Composite positive pole piece as well as preparation method and application thereof

By using a double-layer coating technology on the surface of the positive electrode current collector of lithium ion batteries, using lithium iron phosphate active substance layers with different particle sizes, the high-temperature performance problems caused by lithium supplementation agents are solved, the cycle life and energy density of the battery are improved, and the cycle life and energy density of the battery are improved. Improved fast charging performance.

CN118899404AInactive Publication Date: 2024-11-05安徽得壹能源科技有限公司

Patent Information

Application Number
CN202411174901.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-26
Publication Date
2024-11-05
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The high-temperature performance of lithium supplement agent in the positive electrode in lithium-ion batteries is poor after adding lithium-ion agent, resulting in deterioration of battery circulation and storage performance.

Method used

Using double-layer coating technology, the active material layers of lithium iron phosphate of different particle sizes are applied to the surface of the positive electrode current collector in turn. The first active material layer uses lithium iron phosphate with slightly larger particle size to increase the compaction and energy density of the electrode sheet. The active substance layer uses high-power lithium iron phosphate with a small particle size to reduce the diffusion impedance, avoid contact with the lithium supplement agent and improve the stability of the lithium supplement agent.

Benefits of technology

A composite electrode sheet with high compaction and low resistance is achieved, which improves the active lithium removal of lithium supplements, extends the service life of the battery cell, and improves energy density and fast charging performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005010452140000071
    Figure BDA0005010452140000071
  • Figure HDA0005010452150000011
    Figure HDA0005010452150000011
Patent Text Reader

Abstract

The invention provides a composite positive pole piece and a preparation method and application thereof, the positive pole piece comprises a positive current collector and a first active substance layer, the first active substance layer is arranged on the surface of the positive current collector, the first active substance layer comprises first lithium iron phosphate, a lithium supplement agent, a first conductive agent and a first binder, and the second active material layer is arranged on the surface of the first active material layer, and the second active material layer comprises second lithium iron phosphate, a second conductive agent and a second binder. The positive pole piece has high compactness and low resistance, and can fully improve the active lithium separation of the lithium supplement agent, thereby prolonging the service life of a battery cell, improving the energy density and improving the rapid charging capability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of lithium batteries, and in particular to a composite positive electrode sheet and a preparation method and application thereof. Background Art

[0002] Since its commercialization in the 1990s, lithium-ion batteries have become an indispensable energy storage solution in many fields such as portable electronic devices, electric vehicles and energy storage systems. With the pursuit of higher energy density, longer cycle life and lower cost, the development of long-cycle lithium-ion batteries has become one of the hot topics in battery technology research.

[0003] Lithium replenishers are a strategy to improve the cycle life of lithium-ion batteries. Lithium replenishers can slow down the capacity decay of negative electrode materials by replenishing active lithium ions during the battery charging and discharging process, thereby extending the service life of the battery. Lithium replenishers are usually high-capacity, low-first-efficiency materials, which are added during the positive electrode slurrying process. During the charging process, lithium ions are released from the lithium replenisher to replenish the irreversible capacity loss of the first charge and discharge. Positive electrode lithium replenishment is easy to operate and the process is simple. There is no need to change the production line structure. It only needs to add lithium replenishers to the positive electrode slurry mixing link, which has good application prospects. As an alternative technical route, many lithium replenishment additives for positive electrode materials have entered the research scope. However, the lithium replenisher itself has low conductivity, poor stability and is prone to decomposition. The decomposition potential required for delithiation is high. Although it can reduce irreversible capacity loss, the decomposition products remain in the positive electrode sheet, which will cause a series of problems such as deterioration of high-temperature performance. Summary of the invention

[0004] The present invention aims to solve at least one of the technical problems in the related art to a certain extent. To this end, one object of the present invention is to provide a method for preparing a positive electrode sheet of a lithium-ion battery and its application to solve the problem of poor high temperature performance of the positive electrode after adding a lithium supplement.

[0005] According to an embodiment of the present invention, the present invention provides a positive electrode sheet. According to an embodiment of the present invention, the positive electrode sheet comprises

[0006] Positive electrode current collector,

[0007] a first active material layer, the first active material layer is arranged on the surface of the positive electrode current collector, the first active material layer comprises a first lithium iron phosphate, a lithium supplement, a first conductive agent and a first binder,

[0008] and a second active material layer, the second active material layer is arranged on the surface of the first active material layer, and the second active material layer includes a second lithium iron phosphate, a second conductive agent and a second binder. The positive electrode lithium supplement can improve the gram capacity by supplementing active lithium ions, increase the energy density of the battery, and reduce the irreversible capacity loss of the negative electrode material to increase the cycle life of the battery. However, the conductivity of the lithium supplement material itself is very low, and the conductivity of the decomposed product will be further reduced. The residue in the positive electrode sheet will increase the impedance of the positive electrode sheet, causing the high temperature cycle and storage performance to deteriorate.

[0009] According to an embodiment of the present invention, the positive electrode plate may further include at least one of the following additional technical features:

[0010] According to an embodiment of the present invention, the lithium supplement is Li2NiO2 and / or Li5FeO4.

[0011] According to an embodiment of the present invention, the particle size D50 of the lithium supplement agent is 4-10 μm.

[0012] According to an embodiment of the present invention, the weight ratio of the first lithium iron phosphate, the lithium supplement agent, the first conductive agent, and the first binder is (92% to 98%): (0.1% to 6%): (0.5% to 2%): (1.2% to 2.5%).

[0013] According to an embodiment of the present invention, the particle size D50 of the first lithium iron phosphate is 0.4-2.2 μm.

[0014] According to an embodiment of the present invention, the particle size D50 of the first lithium iron phosphate is 0.8-1.4 μm.

[0015] According to an embodiment of the present invention, the weight ratio of the second lithium iron phosphate, the second conductive agent, and the second binder is (95% to 98%): (0.5% to 2%): (1.2% to 2.5%).

[0016] According to an embodiment of the present invention, the particle size D50 of the second lithium iron phosphate is 0.4-1.8 μm.

[0017] According to an embodiment of the present invention, the particle size D50 of the second lithium iron phosphate is 0.6-1.2 μm.

[0018] According to an embodiment of the present invention, the first conductive agent is selected from one or more of carbon black, conductive graphite, carbon fiber, carbon nanotube and graphene;

[0019] According to an embodiment of the present invention, the second conductive agent is selected from one or more of carbon black, conductive graphite, carbon fiber, carbon nanotube and graphene.

[0020] According to an embodiment of the present invention, the first binder is selected from one or more of polyvinyl alcohol, polytetrafluoroethylene, polyolefins, polyvinylidene fluoride, modified SBR rubber, fluorinated rubber and polyurethane.

[0021] According to an embodiment of the present invention, the second binder is selected from one or more of polyvinyl alcohol, polytetrafluoroethylene, polyolefins, polyvinylidene fluoride, modified SBR rubber, fluorinated rubber and polyurethane.

[0022] According to an embodiment of the present invention, the positive electrode current collector includes at least one selected from aluminum foil, carbon-coated aluminum foil, nickel foil and aluminum-plated polymer film.

[0023] In another aspect of the present invention, the present invention also provides a method for preparing a positive electrode sheet. According to an embodiment of the present invention, the method comprises:

[0024] Performing a first mixing process on the first lithium iron phosphate, the first lithium supplement agent, the first conductive agent, the first binder, and the first solvent to obtain a first active material layer slurry;

[0025] Performing a second mixing process on the second lithium iron phosphate, the second conductive agent, the second binder, and the second solvent to obtain a second active material layer slurry;

[0026] Applying the first active material layer slurry to the surface of the positive electrode current collector to obtain a positive electrode current collector with the first active material layer on the surface;

[0027] The second active material layer slurry is coated on the surface of the first active material layer of the positive electrode current collector whose surface is covered with the first active material layer, so as to obtain a positive electrode current collector whose surfaces are respectively the second active material layer and the first active material layer from top to bottom, and then dried and rolled to obtain a positive electrode plate. The present invention adopts a double-layer coating technology to sequentially coat the first active material layer and the second active material layer on the surface of the positive electrode current collector; the first active material layer adopts lithium iron phosphate with a slightly larger particle size, which can effectively improve the compaction of the plate and the energy density of the battery cell, and at the same time, the lithium supplement agent is added to the first active material layer, which can avoid direct contact between the lithium supplement agent and the air and improve the stability of the lithium supplement agent; the second active material layer adopts high-power lithium iron phosphate with a smaller particle size, which can reduce the diffusion impedance of the positive electrode plate surface, improve the positive electrode dynamics, and reduce the increase in the positive electrode lithium ion diffusion impedance caused by the lithium supplement agent remaining in the positive electrode. The final composite electrode containing the positive electrode lithium supplement has higher electrode compaction and lower membrane resistance, which can fully improve the active lithium release of the lithium supplement, increase the cycle life and energy density of the battery cell, and also has better fast charging performance.

[0028] According to an embodiment of the present invention, the above method may further include at least one of the following additional technical features:

[0029] According to an embodiment of the present invention, the mass ratio of the first active material layer to the second active material layer is (1-9):(1-9).

[0030] According to an embodiment of the present invention, the first solvent is water.

[0031] According to an embodiment of the present invention, the second solvent is water.

[0032] According to an embodiment of the present invention, the lithium supplement is Li2NiO2 and / or Li5FeO4.

[0033] According to an embodiment of the present invention, the particle size D50 of the lithium supplement agent is 4-10 μm.

[0034] According to an embodiment of the present invention, the weight ratio of the first lithium iron phosphate, the lithium supplement agent, the first conductive agent, and the first binder is (92% to 98%): (0.1% to 6%): (0.5% to 2%): (1.2% to 2.5%).

[0035] According to an embodiment of the present invention, the particle size D50 of the first lithium iron phosphate is 0.4-2.2 μm.

[0036] According to an embodiment of the present invention, the particle size D50 of the first lithium iron phosphate is 0.8-1.4 μm.

[0037] According to an embodiment of the present invention, the weight ratio of the second lithium iron phosphate, the second conductive agent, and the second binder is (95% to 98%): (0.5% to 2%): (1.2% to 2.5%).

[0038] According to an embodiment of the present invention, the particle size D50 of the second lithium iron phosphate is 0.4-1.8 μm.

[0039] According to an embodiment of the present invention, the particle size D50 of the second lithium iron phosphate is 0.6-1.2 μm.

[0040] According to an embodiment of the present invention, the first conductive agent is selected from one or more of carbon black, conductive graphite, carbon fiber, carbon nanotube and graphene.

[0041] According to an embodiment of the present invention, the second conductive agent is selected from one or more of carbon black, conductive graphite, carbon fiber, carbon nanotube and graphene.

[0042] According to an embodiment of the present invention, the first binder is selected from one or more of polyvinyl alcohol, polytetrafluoroethylene, polyolefins, polyvinylidene fluoride, modified SBR rubber, fluorinated rubber and polyurethane.

[0043] According to an embodiment of the present invention, the second binder is selected from one or more of polyvinyl alcohol, polytetrafluoroethylene, polyolefins, polyvinylidene fluoride, modified SBR rubber, fluorinated rubber and polyurethane.

[0044] According to an embodiment of the present invention, the positive electrode current collector includes at least one selected from aluminum foil, carbon-coated aluminum foil, nickel foil and aluminum-plated polymer film.

[0045] In another aspect of the present invention, the present invention further provides a lithium battery. According to an embodiment of the present invention, the lithium battery comprises the positive electrode sheet described above or a positive electrode sheet prepared according to any of the methods for preparing a positive electrode sheet described above.

[0046] In another aspect of the present invention, the present invention further provides a method for preparing a composite positive electrode sheet. According to an embodiment of the present invention, the method comprises:

[0047] The first lithium iron phosphate, the lithium supplement agent, the conductive agent, and the binder are uniformly mixed in a certain proportion, and a certain amount of solvent is added to obtain a first active material layer slurry with a viscosity suitable for coating;

[0048] The second lithium iron phosphate, the conductive agent and the binder are uniformly mixed in a certain ratio, and a certain amount of solvent is added to obtain a second active material layer slurry with a viscosity suitable for coating;

[0049] The first active material layer slurry and the second active material layer slurry are coated onto the positive electrode collector in the above order, and a composite positive electrode sheet is obtained after drying and rolling; wherein the mass ratio of the first active material layer to the second active material layer is (1-9): (1-9).

[0050] According to an embodiment of the present invention, the positive electrode current collector includes at least one of aluminum foil, carbon-coated aluminum foil, nickel foil and aluminum-plated polymer film.

[0051] According to an embodiment of the present invention, the positive electrode lithium supplement can improve the gram capacity by supplementing active lithium ions, improve the energy density of the battery, and reduce the irreversible capacity loss of the negative electrode material, thereby improving the cycle life of the battery. However, the conductivity of the lithium supplement material itself is very low, and the conductivity of the decomposed product will be further reduced. The residue in the positive electrode plate will increase the impedance of the positive electrode plate, causing the high-temperature cycle and storage performance to deteriorate. The present invention adopts a double-layer coating technology to sequentially coat the first active material layer and the second active material layer on the surface of the positive electrode current collector; the first active material layer uses lithium iron phosphate with a slightly larger particle size, which can effectively improve the compaction of the electrode plate and the energy density of the battery cell. At the same time, the lithium supplement is added to the first active material layer, which can avoid direct contact between the lithium supplement and the air and improve the stability of the lithium supplement; the second active material layer uses high-power lithium iron phosphate with a smaller particle size, which can reduce the diffusion impedance of the positive electrode plate surface, improve the positive electrode dynamics, and reduce the increase in the positive electrode lithium ion diffusion impedance caused by the lithium supplement remaining in the positive electrode. The final composite electrode containing the positive electrode lithium supplement has higher electrode compaction and lower membrane resistance, which can fully improve the active lithium release of the lithium supplement, increase the cycle life and energy density of the battery cell, and also has better fast charging performance.

[0052] According to the embodiments of the present invention, the present invention solves the problem of poor high temperature performance after adding a lithium supplement to the positive electrode, and adopts a double-layer coating technology to sequentially coat lithium iron phosphate active material layers of different particle sizes on the surface of the positive electrode current collector to achieve optimization of the battery performance. The composite pole piece containing the positive electrode lithium supplement obtained by the present invention has a high compaction degree and low resistance, which can fully improve the active lithium release of the lithium supplement, thereby extending the service life of the battery, improving the energy density, and improving the fast charging capability. BRIEF DESCRIPTION OF THE DRAWINGS

[0053] The above and / or additional aspects and advantages of the present invention will become apparent and easily understood from the description of the embodiments in conjunction with the following drawings, in which:

[0054] Figure 1 It is a schematic diagram of the structure of the composite positive electrode sheet in an embodiment of the present invention. DETAILED DESCRIPTION

[0055] The embodiments described below with reference to the accompanying drawings are exemplary and are intended to be used to explain the present invention, but should not be construed as limiting the present invention.

[0056] In addition, the terms "first" and "second" are used for descriptive purposes only and should not be understood as indicating or implying relative importance or implicitly indicating the number of the indicated technical features. Therefore, the features defined as "first" and "second" may explicitly or implicitly include at least one of the features. In the description of the present invention, the meaning of "plurality" is at least two, such as two, three, etc., unless otherwise clearly and specifically defined.

[0057] The present invention is described below with reference to specific embodiments. It should be noted that these embodiments are merely illustrative and do not limit the present invention in any way.

[0058] Example 1

[0059] A lithium-ion battery comprises the above-mentioned composite positive electrode sheet, a negative electrode sheet, a separator between the positive electrode sheet and the negative electrode sheet, and an electrolyte.

[0060] An energy-type lithium iron phosphate with a particle size D50 of 1.2 μm is used as the first active material, and is evenly mixed with a lithium supplement (such as Li2NiO2), a conductive agent (such as carbon black), and a binder (such as polyvinyl alcohol) in a mass ratio of 96%:1%:1%:2%, and then dispersed in a solvent (such as water) to obtain a first active material layer slurry; a power-type lithium iron phosphate with a particle size D50 of 0.8 μm is used as the second active material, and is evenly mixed with a conductive agent (such as carbon black) and a binder (such as polyvinyl alcohol) in a mass ratio of 97%:1%:2%, and then dispersed in a solvent (such as water) to obtain a second active material layer slurry; the above-mentioned first active material layer slurry and the second active material layer slurry are coated on the positive electrode collector in the above order, and a composite positive electrode sheet is obtained after drying and rolling; wherein the mass ratio of the first active material layer to the second active material layer is 5:5. Figure 1 Schematic diagram of the obtained electrode sheet.

[0061] Example 2

[0062] A lithium-ion battery comprises a positive electrode sheet, a negative electrode sheet, a separator between the positive electrode sheet and the negative electrode sheet, and an electrolyte.

[0063] The particle size D50 of the first active material is 1.0 μm;

[0064] The other conditions and parameters are exactly the same as those in Example 1 and will not be described again here.

[0065] Example 3

[0066] A lithium-ion battery comprises a positive electrode sheet, a negative electrode sheet, a separator between the positive electrode sheet and the negative electrode sheet, and an electrolyte.

[0067] The mass percentage of lithium supplement is 2%;

[0068] The other conditions and parameters are exactly the same as those in Example 1 and will not be described again here.

[0069] Example 4

[0070] A lithium-ion battery comprises a positive electrode sheet, a negative electrode sheet, a separator between the positive electrode sheet and the negative electrode sheet, and an electrolyte.

[0071] The particle size D50 of the second active material is 0.6 μm;

[0072] The other conditions and parameters are exactly the same as those in Example 1 and will not be described again here.

[0073] Example 5

[0074] A lithium-ion battery comprises a positive electrode sheet, a negative electrode sheet, a separator between the positive electrode sheet and the negative electrode sheet, and an electrolyte.

[0075] The mass ratio of the first active material layer to the second active material layer is 3:7;

[0076] The other conditions and parameters are exactly the same as those in Example 1 and will not be described again here.

[0077] Example 6

[0078] A lithium-ion battery comprises a positive electrode sheet, a negative electrode sheet, a separator between the positive electrode sheet and the negative electrode sheet, and an electrolyte.

[0079] The mass ratio of the first active material layer to the second active material layer is 7:3;

[0080] The other conditions and parameters are exactly the same as those in Example 1 and will not be described again here.

[0081] Comparative Example 1

[0082] A lithium-ion battery comprises a positive electrode sheet, a negative electrode sheet, a separator between the positive electrode sheet and the negative electrode sheet, and an electrolyte.

[0083] Energy-type lithium iron phosphate with a particle size D50 of 1.2 μm is used as the first active material, and is evenly mixed with a lithium supplement, a conductive agent, and a binder in a mass ratio of 96%:1%:1%:2%, and then dispersed into a solvent to obtain a first active material layer slurry; the active material and formula of the second active material layer are all consistent with those of the first active material layer;

[0084] The other conditions and parameters are exactly the same as those in Example 1 and will not be described again here.

[0085] Comparative Example 2

[0086] A lithium-ion battery comprises a positive electrode sheet, a negative electrode sheet, a separator between the positive electrode sheet and the negative electrode sheet, and an electrolyte.

[0087] The mass percentage of lithium supplement is 8%;

[0088] The other conditions and parameters are exactly the same as those in Example 1 and will not be described again here.

[0089] Performance Testing:

[0090] Cycle test: Cycle test is carried out in accordance with the cycle life test requirements of GB / T 31484-2015 "Cycle life requirements and test methods for power batteries for electric vehicles", and the capacity retention rate is measured after 600 cycles of 25°C room temperature cycles and 300 cycles of 45°C high temperature cycles.

[0091] DC internal resistance test: At 25°C, the obtained lithium-ion secondary battery was implanted in copper wire and then lithium-plated. The SOC was adjusted to 50%, and the battery was discharged at 2C pulse current for 30s. The voltage drop of the positive electrode to the reference electrode before and after discharge was recorded, and the DC internal resistance of the positive electrode was obtained according to R=U / I.

[0092] Energy density test: The battery was weighed and charged to 3.65V at 1C constant current and constant voltage, then discharged to 2.5V at 1C constant current, the discharge energy was recorded, and the energy density was calculated.

[0093] Specifically, the relevant parameters of Examples 1 to 6 and Comparative Examples 1 to 2 and the performance test results under the same conditions are shown in Table 1 below.

[0094] Table 1 Comparison of physical properties of embodiments and comparative examples

[0095]

[0096] As can be seen from Table 1, the above-mentioned embodiments of the present invention reduce the DCR of the positive electrode within the scope of the present invention, and achieve a higher energy density and good cycle performance; while the comparative examples are not within the scope of the present invention, and show poor high-temperature cycle performance or a higher DCR of the positive electrode. Specifically, compared with Example 1, Examples 2 and 4 respectively reduce the particle size of the second and first active materials, which is beneficial to reducing the DCR of the positive electrode and improving the dynamics of the positive electrode, while reducing the compaction density of the positive electrode and losing the partial energy density of the battery cell; Example 3 increases the content of the lithium supplement, supplements more active lithium, improves the gram capacity of the positive electrode, and improves the energy density and room temperature cycle performance of the battery cell, while the increase in the content of the lithium supplement increases the DCR of the positive electrode, and more lithium supplement decomposition products make the high-temperature cycle performance worse; Examples 5 and 6 respectively change the mass ratio of the first and second active material layers, increase the mass ratio of the first active material layer, which is beneficial to improving the energy density of the battery cell, and the corresponding increase in the lithium supplement will improve the room temperature cycle performance of the battery cell, while increasing the mass ratio of the second active material layer reduces the DCR of the positive electrode, but reduces the energy density of the battery cell.

[0097] Compared with Example 1, Comparative Example 1 has only the first active material layer. Although the energy density of the battery cell is increased, the DCR of the positive electrode is also increased accordingly, which reduces the high temperature cycle performance of the battery cell. In Comparative Example 2, the content of the lithium supplement is too much. Although the room temperature cycle performance is improved, the DCR of the positive electrode is sharply increased, the kinetics of the positive electrode are poor, and the high temperature cycle performance of the battery cell is seriously affected.

[0098] In the description of this specification, the description with reference to the terms "one embodiment", "some embodiments", "example", "specific example", or "some examples" etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representations of the above terms do not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described may be combined in any one or more embodiments or examples in a suitable manner. In addition, those skilled in the art may combine and combine the different embodiments or examples described in this specification and the features of the different embodiments or examples, without contradiction.

[0099] Although the embodiments of the present invention have been shown and described above, it is to be understood that the above embodiments are exemplary and are not to be construed as limitations of the present invention. A person skilled in the art may change, modify, replace and vary the above embodiments within the scope of the present invention.

Claims

1. A positive electrode sheet, characterized in that: The positive electrode sheet comprises Positive electrode current collector, a first active material layer, the first active material layer is arranged on the surface of the positive electrode current collector, the first active material layer comprises a first lithium iron phosphate, a lithium supplement, a first conductive agent and a first binder, and a second active material layer, the second active material layer being disposed on a surface of the first active material layer, the second active material layer comprising a second lithium iron phosphate, a second conductive agent, and a second binder.

2. The positive electrode sheet according to claim 1, characterized in that: The lithium supplement agent is Li2NiO2 and / or Li5FeO4; Optionally, the particle size D50 of the lithium supplement agent is 4 to 10 μm.

3. The positive electrode sheet according to claim 1, characterized in that: The weight ratio of the first lithium iron phosphate, the lithium supplement agent, the first conductive agent, and the first binder is (92% to 98%): (0.1% to 6%): (0.5% to 2%): (1.2% to 2.5%); Optionally, the particle size D50 of the first lithium iron phosphate is 0.4 to 2.2 μm; Preferably, the particle size D50 of the first lithium iron phosphate is 0.8-1.4 μm.

4. The positive electrode sheet according to claim 1, characterized in that: The weight ratio of the second lithium iron phosphate, the second conductive agent, and the second binder is (95% to 98%): (0.5% to 2%): (1.2% to 2.5%); Optionally, the particle size D50 of the second lithium iron phosphate is 0.4 to 1.8 μm; Preferably, the particle size D50 of the second lithium iron phosphate is 0.6-1.2 μm.

5. The positive electrode sheet according to claim 1, characterized in that: The first conductive agent is selected from one or more of carbon black, conductive graphite, carbon fiber, carbon nanotube and graphene; Optionally, the second conductive agent is selected from one or more of carbon black, conductive graphite, carbon fiber, carbon nanotube and graphene.

6. The positive electrode sheet according to claim 1, characterized in that: The first binder is selected from one or more of polyvinyl alcohol, polytetrafluoroethylene, polyolefins, polyvinylidene fluoride, modified SBR rubber, fluorinated rubber and polyurethane; Optionally, the second binder is selected from one or more of polyvinyl alcohol, polytetrafluoroethylene, polyolefins, polyvinylidene fluoride, modified SBR rubber, fluorinated rubber and polyurethane.

7. The positive electrode sheet according to claim 1, characterized in that: The positive electrode current collector comprises at least one selected from aluminum foil, carbon-coated aluminum foil, nickel foil and aluminum-plated polymer film.

8. A method for preparing a positive electrode sheet, characterized in that: include: Performing a first mixing process on the first lithium iron phosphate, the first lithium supplement agent, the first conductive agent, the first binder, and the first solvent to obtain a first active material layer slurry; Performing a second mixing process on the second lithium iron phosphate, the second conductive agent, the second binder, and the second solvent to obtain a second active material layer slurry; Applying the first active material layer slurry to the surface of the positive electrode current collector to obtain a positive electrode current collector with the first active material layer on the surface; The second active material layer slurry is coated onto the surface of the first active material layer of the positive electrode collector whose surface is covered with the first active material layer to obtain a positive electrode collector whose surfaces from top to bottom are the second active material layer and the first active material layer, and then dried and rolled to obtain a positive electrode sheet.

9. The method according to claim 8, characterized in that The mass ratio of the first active material layer to the second active material layer is (1-9): (1-9); Optionally, the first solvent is water; Optionally, the second solvent is water; Optionally, the lithium supplement is Li2NiO2 and / or Li5FeO4; Optionally, the particle size D50 of the lithium supplement agent is 4 to 10 μm; Optionally, the weight ratio of the first lithium iron phosphate, the lithium supplement agent, the first conductive agent, and the first binder is (92% to 98%): (0.1% to 6%): (0.5% to 2%): (1.2% to 2.5%); Optionally, the particle size D50 of the first lithium iron phosphate is 0.4 to 2.2 μm; Preferably, the particle size D50 of the first lithium iron phosphate is 0.8-1.4 μm; Optionally, the weight ratio of the second lithium iron phosphate, the second conductive agent, and the second binder is (95% to 98%): (0.5% to 2%): (1.2% to 2.5%); Optionally, the particle size D50 of the second lithium iron phosphate is 0.4 to 1.8 μm; Preferably, the particle size D50 of the second lithium iron phosphate is 0.6-1.2 μm; Optionally, the first conductive agent is selected from one or more of carbon black, conductive graphite, carbon fiber, carbon nanotube and graphene; Optionally, the second conductive agent is selected from one or more of carbon black, conductive graphite, carbon fiber, carbon nanotubes and graphene; Optionally, the first binder is selected from one or more of polyvinyl alcohol, polytetrafluoroethylene, polyolefins, polyvinylidene fluoride, modified SBR rubber, fluorinated rubber and polyurethane; Optionally, the second binder is selected from one or more of polyvinyl alcohol, polytetrafluoroethylene, polyolefins, polyvinylidene fluoride, modified SBR rubber, fluorinated rubber and polyurethane; Optionally, the positive electrode current collector includes at least one selected from aluminum foil, carbon-coated aluminum foil, nickel foil and aluminum-plated polymer film.

10. A lithium battery, characterized in that: The lithium battery comprises the positive electrode sheet according to any one of claims 1 to 7 or the positive electrode sheet prepared by the method for preparing a positive electrode sheet according to any one of claims 8 to 9.

Citation Information

Patent Citations

  • Positive pole piece, manufacturing method thereof and secondary battery

    CN111916752A

  • High-safety positive plate and lithium ion battery thereof

    CN112467107A

  • Long-circulation lithium iron phosphate thick electrode, preparation method thereof and lithium ion battery

    CN115275109A

  • Lithium supplement positive electrode, preparation method thereof and lithium ion secondary battery

    CN116154100A

  • Positive pole piece, preparation method thereof and battery

    CN118213483A

Cited By

  • Secondary battery and preparation method thereof

    CN119133420A

  • A secondary battery and a method for preparing the same

    CN119133420B

  • Composite positive pole piece as well as preparation method and application thereof

    CN119742310A

  • Positive pole piece containing lithium supplement agent, preparation method of positive pole piece and battery

    CN120453304A

  • Positive electrode sheet, secondary battery, and electric device

    WO2026002262A1