is obtained after reacting at room temperature for 2 hours, lithium fluoride is added to the copper removal solution (the amount of lithium fluoride added is 7 times the mass of aluminum element), the copper removal solution is reacted at 30° C. for 2 hours, and then filtered to obtain a copper removal aluminum solution, and the copper removal aluminum solution is evaporated again until the residual volume is 20% of the initial volume of the copper removal aluminum solution, the steam generated by evaporation can be recovered as hydrochloric acid after condensation, the residue after evaporation is diluted with water to the original volume of the solution, and the insoluble matter is filtered to obtain a calcium and magnesium removal solution.
[0089] (3) The calcium-magnesium-removing solution in step (2) is evaporated and concentrated to a residual volume of 1 / 15 of the initial volume of the calcium-magnesium-removing solution, followed by spray drying and calcination to obtain a lithium iron phosphate positive electrode material, wherein the carbon source is carbon black, the amount of carbon black added is 8% of the solid content of the lithium iron phosphate, the calcination temperature is 750° C., and the calcination time is 4 h.
[0090] (4) The steam generated by the two evaporation and concentration steps is collected and condensed to be recovered as hydrochloric acid.
[0091] Example 7
[0092] This embodiment is basically the same as embodiment 1, except that the amount of lithium fluoride added is different. In embodiment 1, the amount of lithium fluoride added is 7 times the amount of aluminum element substance, while in this embodiment, the amount of lithium fluoride added is 12 times the amount of aluminum element substance.
[0093] Specifically, this embodiment provides a method for preparing lithium iron phosphate from waste lithium iron phosphate powder, which specifically includes the following steps:
[0094] (1) Take 500 g of lithium iron phosphate waste powder (iron content 27%), add 1000 g of 25% hydrochloric acid solution by mass, react at 50° C. for 3 h, and filter to obtain a lithium iron phosphate solution.
[0095] (2) The volume of the lithium iron phosphate solution in step (1) is evaporated until the residual volume is 20% of the initial volume of the lithium iron phosphate solution, the steam generated by evaporation can be recovered as hydrochloric acid after condensation, the residue after evaporation is diluted with water to the original volume, iron powder is added to react (the amount of iron powder added is 1.3 times the mass of copper impurities), and the copper removal solution is obtained after reacting at room temperature for 2 hours, lithium fluoride is added to the copper removal solution (the amount of lithium fluoride added is 12 times the mass of aluminum element), the copper removal solution is reacted at 30° C. for 2 hours, and then filtered to obtain a copper removal aluminum solution, and the copper removal aluminum solution is evaporated again until the residual volume is 20% of the initial volume of the copper removal aluminum solution, the steam generated by evaporation can be recovered as hydrochloric acid after condensation, the residue after evaporation is diluted with water to the original volume of the solution, and the insoluble matter is filtered to obtain a calcium and magnesium removal solution.
[0096] (3) The calcium-magnesium-removing solution in step (2) is evaporated and concentrated to a residual volume of 1 / 15 of the initial volume of the calcium-magnesium-removing solution, followed by spray drying and calcination to obtain a lithium iron phosphate positive electrode material, wherein the carbon source is carbon black, the amount of carbon black added is 8% of the solid content of the lithium iron phosphate, the calcination temperature is 750° C., and the calcination time is 4 h.
[0097] (4) The steam generated by the two evaporation and concentration steps is collected and condensed to be recovered as hydrochloric acid.
[0098] Example 8
[0099] This embodiment is basically the same as embodiment 1, except that the amount of lithium fluoride added is different. In embodiment 1, the amount of lithium fluoride added is 7 times the amount of aluminum element substance, while in this embodiment, the amount of lithium fluoride added is 2 times the amount of aluminum element substance.
[0100] Specifically, this embodiment provides a method for preparing lithium iron phosphate from waste lithium iron phosphate powder, which specifically includes the following steps:
[0101] (1) Take 500 g of lithium iron phosphate waste powder (iron content 27%), add 1000 g of 25% hydrochloric acid solution by mass, react at 50° C. for 3 h, and filter to obtain a lithium iron phosphate solution.
[0102] (2) The volume of the lithium iron phosphate solution in step (1) is evaporated until the residual volume is 20% of the initial volume of the lithium iron phosphate solution, the steam generated by evaporation can be recovered as hydrochloric acid after condensation, the residue after evaporation is diluted with water to the original volume, iron powder is added to react (the amount of iron powder added is 1.3 times the mass of copper impurities), and the reaction is carried out at room temperature for 2 hours to obtain a copper removal solution, lithium fluoride is added to the copper removal solution (the amount of lithium fluoride added is 2 times the mass of aluminum element), the reaction is carried out at 30° C. for 2 hours, and then filtered to obtain a copper removal aluminum solution, and the copper removal aluminum solution is evaporated again until the residual volume is 20% of the initial volume of the copper removal aluminum solution, the steam generated by evaporation can be recovered as hydrochloric acid after condensation, the residue after evaporation is diluted with water to the original volume of the solution, and the insoluble matter is filtered to obtain a calcium and magnesium removal solution.
[0103] (3) The calcium-magnesium-removing solution in step (2) is evaporated and concentrated to a residual volume of 1 / 15 of the initial volume of the calcium-magnesium-removing solution, followed by spray drying and calcination to obtain a lithium iron phosphate positive electrode material, wherein the carbon source is carbon black, the amount of carbon black added is 8% of the solid content of the lithium iron phosphate, the calcination temperature is 750° C., and the calcination time is 4 h.
[0104] (4) The steam generated by the two evaporation and concentration steps is collected and condensed to be recovered as hydrochloric acid.
[0105] Comparative Example 1
[0106] This comparative example is substantially the same as Example 1, except that the concentration and evaporation of the copper-aluminum removal solution and the subsequent dilution in Example 1 are omitted in this comparative example.
[0107] Specifically, this comparative example provides a method for preparing battery-grade lithium iron phosphate from waste lithium iron phosphate powder, which specifically includes the following steps:
[0108] (1) Take 500 g of lithium iron phosphate waste powder (iron content 27%), add 1000 g of 25% hydrochloric acid solution by mass, react at 50° C. for 3 h, and filter to obtain a lithium iron phosphate solution.
[0109] (2) The volume of the lithium iron phosphate solution in step (1) is evaporated until the remaining volume is 20% of the initial volume of the lithium iron phosphate solution, and then diluted with water to the original volume, iron powder is added to react (the amount of iron powder added is 1.3 times the mass of copper impurities), and the copper removal solution is obtained after reacting at room temperature for 2 hours, and lithium fluoride is added to the copper removal solution (the amount of lithium fluoride added is 7 times the mass of aluminum element), and the copper removal aluminum solution is obtained after filtering after reacting at 30° C. for 2 hours.
[0110] (3) The calcium-magnesium-removing solution in step (2) is evaporated and concentrated to a residual volume of 1 / 15 of the initial volume of the calcium-magnesium-removing solution, followed by spray drying and calcination to obtain a lithium iron phosphate positive electrode material, wherein the carbon source is carbon black, the amount of carbon black added is 8% of the solid content of the lithium iron phosphate, the calcination temperature is 750° C., and the calcination time is 4 h.
[0111] (4) The steam generated by the two evaporation and concentration steps is collected and condensed to be recovered as hydrochloric acid.
[0112] Comparative Example 2
[0113] This comparative example is basically the same as Example 1, except that the pH value is adjusted by dilution after evaporation instead of using sodium hydroxide as a pH adjuster.
[0114] Specifically, this comparative example provides a method for preparing lithium iron phosphate from waste lithium iron phosphate powder, which specifically includes the following steps:
[0115] (1) Take 500 g of lithium iron phosphate waste powder (iron content 27%), add 1000 g of 25% hydrochloric acid solution by mass, react at 50° C. for 3 h, and filter to obtain a lithium iron phosphate solution.
[0116] (2) The volume of the lithium iron phosphate solution in step (1) is adjusted to pH 1.2 using sodium hydroxide, and iron powder is added to react (the amount of iron powder added is 1.3 times the mass of copper impurities), and the reaction is carried out at room temperature for 2 hours to obtain a copper removal solution, lithium fluoride is added to the copper removal solution (the amount of lithium fluoride added is 7 times the mass of aluminum element), and the reaction is carried out at 30° C. for 2 hours, and then filtered to obtain a copper removal aluminum solution, and sodium hydroxide is added again to adjust the pH to 6.8, and the insoluble matter is filtered to obtain a calcium and magnesium removal solution.
[0117] (3) The calcium-magnesium-removing solution in step (2) is evaporated and concentrated to a residual volume of 1 / 15 of the initial volume of the calcium-magnesium-removing solution, followed by spray drying and calcination to obtain a lithium iron phosphate positive electrode material, wherein the carbon source is carbon black, the amount of carbon black added is 8% of the solid content of the lithium iron phosphate, the calcination temperature is 750° C., and the calcination time is 4 h.
[0118] The lithium iron phosphate provided in the above-mentioned Examples 1-8 and Comparative Examples 1-2 was tested, wherein the impurity detection was performed using an inductively coupled plasma emission spectrometer (ICP), and the 0.1C first discharge capacity and first effect were both tested using an electrochemical workstation.
[0119] The test results are as follows:
[0120] Table 1. Analysis of physical properties of lithium iron phosphate prepared from waste lithium iron phosphate powder
[0121]
[0122]
[0123] As can be seen from the above table, the impurity content in the battery-grade lithium iron phosphate prepared in Examples 1-5 of the present invention is significantly less than that in Comparative Examples 1-2, and the first discharge capacity and the first effect are significantly higher than those in Comparative Examples 1-2, wherein the degree of evaporation concentration in Example 6 is outside the preferred range of the present application, resulting in a large pH concentration in the system and poor removal of copper, and when the amount of lithium fluoride added in Example 7 exceeds the preferred range of the present application, a large amount of fluoride ions will be introduced, causing the final battery to be "poisoned", affecting its electrochemical properties, and its first discharge capacity and first effect are significantly lower than those in Example 1. It can be seen from Example 8 that when the amount of lithium fluoride added is too little and is lower than the preferred range in the present application, Al cannot be fully and effectively removed, and the content of impurity Al is significantly higher than other embodiments and comparative examples. In Comparative Example 1, due to the omission of the second evaporation concentration and dilution process, Ca and Mg cannot be fully and effectively removed, and the content of impurities Ca and Mg is significantly higher than that in Example 1-7. It can be seen from Comparative Example 2 that evaporation concentration has the advantage of having a lower impurity content in the product while greatly reducing the amount of waste salt compared to conventional alkali regulation.
[0124] In summary, the method for preparing battery-grade lithium iron phosphate from lithium iron phosphate waste powder provided by the present invention adopts hydrochloric acid solution to dissolve lithium iron phosphate waste powder, and through two evaporation concentrations and dilutions, not only can the pH be adjusted, but also the hydrochloric acid solution can be recovered by condensing the evaporated steam, the recovery ratio exceeds 96%, the direct recovery rate of lithium is >99.5%, the recovery cost is low, and the raw material (hydrochloric acid solution for dissolution) can be recycled; the present invention does not add any alkaline solution in the process of removing impurities and adjusting the pH of the solution, while reducing the pressure of wastewater treatment, the high purity of the prepared lithium iron phosphate material is guaranteed, and the product performance is more superior; in addition, in the present application, copper impurities and aluminum impurities are removed by introducing iron powder and lithium fluoride, and the excess fluorine can also remove calcium and magnesium in the second evaporation concentration and dilution process, and the entire impurity removal process does not introduce other impurity components, so that the impurity content of the lithium iron phosphate prepared by the present application is low, the first discharge capacity is large and the first efficiency is high. The present invention removes impurities from the lithium iron waste powder by concentrating and drying the slurry, and then calcining at normal pressure to prepare battery-grade lithium iron phosphate, and the recovery process is short.
[0125] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A method for preparing battery-grade lithium iron phosphate from waste lithium iron phosphate powder, characterized in that: include: Dissolution step: dissolving the waste lithium iron phosphate powder in a hydrochloric acid solution and then separating the solid and the liquid to obtain a lithium iron phosphate solution; The impurity removal step includes: concentrating and evaporating the lithium iron phosphate solution without adding alkali, and then diluting it to adjust the pH, wherein the lithium iron phosphate solution is concentrated and evaporated to 10-25% of the initial volume of the lithium iron phosphate solution, and then diluting it with water to the initial volume of the lithium iron phosphate solution; adding iron powder to remove copper impurities, and then adding lithium fluoride to remove aluminum impurities, wherein the amount of lithium fluoride added is 6-10 times the mass of aluminum element in the lithium iron phosphate solution; solid-liquid separation to obtain a copper-aluminum removal solution; concentrating and evaporating the copper-aluminum removal solution without adding alkali, and then diluting it to adjust the pH, separating insoluble matter, and obtaining a calcium-magnesium removal solution; Calcination step: drying the calcium and magnesium removal solution and then calcining it to obtain battery-grade lithium iron phosphate powder.
2. The method for preparing battery-grade lithium iron phosphate from waste lithium iron phosphate powder according to claim 1, characterized in that: The impurity removal step includes at least one of the following features (1) to (2): Feature (1): The amount of the iron powder added is 1.2-2.0 times the amount of copper impurities in the lithium iron phosphate solution; Feature (2): After adding the lithium fluoride, react at 30-70°C for 1-3 hours.
3. The method for preparing battery-grade lithium iron phosphate from waste lithium iron phosphate powder according to claim 1, characterized in that: The copper-aluminum removal solution is concentrated and evaporated to 10-25% of the initial volume of the copper-aluminum removal solution, and then water is added to dilute it to the initial volume of the copper-aluminum removal solution.
4. The method for preparing battery-grade lithium iron phosphate from waste lithium iron phosphate powder according to claim 1, characterized in that: The mass concentration of the hydrochloric acid solution is 15-40%.
5. The method for preparing battery-grade lithium iron phosphate from waste lithium iron phosphate powder according to claim 4, characterized in that: The dissolving step comprises at least one of the following features (3) to (5): Feature (3): The mass ratio of the lithium iron phosphate waste powder to the hydrochloric acid solution is 1:1.4-1:3.5; Feature (4): The iron content in the lithium iron phosphate waste powder is 25-33%; Feature (5): The reaction temperature in the dissolution step is 20-100°C and the reaction time is 1-4h.
6. The method for preparing battery-grade lithium iron phosphate from waste lithium iron phosphate powder according to claim 1, characterized in that: The calcination temperature is 500-850°C and the calcination time is 1-7h.
7. The method for preparing battery-grade lithium iron phosphate from waste lithium iron phosphate powder according to claim 1, characterized in that: Before drying the decalcification and magnesium solution, the method further comprises evaporating and concentrating the decalcification and magnesium solution to 1 / 20-1 / 12 of the initial volume of the decalcification and magnesium solution.
8. The method for preparing battery-grade lithium iron phosphate from waste lithium iron phosphate powder according to claim 1, characterized in that: A carbon source is added as an additive during the calcination process, and the amount of the carbon source added is 5-10% of the solid content of the lithium iron phosphate.
9. The method for preparing battery-grade lithium iron phosphate from waste lithium iron phosphate powder according to claim 1, characterized in that: The method for preparing battery-grade lithium iron phosphate from waste lithium iron phosphate powder also includes a hydrochloric acid recovery step: condensing and recovering the steam generated when the lithium iron phosphate solution and the copper-aluminum removal solution are concentrated and evaporated.
10. The method for preparing battery-grade lithium iron phosphate from waste lithium iron phosphate powder according to claim 9, characterized in that: The recovery rate of the hydrochloric acid is greater than 96%.
Citation Information
Patent Citations
Method for preparing battery-grade iron phosphate and industrial-grade lithium phosphate in waste lithium iron phosphate battery
CN109775678A
Preparation method of battery-grade iron phosphate
CN110482512A
Method for recycling and regenerating waste lithium iron phosphate battery positive electrode material
CN113501510A
Recycling method of waste lithium iron phosphate battery
CN114394610A
Method for recovering iron phosphate from lithium iron phosphate extraction slag and application thereof
CN115196609A