Hard carbon coated graphite composite material and preparation method and application thereof

Through the preparation of hard carbon-coated graphite composite materials, the safety and performance problems of lithium-ion batteries during fast charging are solved, and high energy density and fast charging performance are improved, which is suitable for negative electrode materials for commercial fast charging batteries.

CN115626642BActive Publication Date: 2024-12-03GUANGDONG KAIJIN NEW ENERGY TECH CORP LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211322545.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-10-25
Publication Date
2024-12-03
Estimated Expiration
2042-10-25

AI Technical Summary

Technical Problem

The fast charging performance and safety of existing lithium-ion batteries are poor, resulting in the increase in the polarization intensity of the electrode material during charging and discharging at high rate, the voltage decreases, and the increase in internal resistance leads to high thermal effects and irreversible reactions, which reduces the safety of the battery. and cycle life.

Method used

Using hard carbon coated graphite composite material, a coating is formed by grinding soft carbon coaters, activators and nitrogen sources, mixing artificial graphite precursors and carbonizing and graphitizing treatments, and preparing nitrogen doping and hardness. Carbon-coated graphite composite material improves its conductivity and lithium ion diffusion speed.

Benefits of technology

It achieves better first-time reversible specific capacity, first-time Coulomb efficiency and fast charging performance, improves the energy density and safety of lithium-ion batteries, and is suitable as the negative electrode material for commercial fast charging batteries.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0003906794350000201
    Figure BDA0003906794350000201
  • Figure BDA0003906794350000211
    Figure BDA0003906794350000211
Patent Text Reader

Abstract

The present invention relates to the technical field of material preparation, and discloses a preparation method of a hard carbon-coated graphite composite material, a hard carbon-coated graphite composite material and its application. The preparation method of the hard carbon-coated graphite composite material comprises the following steps: (I) grinding and mixing a soft carbon coating agent, an activator and a nitrogen source to form a coating, wherein the activator is a particle having oxygen-containing groups on the surface; (II) mixing the coating and an artificial graphite precursor to obtain a precursor; (III) carbonizing the precursor to obtain a carbonized product, and post-treating the carbonized product, wherein the post-treatment at least includes graphitizing the carbonized product. In the preparation method of the present invention, a coating is first prepared, and then the coating and an artificial graphite precursor are mixed to obtain a precursor, and then after carbonization and graphitization, a graphite composite material with nitrogen doping and hard carbon coating can be obtained, which has a low specific surface area and has better first reversible specific capacity, first coulomb efficiency and fast charging performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of material preparation, and in particular to a hard carbon-coated graphite composite material and a preparation method and application thereof. Background Art

[0002] In order to limit the impact of global climate change, clean and renewable energy such as wind power and solar energy has been rapidly developed. Since internal combustion engine vehicles have long been a major source of air pollution, the use of clean energy to drive vehicles plays an important role in reducing carbon dioxide emissions. Therefore, electric vehicles powered by lithium-ion batteries have developed rapidly. As we all know, lithium-ion batteries occupy an important position in the digital products and electric vehicle markets with their high energy density and power density and long life. In recent years, the mileage of electric vehicles has been greatly improved. However, the long charging time still hinders the large-scale application of electric vehicles. High-energy-density lithium batteries cannot be safely and quickly charged due to the unsatisfactory rate performance of their electrode materials. Therefore, it is very necessary to improve the performance of the negative electrode materials of fast-charging lithium batteries.

[0003] Graphite has many disadvantages, such as poor compatibility with electrolyte, low charge and discharge efficiency, unsuitable for high current rapid charge and discharge, and poor cycle stability. In the process of rapid charging, the electrode material must not only have a high lithium diffusion rate, but also have high safety. When lithium-ion batteries are charged at high speed for a long time, the Li in the electrode + The increase in concentration leads to an increase in the polarization strength of the lithium-ion battery pack, which in turn leads to a decrease in the voltage of the lithium-ion battery. In addition, during the fast charging process, the increase in internal resistance leads to a high thermal effect, resulting in irreversible reactions such as electrolyte decomposition and gas production, which reduces the safety and cycle life of the lithium battery. Therefore, domestic and foreign manufacturers use a series of modification methods to design negative electrode materials, so that the main properties of the electrode, including the conductivity of the negative electrode (reducing internal resistance), diffusion (ensuring reaction kinetics), life, safety and appropriate processing performance (specific surface area cannot be too large, reducing side reactions, and serving safety) are optimized to meet customers' high-rate charging and discharging needs.

[0004] There are many ways designed to meet the fast charging performance. One of the more common methods is to carry out a granulation process before graphitization. Generally, the shaped precursor is mixed with the binder asphalt and then granulated in a reactor. The pre-granulation process causes the material to coke and combines large and small particles to form secondary particles, so that the negative electrode material has high compaction, low expansion and improved kinetics. However, its performance improvement is still limited, and when applied to commercial batteries, the actual effect is not obvious. Summary of the invention

[0005] In view of this, the purpose of the present invention is to provide a hard carbon-coated graphite composite material and a preparation method and application thereof. The obtained hard carbon-coated graphite composite material has a low specific surface area and has a good first reversible specific capacity and first coulombic efficiency. At the same time, it has good fast charging performance and can be used as an alternative negative electrode material for power fast charging batteries in the market.

[0006] To achieve the above object, the first aspect of the present invention provides a method for preparing a hard carbon-coated graphite composite material, comprising the steps of:

[0007] (I) Preparation of coating

[0008] A soft carbon coating agent, an activator and a nitrogen source are ground and mixed to form a coating body, wherein the activator is a particle having oxygen-containing groups on the surface;

[0009] (II) Preparation of Precursor

[0010] Mixing the coating body and the artificial graphite precursor to obtain a precursor;

[0011] (III) Carbonization treatment

[0012] The precursor is carbonized to obtain a carbonized product, and the carbonized product is post-processed, wherein the post-processing at least includes graphitizing the carbonized product.

[0013] In the preparation method of the present invention, the coating is first prepared, and then the coating and an artificial graphite precursor are mixed to obtain a precursor, and then after carbonization and graphitization, a graphite composite material with nitrogen doping and hard carbon coating can be obtained. The specific surface area is not high, and it has better first reversible specific capacity, first coulomb efficiency and fast charging performance.

[0014] Compared with graphite, hard carbon has good conductivity, higher specific capacity, and good compatibility with electrolytes. In addition, hard carbon has a larger interlayer spacing than graphite (the former is 0.36nm to 0.38nm, and the latter is 0.33nm), so the diffusion rate of lithium ions in its interlayer is faster. However, hard carbon has a large specific surface area, which will cause serious decomposition of the electrolyte on its surface, and thus the first coulomb efficiency is greatly reduced. The present invention uses particles with oxygen-containing groups on the surface as activators, and its oxygen-containing groups can activate soft carbon coating agents to convert them into hard carbon structures after carbonization, and further discharge volatile substances on the surface during the subsequent graphitization process, which can reduce the specific area, thereby improving the first coulomb efficiency. At the same time, the nitrogen source can be nitrogen-doped on the surface of artificial graphite after carbonization, thereby providing active sites for rapid deintercalation of lithium ions, so that the energy density and fast charging performance are excellent.

[0015] In some embodiments, the soft carbon-based coating agent is solid-phase asphalt and / or liquid-phase asphalt.

[0016] In some embodiments, the coking value of the soft carbon-based coating agent is 10% to 80%.

[0017] In some embodiments, the nitrogen source is at least one of melamine, urea, and dopamine.

[0018] In some embodiments, the activator is at least one of potassium hydroxide, sodium hydroxide, calcium carbonate, and magnesium oxide.

[0019] In some embodiments, the raw materials for preparing the coating body further include a pore-forming aid, and the pore-forming aid is at least one of coal tar, resin and aromatic oil.

[0020] In some embodiments, the mass ratio of the soft carbon coating agent, the activating agent and the nitrogen source is 18.2-66.6:15.2-37.5:0.5-10.0.

[0021] In some embodiments, the grinding device is a ball mill, and the ball milling time is 8 hours to 20 hours.

[0022] In some embodiments, the mixing equipment used in step (I) for preparing the coating is a fusion machine or a VC mixer, and the mixing time is 30 min to 180 min.

[0023] In some embodiments, the artificial graphite precursor is shaped petroleum coke or coal-based coke.

[0024] In some embodiments, the artificial graphite precursor has a Dv50 of 2 μm to 50 μm and a carbon content of ≥99%.

[0025] In some embodiments, the mass ratio of the coating body to the artificial graphite precursor is 5-15:85-95.

[0026] In some embodiments, the mixing device used in step (II) of preparing the precursor is a fusion machine or a VC mixer, and the mixing time is 60 min to 240 min.

[0027] In some embodiments, the precursor is carbonized in an inert atmosphere, and the flow rate of the inert atmosphere is 0.5 L / min to 20.0 L / min.

[0028] In some embodiments, the equipment used for carbonization is a roller kiln, a rotary kiln, a box furnace or a vertical kettle.

[0029] In some embodiments, the carbonization temperature is increased in a gradient manner, and the maximum temperature is increased to 800° C. to 900° C.

[0030] In some embodiments, the temperature ramp rate for carbonization is 1° C. / min to 5° C. / min.

[0031] In some embodiments, the carbonization temperature is first increased to 250° C. to 300° C., then increased to 300° C. to 480° C., and then to 480° C. to 850° C., and then maintained.

[0032] In some embodiments, the holding time is 120 min to 300 min.

[0033] In some embodiments, the post-treatment includes cooling the carbonized product to room temperature and then sequentially performing acid washing, filtering, drying, breaking up, screening, and graphitization.

[0034] In some embodiments, the solution used for pickling is hydrochloric acid, nitric acid or hydrofluoric acid.

[0035] In some embodiments, the filtering method is suction filtration, centrifugation or pressure filtration.

[0036] In some embodiments, the drying device is an oven or a dryer, the drying temperature is 60° C. to 160° C., and the drying time is 1 hour to 48 hours.

[0037] In some embodiments, the device used for breaking up is a disaggregation break-up machine.

[0038] In some embodiments, the equipment used for graphitization is an Acheson graphitization furnace, an inner string graphitization furnace, a box-type graphitization furnace, a vacuum graphitization furnace, or a continuous graphitization furnace.

[0039] To achieve the above objectives, the second aspect of the present invention provides a method for preparing a hard carbon-coated graphite composite material. The hard carbon-coated graphite composite material prepared by the method has a first reversible specific capacity of not less than 350 mAh / g and a first coulombic efficiency of ≥88%.

[0040] The hard carbon-coated graphite composite material of the present invention is an artificial graphite with nitrogen doping and a hard carbon coating layer. It has a low specific surface area, better first reversible specific capacity, first coulombic efficiency and fast charging performance, and has excellent product performance, and is expected to be mass-produced and used in commercial fast-charging graphite negative electrode materials.

[0041] The present invention also provides an application of the hard carbon-coated graphite composite material in a negative electrode material. The hard carbon-coated graphite composite material is used as a negative electrode active material to meet the requirements of batteries for energy storage devices. DETAILED DESCRIPTION

[0042] The hard carbon-coated graphite composite material of the present invention can be used as a negative electrode active material in lithium ion batteries, sodium ion batteries or supercapacitors, etc. It can be used alone as a negative electrode active material, or it can be mixed with other negative electrode active materials (such as silicon-based negative electrode active materials, natural graphite, artificial graphite, etc.). The hard carbon-coated graphite composite material of the present invention itself has good electrical conductivity, so it can be selected to add or not add a conductive agent according to actual use.

[0043] The hard carbon-coated graphite composite material of the present invention comprises artificial graphite and a nitrogen-doped hard carbon coating layer coated on the surface of the artificial graphite. The first reversible specific capacity of the hard carbon-coated graphite composite material is not less than 350 mAh / g, and specifically can be but not limited to 350 mAh / g, 351 mAh / g, 352 mAh / g, 353 mAh / g, 354 mAh / g, 355 mAh / g, 356 mAh / g, 357 mAh / g, 358 mAh / g. The first coulombic efficiency is ≥ 88%, and specifically can be but not limited to 88%, 89%, 90%, 91%, 92%, 93%, 94%, 95%.

[0044] The method for preparing the hard carbon-coated graphite composite material of the present invention comprises the steps of (I) preparing a coating body, (II) preparing a precursor and (III) carbonization treatment.

[0045] Wherein, step (I) of preparing the coating body comprises grinding and mixing a soft carbon coating agent, an activator and a nitrogen source to form a coating body, wherein the activator is a particle having oxygen-containing groups on the surface.

[0046] As one embodiment, the mass ratio of the soft carbon coating agent, the activator and the nitrogen source is 18.2-66.6:15.2-37.5:0.5-10.0. As an example, the mass ratio may be but is not limited to 25:25:1, 35:25:1, 45:25:1, 55:25:1, 65:25:1, 35:25:10, 35:16:10, 35:35:10, 45:20:10, 45:16:30, 55:35:10, 25:25:0.5, 35:25:1.5, 45:25:2, 55:25:3, 65:25:4, 35:25:5, 35:16:6, 35:35:7, 45:20:8, 45:16:9, and 60:35:10.

[0047] As an embodiment, the soft carbon coating agent is solid phase asphalt and / or liquid phase asphalt, and the coking value is 10% to 80%, as some embodiments, the coking value is 30% to 80%, as some embodiments, the coking value is 50% to 80%. The coking value can be specifically but not limited to 10%, 20%, 30%, 40%, 50%, 60%, 70%, 80%.

[0048] As an embodiment, the activator is at least one of potassium hydroxide, sodium hydroxide, calcium carbonate and magnesium oxide, and as an example, the activator is potassium hydroxide. During the preparation process of such substances, the particles inevitably have surface groups, such as phenolic groups, ether groups, carbonyl groups and other oxygen-containing groups, and some contain some acidic groups, so they can be used as activators to provide oxygen components to help the soft carbon coating agent to be converted from soft carbon to hard carbon structure after carbonization.

[0049] As an embodiment, the nitrogen source is at least one of melamine, urea and dopamine. These nitrogen-containing substances can form a three-dimensional network structure before carbonization. After sintering, the nitrogen atoms are combined in the complex mesh structure, which can improve the conductivity of the material. Therefore, the obtained hard carbon-coated graphite composite material can have a better first efficiency.

[0050] As an embodiment, the raw material for preparing the coating body also includes a pore-forming aid, which is at least one of coal tar, resin and aromatic oil. Such substances form hard carbon materials before carbonization and can play a pore-forming role during the activation process to increase the porosity of the hard carbon-coated graphite composite material, thereby improving the dynamic properties of the material.

[0051] As an embodiment, the grinding equipment is a ball mill, and the ball milling time is 8h to 20h, specifically but not limited to 8h, 9h, 10h, 11h, 12h, 13h, 14h, 15h, 16h, 17h, 18h, 19h, 20h. As an example, the ball milling time is 12h.

[0052] As an embodiment, the equipment used for mixing in preparing the coating in step (I) is a fusion machine or a VC mixer. The fusion machine can be a room temperature fusion machine or a heated fusion machine, including but not necessarily limited to a VC mixer.

[0053] The mixing time is 30 min to 180 min, specifically but not limited to 30 min, 40 min, 50 min, 60 min, 70 min, 80 min, 90 min, 100 min, 110 min, 120 min, 130 min, 140 min, 150 min, 160 min, 170 min, 180 min. As an example, the mixing time is 90 min.

[0054] Wherein, the step (II) of preparing the precursor comprises mixing the coating body and the artificial graphite precursor.

[0055] As an embodiment, the artificial graphite precursor is petroleum coke or coal-based coke after shaping, and the equipment used for shaping can be a spheroidizing shaping machine. The Dv50 of the artificial graphite precursor is 2μm to 50μm. As some embodiments, the Dv50 of the artificial graphite precursor is 2μm to 30μm. As some embodiments, the Dv50 of the artificial graphite precursor is 8μm to 11μm. The Dv50 of the artificial graphite precursor can be, but is not limited to, 2μm, 4μm, 5μm, 8μm, 10μm, 12μm, 16μm, 20μm, 24μm, 28μm, 30μm, 35μm, 40μm, 43μm, 48μm 50μm. The carbon content of the artificial graphite precursor is ≥99%. As some embodiments, the carbon content of the artificial graphite precursor is ≥99.9%. The carbon content of the artificial graphite precursor may be, but is not limited to, 99.1%, 99.2%, 99.3%, 99.4%, 99.5%, 99.6%, 99.7%, 99.8%, 99.9%, 99.91%, 99.92%, 99.93%, 99.94%, 99.95%, 99.96%, 99.97%, 99.98%, and 99.99%.

[0056] As an embodiment, the mass ratio of the coating body and the artificial graphite precursor is 5-15:85-95. As an example, the weight ratio may be but is not limited to 5:95, 6:94, 7:93, 8:92, 9:91, 10:90, 11:89, 12:88, 13:87, 14:86, 15:85.

[0057] As an embodiment, the equipment used for mixing in the preparation of the precursor in step (II) is a fusion machine or a VC mixer, and the fusion machine can be a room temperature fusion machine or a heated fusion machine, including but not limited to a VC mixer. The mixing time is 60min to 240min, and specifically can be but not limited to 60min, 70min, 80min, 90min, 100min, 110min, 120min, 130min, 140min, 150min, 160min, 170min, 180min, 190min, 200min, 210min, 220min, 230min, 240min. As an example, the mixing time is 120min.

[0058] Wherein, the carbonization treatment in step (III) comprises carbonizing the precursor to obtain a carbonized product, and performing post-treatment on the carbonized product, wherein the post-treatment at least comprises graphitizing the carbonized product.

[0059] As an embodiment, the precursor is carbonized in an inert atmosphere, and the inert atmosphere may be, but is not limited to, nitrogen, argon or helium. The flow rate of the inert atmosphere is 0.5 L / min to 20.0 L / min, and may be, but is not limited to, 0.5 L / min, 1 L / min, 1.5 L / min, 2.5 L / min, 3.5 L / min, 4.5 L / min, 5 L / min, 5.5 L / min, 6.5 L / min, 7.5 L / min, 8.5 L / min, 9.5 L / min, 11 L / min, 13 L / min, 15 L / min, 16 L / min, 7 L / min, 19 L / min, 20.0 L / min. As an example, the flow rate of the inert atmosphere is 5 L / min.

[0060] As an embodiment, the equipment used for carbonization is a roller kiln, a rotary kiln, a box furnace or a vertical kettle. As an example, the equipment used for carbonization is a roller kiln.

[0061] As an embodiment, the temperature of carbonization is increased by gradient, and the maximum temperature is increased to 800°C to 900°C, and the maximum temperature may be, but not limited to, 800°C, 810°C, 820°C, 830°C, 840°C, 850°C, 860°C, 870°C, 880°C, 890°C, and 900°C. The use of gradient heating is conducive to the conversion of soft carbon coating agents from soft carbon to hard carbon. The temperature increase rate of carbonization is 1°C / min to 5°C / min, and the heating rate may be, but not limited to, 1°C / min, 1.5°C / min, 2°C / min, 2.5°C / min, 3°C / min, 3.5°C / min, 4°C / min, 4.5°C / min, and 5°C / min. The carbonization temperature can be increased in four gradients. As an example, the carbonization temperature is first increased to 250°C to 300°C, then increased to 300°C to 480°C, and then to 480°C to 850°C, and then kept warm for 120min to 300min, specifically but not limited to 120min, 140min, 160min, 180min, 200min, 220min, 240min, 260min, 280min, and 300min.

[0062] As an embodiment, the post-treatment includes cooling the carbonized product to room temperature and then sequentially performing acid washing, filtering, drying, breaking up, screening and graphitization.

[0063] The solution used for pickling is hydrochloric acid, nitric acid or hydrofluoric acid, or a dilution of hydrochloric acid, nitric acid or hydrofluoric acid, and the pickling is to remove residual ions. The filtering method is suction filtration, centrifugation or filter pressing. The equipment used for drying is an oven or a dryer, and the temperature used for drying is 60°C to 160°C, and the drying temperature may be but not limited to 60°C, 70°C, 80°C, 90°C, 100°C, 110°C, 120°C, 130°C, 140°C, 150°C, 160°C. The drying time is 1h to 48h, and the drying time may be but not limited to 1h, 5h, 10h, 15h, 20h, 25h, 30h, 35h, 40h, 45h, 48h. The equipment used for disintegration is a disintegration disintegrator. Screening can pass through a 200-mesh sieve. The equipment used for graphitization is Acheson graphitization furnace, inner string graphitization furnace, box-type graphitization furnace, vacuum graphitization furnace or continuous graphitization furnace.

[0064] In order to better illustrate the purpose, technical scheme and beneficial effects of the present invention, the present invention will be further described below in conjunction with specific embodiments. It should be noted that the following implementation method is a further explanation of the present invention and should not be used as a limitation of the present invention.

[0065] Example 1

[0066] The method for preparing the hard carbon-coated graphite composite material of this embodiment includes the following steps.

[0067] (I) Preparation of coating

[0068] 13.2 kg of liquid asphalt (softening point of 280°C, coking value of 70%), 6.6 kg of KOH and 2.2 kg of dopamine were ground by a ball mill for 12 hours, and then mixed by a VC100 mixer at a speed of 200 r / min for 30 minutes to form a coating.

[0069] (II) Preparation of Precursor

[0070] 22 kg of the coated body and 200 kg of shaped petroleum coke A (Dv50 is 10 μm, carbon content ≥ 99%) were batch mixed in VC500 for 90 minutes to obtain a precursor.

[0071] (III) Carbonization treatment

[0072] The precursor was loaded into a carbonization crucible and then placed in a roller kiln for carbonization. Under the flow of 5 L / min nitrogen, the carbonization product was reacted according to the following heating method. After the carbonization product was cooled to room temperature, it was pickled with 2 mol / L hydrochloric acid and then washed with water until neutral, filtered, dried in an oven at 80°C for 3 h, depolymerized with VC500, and sieved through a 200-mesh sieve, and then graphitized in an Acheson graphitization furnace.

[0073] Heating method:

[0074] (1) First heating step: room temperature to 300 °C, heating rate 3 °C / min;

[0075] (2) Second heating step: the temperature rises to 480 °C, and the heating rate is 1.25 °C / min;

[0076] (3) The third heating step: the temperature rises to 850 °C, and the heating rate is 2.06 °C / min;

[0077] (4) Fourth heating step: 850°C for 180 min.

[0078] Example 2

[0079] The method for preparing the hard carbon-coated graphite composite material of this embodiment includes the following steps.

[0080] (I) Preparation of coating

[0081] 13.2 kg of liquid asphalt (softening point of 280°C, coking value of 70%), 6.6 kg of KOH and 2.2 kg of urea were ground by a ball mill for 12 hours, and then mixed by a VC100 mixer at a speed of 200 r / min for 30 minutes to form a coating.

[0082] (II) Preparation of Precursor

[0083] 22 kg of the coated body and 200 kg of shaped petroleum coke A (Dv50 is 10 μm, carbon content ≥ 99%) were batch mixed in VC500 for 90 minutes to obtain a precursor.

[0084] (III) Carbonization treatment

[0085] The precursor was loaded into a carbonization crucible and then placed in a roller kiln for carbonization. Under the flow of 5 L / min nitrogen, the carbonization product was reacted according to the following heating method. After the carbonization product was cooled to room temperature, it was pickled with 2 mol / L hydrochloric acid and then washed with water until neutral, filtered, dried in an oven at 80°C for 3 h, depolymerized with VC500, and sieved through a 200-mesh sieve, and then graphitized in an Acheson graphitization furnace.

[0086] Heating method:

[0087] (1) First heating step: room temperature to 300 °C, heating rate 3 °C / min;

[0088] (2) Second heating step: the temperature rises to 480 °C, and the heating rate is 1.25 °C / min;

[0089] (3) The third heating step: the temperature rises to 850 °C, and the heating rate is 2.06 °C / min;

[0090] (4) Fourth heating step: 850°C for 180 min.

[0091] Example 3

[0092] The method for preparing the hard carbon-coated graphite composite material of this embodiment includes the following steps.

[0093] (I) Preparation of coating

[0094] 15.0 kg of liquid asphalt (softening point of 280°C, coking value of 70%), 6.6 kg of KOH and 0.44 kg of urea were ground by a ball mill for 12 hours, and then mixed by a VC100 mixer at a speed of 200 r / min for 30 minutes to form a coating.

[0095] (II) Preparation of Precursor

[0096] 22 kg of the coated body and 200 kg of shaped petroleum coke A (Dv50 is 10 μm, carbon content ≥ 99%) were batch mixed in VC500 for 90 minutes to obtain a precursor.

[0097] (III) Carbonization treatment

[0098] The precursor was loaded into a carbonization crucible and then placed in a roller kiln for carbonization. Under the flow of 5 L / min nitrogen, the carbonization product was reacted according to the following heating method. After the carbonization product was cooled to room temperature, it was pickled with 2 mol / L hydrochloric acid and then washed with water until neutral, filtered, dried in an oven at 80°C for 3 h, depolymerized with VC500, and sieved through a 200-mesh sieve, and then graphitized in an Acheson graphitization furnace.

[0099] Heating method:

[0100] (1) First heating step: room temperature to 300 °C, heating rate 3 °C / min;

[0101] (2) Second heating step: the temperature rises to 480 °C, and the heating rate is 1.25 °C / min;

[0102] (3) The third heating step: the temperature rises to 850 °C, and the heating rate is 2.06 °C / min;

[0103] (4) Fourth heating step: 850°C for 180 min.

[0104] Example 4

[0105] The method for preparing the hard carbon-coated graphite composite material of this embodiment includes the following steps.

[0106] (I) Preparation of coating

[0107] 11kg of liquid asphalt (softening point of 280°C, coking value of 70%), 2.2kg of coal tar (coking value of 66%), 6.6kg of KOH and 2.2kg of dopamine were ground by a ball mill for 12h, and then mixed by a VC100 mixer at a speed of 200r / min for 30min to form a coating.

[0108] (II) Preparation of Precursor

[0109] 22 kg of the coated body and 200 kg of shaped petroleum coke A (Dv50 is 10 μm, carbon content ≥ 99%) were batch mixed in VC500 for 90 minutes to obtain a precursor.

[0110] (III) Carbonization treatment

[0111] The precursor was loaded into a carbonization crucible and then placed in a roller kiln for carbonization. Under the flow of 5 L / min nitrogen, the carbonization product was reacted according to the following heating method. After the carbonization product was cooled to room temperature, it was pickled with 2 mol / L hydrochloric acid and then washed with water until neutral, filtered, dried in an oven at 80°C for 3 h, depolymerized with VC500, and sieved through a 200-mesh sieve, and then graphitized in an Acheson graphitization furnace.

[0112] Heating method:

[0113] (1) First heating step: room temperature to 300 °C, heating rate 3 °C / min;

[0114] (2) Second heating step: the temperature rises to 480 °C, and the heating rate is 1.25 °C / min;

[0115] (3) The third heating step: the temperature rises to 850 °C, and the heating rate is 2.06 °C / min;

[0116] (4) Fourth heating step: 850°C for 180 min.

[0117] Example 5

[0118] The method for preparing the hard carbon-coated graphite composite material of this embodiment includes the following steps.

[0119] (I) Preparation of coating

[0120] 11kg of liquid asphalt (softening point of 280°C, coking value of 70%), 2.2kg of coal tar (coking value of 66%), 6.6kg of KOH and 2.2kg of urea were ground by a ball mill for 12 hours, and then mixed by a VC100 mixer at a speed of 200r / min for 30 minutes to form a coating.

[0121] (II) Preparation of Precursor

[0122] 22 kg of the coated body and 200 kg of shaped petroleum coke A (Dv50 is 10 μm, carbon content ≥ 99%) were batch mixed in VC500 for 90 minutes to obtain a precursor.

[0123] (III) Carbonization treatment

[0124] The precursor was loaded into a carbonization crucible and then placed in a roller kiln for carbonization. Under the flow of 5 L / min nitrogen, the carbonization product was reacted according to the following heating method. After the carbonization product was cooled to room temperature, it was pickled with 2 mol / L hydrochloric acid and then washed with water until neutral, filtered, dried in an oven at 80°C for 3 h, depolymerized with VC500, and sieved through a 200-mesh sieve, and then graphitized in an Acheson graphitization furnace.

[0125] Heating method:

[0126] (1) First heating step: room temperature to 300 °C, heating rate 3 °C / min;

[0127] (2) Second heating step: the temperature rises to 480 °C, and the heating rate is 1.25 °C / min;

[0128] (3) The third heating step: the temperature rises to 850 °C, and the heating rate is 2.06 °C / min;

[0129] (4) Fourth heating step: 850°C for 180 min.

[0130] Example 6

[0131] The method for preparing the hard carbon-coated graphite composite material of this embodiment includes the following steps.

[0132] (I) Preparation of coating

[0133] 12.0 kg of liquid asphalt (softening point of 280 ° C, coking value of 70%), 3 kg of coal tar (coking value of 66%), 6.6 kg of KOH and 2.2 kg of urea were ground by a ball mill for 12 hours, and then mixed by a VC100 mixer at a speed of 200 r / min for 30 minutes to form a coating.

[0134] (II) Preparation of Precursor

[0135] 22 kg of the coated body and 200 kg of shaped petroleum coke A (Dv50 is 10 μm, carbon content ≥ 99%) were batch mixed in VC500 for 90 minutes to obtain a precursor.

[0136] (III) Carbonization treatment

[0137] The precursor was loaded into a carbonization crucible and then placed in a roller kiln for carbonization. Under the flow of 5 L / min nitrogen, the carbonization product was reacted according to the following heating method. After the carbonization product was cooled to room temperature, it was pickled with 2 mol / L hydrochloric acid and then washed with water until neutral, filtered, dried in an oven at 80°C for 3 h, depolymerized with VC500, and sieved through a 200-mesh sieve, and then graphitized in an Acheson graphitization furnace.

[0138] Heating method:

[0139] (1) First heating step: room temperature to 300 °C, heating rate 3 °C / min;

[0140] (2) Second heating step: the temperature rises to 480 °C, and the heating rate is 1.25 °C / min;

[0141] (3) The third heating step: the temperature rises to 850 °C, and the heating rate is 2.06 °C / min;

[0142] (4) Fourth heating step: 850°C for 180 min.

[0143] Example 7

[0144] The method for preparing the hard carbon-coated graphite composite material of this embodiment includes the following steps.

[0145] (I) Preparation of coating

[0146] 13.2 kg of liquid asphalt (softening point of 280° C., coking value of 70%), 6.6 kg of KOH and 2.2 kg of melamine were ground by a ball mill for 12 hours, and then mixed by a VC100 mixer at a speed of 200 r / min for 30 minutes to form a coating.

[0147] (II) Preparation of Precursor

[0148] 22 kg of the coated body and 200 kg of shaped petroleum coke A (Dv50 is 10 μm, carbon content ≥ 99%) were batch mixed in VC500 for 90 minutes to obtain a precursor.

[0149] (III) Carbonization treatment

[0150] The precursor was loaded into a carbonization crucible and then placed in a roller kiln for carbonization. Under the flow of 5 L / min nitrogen, the carbonization product was reacted according to the following heating method. After the carbonization product was cooled to room temperature, it was pickled with 2 mol / L hydrochloric acid and then washed with water until neutral, filtered, dried in an oven at 80°C for 3 h, depolymerized with VC500, and sieved through a 200-mesh sieve, and then graphitized in an Acheson graphitization furnace.

[0151] Heating method:

[0152] (1) First heating step: room temperature to 300 °C, heating rate 3 °C / min;

[0153] (2) Second heating step: the temperature rises to 480 °C, and the heating rate is 1.25 °C / min;

[0154] (3) The third heating step: the temperature rises to 850 °C, and the heating rate is 2.06 °C / min;

[0155] (4) Fourth heating step: 850°C for 180 min.

[0156] Example 8

[0157] The method for preparing the hard carbon-coated graphite composite material of this embodiment includes the following steps.

[0158] (I) Preparation of coating

[0159] 15.0 kg of liquid asphalt (softening point of 280° C., coking value of 70%), 6.6 kg of KOH and 0.44 kg of melamine were ground by a ball mill for 12 hours, and then mixed by a VC100 mixer at a speed of 200 r / min for 30 minutes to form a coating.

[0160] (II) Preparation of Precursor

[0161] 22 kg of the coated body and 200 kg of shaped petroleum coke A (Dv50 is 10 μm, carbon content ≥ 99%) were batch mixed in VC500 for 90 minutes to obtain a precursor.

[0162] (III) Carbonization treatment

[0163] The precursor was loaded into a carbonization crucible and then placed in a roller kiln for carbonization. Under the flow of 5 L / min nitrogen, the carbonization product was reacted according to the following heating method. After the carbonization product was cooled to room temperature, it was pickled with 2 mol / L hydrochloric acid and then washed with water until neutral, filtered, dried in an oven at 80°C for 3 h, depolymerized with VC500, and sieved through a 200-mesh sieve, and then graphitized in an Acheson graphitization furnace.

[0164] Heating method:

[0165] (1) First heating step: room temperature to 300 °C, heating rate 3 °C / min;

[0166] (2) Second heating step: the temperature rises to 480 °C, and the heating rate is 1.25 °C / min;

[0167] (3) The third heating step: the temperature rises to 850 °C, and the heating rate is 2.06 °C / min;

[0168] (4) Fourth heating step: 850°C for 180 min.

[0169] Example 9

[0170] The method for preparing the hard carbon-coated graphite composite material of this embodiment includes the following steps.

[0171] (I) Preparation of coating

[0172] 13.2 kg of liquid asphalt (softening point of 280°C, coking value of 70%), 6.6 kg of calcium carbonate and 2.2 kg of dopamine were ground by a ball mill for 12 hours, and then mixed by a VC100 mixer at a speed of 200 r / min for 30 minutes to form a coating.

[0173] (II) Preparation of Precursor

[0174] 22 kg of the coated body and 200 kg of shaped petroleum coke A (Dv50 is 10 μm, carbon content ≥ 99%) were batch mixed in VC500 for 90 minutes to obtain a precursor.

[0175] (III) Carbonization treatment

[0176] The precursor was loaded into a carbonization crucible and then placed in a roller kiln for carbonization. Under the flow of 5 L / min nitrogen, the carbonization product was reacted according to the following heating method. After the carbonization product was cooled to room temperature, it was pickled with 2 mol / L hydrochloric acid and then washed with water until neutral, filtered, dried in an oven at 80°C for 3 h, depolymerized with VC500, and sieved through a 200-mesh sieve, and then graphitized in an Acheson graphitization furnace.

[0177] Heating method:

[0178] (1) First heating step: room temperature to 300 °C, heating rate 3 °C / min;

[0179] (2) Second heating step: the temperature rises to 480 °C, and the heating rate is 1.25 °C / min;

[0180] (3) The third heating step: the temperature rises to 850 °C, and the heating rate is 2.06 °C / min;

[0181] (4) Fourth heating step: 850°C for 180 min.

[0182] Example 10

[0183] The method for preparing the hard carbon-coated graphite composite material of this embodiment includes the following steps.

[0184] (I) Preparation of coating

[0185] 13.2 kg of liquid asphalt (softening point of 280°C, coking value of 70%), 6.6 kg of magnesium oxide and 2.2 kg of dopamine were ground by a ball mill for 12 hours, and then mixed by a VC100 mixer at a speed of 200 r / min for 30 minutes to form a coating.

[0186] (II) Preparation of Precursor

[0187] 22 kg of the coated body and 200 kg of shaped petroleum coke A (Dv50 is 10 μm, carbon content ≥ 99%) were batch mixed in VC500 for 90 minutes to obtain a precursor.

[0188] (III) Carbonization treatment

[0189] The precursor was loaded into a carbonization crucible and then placed in a roller kiln for carbonization. Under the flow of 5 L / min nitrogen, the carbonization product was reacted according to the following heating method. After the carbonization product was cooled to room temperature, it was pickled with 2 mol / L hydrochloric acid and then washed with water until neutral, filtered, dried in an oven at 80°C for 3 h, depolymerized with VC500, and sieved through a 200-mesh sieve, and then graphitized in an Acheson graphitization furnace.

[0190] Heating method:

[0191] (1) First heating step: room temperature to 300 °C, heating rate 3 °C / min;

[0192] (2) Second heating step: the temperature rises to 480 °C, and the heating rate is 1.25 °C / min;

[0193] (3) The third heating step: the temperature rises to 850 °C, and the heating rate is 2.06 °C / min;

[0194] (4) Fourth heating step: 850°C for 180 min.

[0195] Embodiment 11

[0196] The method for preparing the hard carbon-coated graphite composite material of this embodiment includes the following steps.

[0197] (I) Preparation of coating

[0198] 13.2 kg of solid asphalt (softening point of 250°C, coking value of 77%), 6.6 kg of KOH and 2.2 kg of dopamine were ground by a ball mill for 18 hours, and then mixed by a heating fusion machine at a speed of 250 r / min for 100 minutes to form a coating.

[0199] (II) Preparation of Precursor

[0200] 22 kg of the coated body and 200 kg of shaped coal-based coke (Dv50 is 30 μm, carbon content ≥ 99.9%) were batch mixed in VC500 for 150 minutes to obtain a precursor.

[0201] (III) Carbonization treatment

[0202] The precursor was loaded into a carbonization crucible and then placed in a roller kiln for carbonization. Under the flow of 10 L / min nitrogen, the carbonization product was reacted according to the following heating method. After the carbonization product was cooled to room temperature, it was acid-washed with 1 mol / L nitric acid and then washed with water until neutral, filtered, dried in an oven at 80°C for 3 h, depolymerized with VC500, and sieved through a 200-mesh sieve, and then graphitized in an Acheson graphitization furnace.

[0203] Heating method:

[0204] (1) First heating step: room temperature to 300 °C, heating rate 3 °C / min;

[0205] (2) Second heating step: the temperature rises to 480 °C, and the heating rate is 1.25 °C / min;

[0206] (3) The third heating step: the temperature rises to 850 °C, and the heating rate is 2.06 °C / min;

[0207] (4) Fourth heating step: 850°C for 180 min.

[0208] Example 12

[0209] The method for preparing the hard carbon-coated graphite composite material of this embodiment includes the following steps.

[0210] (I) Preparation of coating

[0211] 25 kg of liquid asphalt (softening point of 250°C, coking value of 77%), 20 kg of KOH and 3 kg of dopamine were ground by a ball mill for 12 hours, and then mixed by a VC100 mixer at a speed of 250 r / min for 30 minutes to form a coating.

[0212] (II) Preparation of Precursor

[0213] 15 kg of the coated body and 90 kg of shaped petroleum coke A (Dv50 is 10 μm, carbon content ≥ 99%) were batch mixed in VC500 for 90 minutes to obtain a precursor.

[0214] (III) Carbonization treatment

[0215] The precursor was loaded into a carbonization crucible and then placed in a roller kiln for carbonization. Under the flow of 5 L / min nitrogen, the carbonization product was reacted according to the following heating method. After the carbonization product was cooled to room temperature, it was pickled with 1 mol / L hydrofluoric acid and then washed with water until neutral, filtered, dried in an oven at 100°C for 4 h, depolymerized with VC500, and sieved through a 200-mesh sieve, and then graphitized in an Acheson graphitization furnace.

[0216] Heating method:

[0217] (1) First heating step: room temperature to 300 °C, heating rate 3 °C / min;

[0218] (2) Second heating step: the temperature rises to 480 °C, and the heating rate is 1.25 °C / min;

[0219] (3) The third heating step: the temperature rises to 850 °C, and the heating rate is 2.06 °C / min;

[0220] (4) Fourth heating step: 850°C for 180 min.

[0221] Embodiment 13

[0222] The method for preparing the hard carbon-coated graphite composite material of this embodiment includes the following steps.

[0223] (I) Preparation of coating

[0224] 13.2 kg of liquid asphalt (softening point of 280°C, coking value of 70%), 6.6 kg of KOH and 2.2 kg of dopamine were ground by a ball mill for 12 hours, and then mixed by a VC100 mixer at a speed of 200 r / min for 30 minutes to form a coating.

[0225] (II) Preparation of Precursor

[0226] 22 kg of the coated body and 200 kg of shaped petroleum coke A (Dv50 is 10 μm, carbon content ≥ 99%) were batch mixed in VC500 for 90 minutes to obtain a precursor.

[0227] (III) Carbonization treatment

[0228] The precursor was loaded into a carbonization crucible and then placed in a roller kiln for carbonization. Under the flow of 5 L / min nitrogen, the carbonization product was reacted according to the following heating method. After the carbonization product was cooled to room temperature, it was pickled with 2 mol / L hydrochloric acid and then washed with water until neutral, filtered, dried in an oven at 80°C for 3 h, depolymerized with VC500, and sieved through a 200-mesh sieve, and then graphitized in an Acheson graphitization furnace.

[0229] Heating method:

[0230] (1) First heating step: room temperature to 300 °C, heating rate 3 °C / min;

[0231] (2) Second heating step: the temperature rises to 450 °C, and the heating rate is 1.5 °C / min;

[0232] (3) The third heating step: the temperature rises to 550 °C, and the heating rate is 1.25 °C / min;

[0233] (4) Fourth heating step: the temperature rises to 800 °C, and the heating rate is 2.5 °C / min;

[0234] (5) Fifth heating step: 800°C for 200 min.

[0235] Embodiment 14

[0236] The method for preparing the hard carbon-coated graphite composite material of this embodiment includes the following steps.

[0237] (I) Preparation of coating

[0238] 13.2 kg of liquid asphalt (softening point of 280°C, coking value of 70%), 6.6 kg of KOH and 2.2 kg of dopamine were ground by a ball mill for 12 hours, and then mixed by a VC100 mixer at a speed of 200 r / min for 30 minutes to form a coating.

[0239] (II) Preparation of Precursor

[0240] 22 kg of the coated body and 200 kg of shaped petroleum coke A (Dv50 is 10 μm, carbon content ≥ 99%) were batch mixed in VC500 for 90 minutes to obtain a precursor.

[0241] (III) Carbonization treatment

[0242] The precursor was loaded into a carbonization crucible and then placed in a roller kiln for carbonization. Under the flow of 5L / min nitrogen, the temperature was raised from room temperature to 850°C at a heating rate of 2.5°C / min, and the reaction was carried out for 180 minutes to obtain a carbonized product. After the carbonized product was cooled to room temperature, it was pickled with 2mol / L hydrochloric acid and then washed with water to neutrality, filtered, dried in an oven at 80°C for 3h, depolymerized with VC500, and sieved through a 200-mesh sieve, and then graphitized in an Acheson graphitization furnace.

[0243] Comparative Example 1

[0244] The method for preparing the hard carbon-coated graphite composite material of this embodiment includes the following steps.

[0245] (I) Preparation of Precursor

[0246] 22 kg of liquid asphalt (softening point of 280°C, coking value of 70%) and 200 kg of shaped petroleum coke A (Dv50 of 10 μm, carbon content ≥99%) were batch mixed in VC500 for 90 minutes to obtain a precursor.

[0247] (II) Carbonization treatment

[0248] The precursor was loaded into a carbonization crucible and then placed in a roller kiln for carbonization. Under the flow of 5 L / min nitrogen, the carbonization product was reacted according to the following heating method. After the carbonization product was cooled to room temperature, it was pickled with 2 mol / L hydrochloric acid and then washed with water until neutral, filtered, dried in an oven at 80°C for 3 h, depolymerized with VC500, and sieved through a 200-mesh sieve, and then graphitized in an Acheson graphitization furnace.

[0249] Heating method:

[0250] (1) First heating step: room temperature to 300 °C, heating rate 3 °C / min;

[0251] (2) Second heating step: the temperature rises to 480 °C, and the heating rate is 1.25 °C / min;

[0252] (3) The third heating step: the temperature rises to 850 °C, the heating rate is 2.06 °C / min, and the duration is 180 min.

[0253] (4) Fourth heating step: 850°C for 180 min.

[0254] Comparative Example 2

[0255] The method for preparing the hard carbon-coated graphite composite material of this embodiment includes the following steps.

[0256] (I) Preparation of coating

[0257] 15.4 kg of liquid asphalt (softening point of 280° C., coking value of 70%) and 6.6 kg of KOH were ground by a ball mill for 12 hours, and then mixed by a VC100 mixer at a speed of 200 r / min for 30 minutes to form a coating.

[0258] (II) Preparation of Precursor

[0259] 22 kg of the coated body and 200 kg of shaped petroleum coke A (Dv50 is 10 μm, carbon content ≥ 99%) were batch mixed in VC500 for 90 minutes to obtain a precursor.

[0260] (III) Carbonization treatment

[0261] The precursor was loaded into a carbonization crucible and then placed in a roller kiln for carbonization. Under the flow of 5 L / min nitrogen, the carbonization product was reacted according to the following heating method. After the carbonization product was cooled to room temperature, it was pickled with 2 mol / L hydrochloric acid and then washed with water until neutral, filtered, dried in an oven at 80°C for 3 h, depolymerized with VC500, and sieved through a 200-mesh sieve, and then graphitized in an Acheson graphitization furnace.

[0262] Heating method:

[0263] (1) First heating step: room temperature to 300 °C, heating rate 3 °C / min;

[0264] (2) Second heating step: the temperature rises to 480 °C, and the heating rate is 1.25 °C / min;

[0265] (3) The third heating step: the temperature rises to 850 °C, the heating rate is 2.06 °C / min, and the duration is 180 min.

[0266] (4) Fourth heating step: 850°C for 180 min.

[0267] Comparative Example 3

[0268] The method for preparing the hard carbon-coated graphite composite material of this embodiment includes the following steps.

[0269] (I) Preparation of coating

[0270] 19.8 kg of liquid asphalt (softening point of 280° C., coking value of 70%) and 2.2 kg of dopamine were ground by a ball mill for 12 hours, and then mixed by a VC100 mixer at a speed of 200 r / min for 30 minutes to form a coating.

[0271] (II) Preparation of Precursor

[0272] 22 kg of the coated body and 200 kg of shaped petroleum coke A (Dv50 is 10 μm, carbon content ≥ 99%) were batch mixed in VC500 for 90 minutes to obtain a precursor.

[0273] (III) Carbonization treatment

[0274] The precursor was loaded into a carbonization crucible and then placed in a roller kiln for carbonization. Under the flow of 5 L / min nitrogen, the carbonization product was reacted according to the following heating method. After the carbonization product was cooled to room temperature, it was pickled with 2 mol / L hydrochloric acid and then washed with water until neutral, filtered, dried in an oven at 80°C for 3 h, depolymerized with VC500, and sieved through a 200-mesh sieve, and then graphitized in an Acheson graphitization furnace.

[0275] Heating method:

[0276] (1) First heating step: room temperature to 300 °C, heating rate 3 °C / min;

[0277] (2) Second heating step: the temperature rises to 480 °C, and the heating rate is 1.25 °C / min;

[0278] (3) The third heating step: the temperature rises to 850 °C, the heating rate is 2.06 °C / min, and the duration is 180 min.

[0279] (4) Fourth heating step: 850°C for 180 min.

[0280] The hard carbon-coated graphite composite materials obtained in Examples 1 to 14 and Comparative Examples 1 to 3 were respectively measured for their average particle size Dv50 using a particle size analyzer, and their specific surface area was measured using a Micromeritics Surface Area Analyzer 3020. The results are shown in Table 1.

[0281] The hard carbon-coated graphite composite materials obtained in Examples 1 to 14 and Comparative Examples 1 to 3 were respectively used as negative electrode active materials, and were evenly mixed with polyvinylidene fluoride and conductive carbon black Super-P in a mass ratio of 70:15:15. An appropriate amount of N-methylpyrrolidone was added as a solvent to form a slurry and applied on a copper foil. The coated negative electrode sheet was placed in a vacuum drying oven at a temperature of 110°C and vacuum dried for 4 hours, and then roll-pressed to prepare a negative electrode sheet.

[0282] A metal lithium sheet was used as the counter electrode, the electrolyte was 1M LiPF6+EC:DEC:DMC=1:1:1 (volume ratio), and a polypropylene microporous membrane was used as the separator. The button cell was assembled into a CR2032 button cell in a glove box filled with inert gas. The charge and discharge test of the button cell was carried out on the battery test system of Wuhan Blue Electric Electronics Co., Ltd. at room temperature, 0.1C constant current charge and discharge, and the charge and discharge voltage was limited to 0.005V to 1.5V. The first reversible specific capacity, first coulomb efficiency and cycle performance were tested. The test results are shown in Table 1.

[0283] Table 1 Physical properties and electrochemical properties of graphite-based negative electrode materials obtained in each group of examples

[0284]

[0285]

[0286] It can be seen from the results in Table 1 that compared with comparative examples 1 to 3, in the preparation method of the hard carbon-coated graphite composite material of embodiments 1 to 11 of the present invention, by using oxygen-containing group-containing particles as an activator and combining nitrogen source coating, a nitrogen-doped and hard carbon-coated graphite composite material can be obtained, which has a low specific surface area and has better first reversible specific capacity, first coulombic efficiency and fast charging performance.

[0287] By comparing Examples 1, 2, and 7, it can be seen that when the nitrogen-containing compound is melamine, the 500-week capacity retention performance is better. This may be related to the fact that melamine contains more nitrogen per unit mass than the other two dopants, making it easier to dope N into the graphite and hard carbon surfaces, thereby improving the conductivity of the material. The high nitrogen content provides more reactive sites, thereby obtaining a higher specific capacity.

[0288] By comparing Examples 1, 9, and 10, it can be seen that when the activator is KOH, the 500-week capacity retention performance is better. This may be related to the chemical reaction between KOH and the asphalt surface, and the combination to generate relatively stable oxygen-containing groups, thereby making the produced hard carbon structure the most stable.

[0289] From comparative examples 1, 13 and 14, it can be seen that the graphite composite material obtained by adopting gradient heating during carbonization is better, which may be because the gradient heating is conducive to the conversion of the soft carbon coating agent from soft carbon to hard carbon.

[0290] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit the scope of protection of the present invention. Although the present invention is described in detail with reference to the preferred embodiments, it is not limited to those listed in the embodiments. Those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the essence and scope of the technical solution of the present invention.

Claims

1. Preparation method of hard carbon-coated graphite composite material, It is characterized in that Includes steps: (I) Preparation of coating Grinding and mixing a soft carbon coating agent, an activator and a nitrogen source to form a coating body, wherein the soft carbon coating agent is solid phase asphalt and / or liquid phase asphalt, the nitrogen source is at least one of melamine, urea and dopamine, and the activator is a particle having oxygen-containing groups on the surface; (II) Preparation of Precursor Mixing the coating body and an artificial graphite precursor to obtain a precursor; (III) Carbonization treatment The precursor is carbonized to obtain a carbonized product, and the carbonized product is post-processed. The post-processing at least includes graphitizing the carbonized product. The carbonization temperature is increased by a gradient.

2. The method for preparing the hard carbon-coated graphite composite material according to claim 1, It is characterized in that The invention comprises at least one of the following features (1) to (12): (1) The coking value of the soft carbon coating agent is 10% to 80%; (2) The activator is at least one of potassium hydroxide, sodium hydroxide, calcium carbonate and magnesium oxide; (3) The raw materials for preparing the coating body further include a pore-forming aid, and the pore-forming aid is at least one of coal tar, resin and aromatic oil; (4) The mass ratio of the soft carbon coating agent, the activating agent and the nitrogen source is 18.2-66.6:15.2-37.5:0.5-10.0; (5) The grinding equipment is a ball mill, and the ball milling time is 8h to 20h; (6) The mixing equipment used in step (I) of preparing the coating is a fusion machine or a VC mixer, and the mixing time is 30 min to 180 min; (7) The artificial graphite precursor is shaped petroleum coke or coal-based coke; (8) The Dv50 of the artificial graphite precursor is 2 μm to 50 μm, and the carbon content is ≥ 99%; (9) The mass ratio of the coating body to the artificial graphite precursor is 5-15:85-95; (10) The mixing equipment used in the step (II) of preparing the precursor is a fusion machine or a VC mixer, and the mixing time is 60 min to 240 min; (11) The precursor is carbonized in an inert atmosphere, and the flow rate of the inert atmosphere is 0.5 L / min to 20.0 L / min; (12) The equipment used for the carbonization is a roller kiln, a rotary kiln, a box furnace or a vertical kettle.

3. The method for preparing the hard carbon-coated graphite composite material according to claim 1, It is characterized in that The maximum temperature of the gradient heating is raised to 800°C to 900°C.

4. The method for preparing the hard carbon-coated graphite composite material according to claim 3, It is characterized in that The carbonization temperature rising rate is 1°C / min to 5°C / min.

5. The method for preparing the hard carbon-coated graphite composite material according to claim 3, It is characterized in that The carbonization temperature is first raised to 250° C. to 300° C., then raised to 300° C. to 480° C., and then raised to 480° C. to 850° C., and then kept warm.

6. The method for preparing the hard carbon-coated graphite composite material according to claim 5, It is characterized in that The insulation time is 120 min to 300 min.

7. The method for preparing the hard carbon-coated graphite composite material according to claim 1, It is characterized in that The post-treatment includes cooling the carbonized product to room temperature and then sequentially performing acid washing, filtering, drying, breaking up and screening, and graphitization.

8. The method for preparing the hard carbon-coated graphite composite material according to claim 7, It is characterized in that Includes at least one of the following features ① to ⑤: ① The solution used for pickling is hydrochloric acid, nitric acid or hydrofluoric acid; ② The filtering method is suction filtration, centrifugation or filter press; ③ The drying equipment is an oven or a dryer, the drying temperature is 60°C to 160°C, and the drying time is 1h to 48h; ④ The equipment used for the dispersing is a dispersing and dispersing machine; ⑤ The equipment used for the graphitization is an Acheson graphitization furnace, an inner string graphitization furnace, a box-type graphitization furnace, a vacuum graphitization furnace or a continuous graphitization furnace.

9. A hard carbon-coated graphite composite material prepared by the method for preparing a hard carbon-coated graphite composite material according to any one of claims 1 to 8, It is characterized in that The first reversible capacity is not less than 350mAh / g, and the first coulombic efficiency is ≥88%.

10. Use of the hard carbon-coated graphite composite material prepared by the method for preparing the hard carbon-coated graphite composite material according to any one of claims 1 to 8 or the hard carbon-coated graphite composite material according to claim 9 in negative electrode materials.