A method for improving laser shock spraying efficiency

By utilizing high-speed collision of pre-treated particles in laser shock spraying technology to form a boundary deposition area, combined with the principle of mechanical self-locking, the problems of low efficiency and high cost in laser shock spraying technology are solved, and more efficient coating deposition and quality are achieved. promote.

CN115673556BActive Publication Date: 2024-10-18NING XIA JU NENG ROBOTICS CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202211245086.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-10-12
Publication Date
2024-10-18
Estimated Expiration
2042-10-12

AI Technical Summary

Technical Problem

The processing frequency of laser shock spraying technology is high, resulting in low processing efficiency and reduced coating material deposition rate, resulting in material waste and increased economic costs.

Method used

The pretreatment particles impact the substrate surface at high speed to form a boundary deposition area, and the pure mechanical action generated by the laser shock wave is used to make the spray material and the substrate more closely combined. The mechanical self-locking principle is used to reduce rebound and diffusion phenomena and improve deposition efficiency.

Benefits of technology

It significantly improves the efficiency and coating quality of laser shock spraying, reduces processing frequency and cost, and avoids the use of chemical reagents and heat treatment, ensuring the purity and unchanged properties of the material.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115673556B_ABST
    Figure CN115673556B_ABST
Patent Text Reader

Abstract

The present invention provides a method for improving the efficiency of laser shock spraying. The method uses a method in which pretreated particles impact a substrate at high speed. On the one hand, plastic deformation can be formed on the substrate surface to generate a large residual compressive stress. When laser shock spraying is performed, the spraying material offsets most of the substrate rebound effect under the action of the laser normal shock wave. On the other hand, due to the erosion effect on the substrate surface during the high-speed impact of the pretreated particles, some high-speed pretreated particles form a deposition boundary layer on the substrate surface, and the substrate surface undergoes morphological changes to varying degrees. Since the pretreated particles and the spraying material are isotropic, effective deposition can be more efficiently formed at this interface during laser shock spraying. Therefore, the scheme can greatly improve the efficiency of laser shock coating preparation, make the coating and the substrate more compact, improve the coating quality, and reduce the processing frequency and processing cost.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of chemical technology, and in particular to a method for improving laser shock spraying efficiency. Background Art

[0002] Laser shock spraying technology for coating preparation has been around for less than 20 years, but it has gradually attracted attention from the academic community due to its advantages of high power density and no thermal effect.

[0003] However, the high frequency of processing links leads to reduced processing efficiency, which greatly affects the promotion of this technology. In addition, due to the radial and axial loads caused by the shock wave, the deposition rate of the coating material is reduced, resulting in a certain degree of waste and increasing economic costs.

[0004] At present, in order to improve the deposition efficiency of spraying materials, the commonly used treatment methods mainly include inorganic binder pre-coating and suspension drop coating. Although these two methods can fix the coating material on the surface of the substrate material to a certain extent, the bonding force between the substrate and the spraying material is limited, and the axial and radial power density generated by the laser can often exceed the gigawatt level, resulting in the spraying material cannot be completely deposited on the substrate surface to form a dense coating. The above process needs to be repeated continuously to effectively protect the substrate, which greatly reduces production efficiency and wastes a lot of spraying materials.

[0005] Therefore, a method for improving the processing efficiency of laser shock spraying and reducing the processing cost is needed. Summary of the invention

[0006] The present invention aims to solve the problem of how to reduce the rebound and diffusion of coating materials during laser impact spraying and increase the deposition efficiency of laser impact spraying, and provides a method for improving the efficiency of laser impact spraying. According to the mechanical self-locking principle of the coating material, the pure mechanical action generated by the laser shock wave is utilized to form a strong residual compressive stress at the interface between the substrate and the coating, so that the spraying material and the substrate are more closely combined. This process does not require the participation of chemical reagents and no heat treatment process. Not only will no processing impurities be introduced, but the material will not undergo phase change and change the material properties. Compared with the existing method, it can more effectively improve the processing efficiency.

[0007] The present invention provides a method for improving the efficiency of laser shock spraying, comprising the following steps:

[0008] S1. After grinding and polishing the surface of the substrate, ultrasonically clean it in an alcohol solution, and then dry it in a vacuum drying oven for later use. Prepare pre-treated particles and spray materials. The pre-treated particles are used to impact the substrate at high speed through laser impact to form a barrier deposition area. The spray materials are used for laser impact spraying. The pre-treated particles have the same composition as the spray materials but different particle sizes.

[0009] S2, placing the pretreated particles in a beaker containing an alcohol solution and stirring, using a dropper to absorb the suspension droplets and apply them to the surface of the substrate before the pretreated particles have settled, and allowing the suspension to spread on the surface of the substrate, and then placing the sample in a drying oven to evaporate and remove the surface alcohol to obtain a pretreated particle layer attached to the surface of the substrate; taking out the sample, and continuing to absorb the suspension droplets and apply them to the surface of the substrate until the thickness of the pretreated particle layer reaches more than twice the particle size of the pretreated particles, thereby obtaining a sample to be pretreated;

[0010] S3, covering the surface of the sample to be pretreated with aluminum foil, placing a constraint layer on the aluminum foil layer, and fixing it on a movable processing platform;

[0011] S4. According to the Hugo Neo elastic limit of the matrix material, the laser parameters are calculated by the Fabrro pressure model. A laser with a pressure load more than 2 times higher than the pre-treated particles HEL is used for a single impact. The pre-treated particles collide with the matrix at high speed under the action of the laser impact, causing the surface of the matrix to produce plastic deformation to the boundary deposition area. Some pre-treated particles are embedded in the matrix to form deposition. The boundary deposition area is a spray pre-treatment area with compressive stress and an uneven surface. The floating powder remaining on the surface of the matrix is ​​cleaned to obtain a pre-treated sample, and the pre-treatment is completed.

[0012] S5, using a press sheet to fix the spraying material on the surface of the boundary deposition area to obtain a sample to be sprayed;

[0013] S6. After covering the surface of the sample to be sprayed with aluminum foil and the constraint layer, fix it on a movable processing platform, adjust the laser parameters, and use a laser with a pressure load 2 to 5 times higher than the HEL of the spray material for single impact processing. The spray material partially offsets the rebound caused by the laser normal shock wave under the action of the compressive stress, and at the same time partially offsets the diffusion effect caused by the laser tangential shock wave under the action of the spray pretreatment area, so that the spray material and the boundary deposition area form a mechanical self-locking and combination;

[0014] S7, after removing the aluminum foil and the constraining layer, cleaning and drying are performed, and the laser shock spraying is completed.

[0015] The method for improving the efficiency of laser shock spraying described in the present invention is, as a preferred embodiment, in step S1, the particle size of the pre-treated particles is larger than the particle size of the spraying material.

[0016] In the method for improving the efficiency of laser impact spraying described in the present invention, as a preferred embodiment, the particle sizes of the spraying material and the pre-treated particles are both in the micron level, and the particle size of the pre-treated particles is more than twice the particle size of the spraying material;

[0017] In step S2, the thickness of the pretreated particle layer on the surface of the sample to be pretreated is 60-100 μm.

[0018] The method for improving the efficiency of laser shock spraying described in the present invention is, as a preferred embodiment, in step S1, the materials of the spraying material and the pre-treated particles are any one of the following: aluminum-based particles, titanium alloy particles and copper alloy particles.

[0019] The method for improving the efficiency of laser shock spraying described in the present invention is, as a preferred embodiment, in step S1, the material of the substrate is a metal material.

[0020] In the method for improving the efficiency of laser shock spraying described in the present invention, as a preferred embodiment, the material of the substrate is any one of the following: martensitic steel, stainless steel, copper, pure titanium and titanium alloy, aluminum alloy and copper-based alloy.

[0021] The method for improving the efficiency of laser impact spraying described in the present invention is preferably such that in step S1, the volume concentration of the alcohol solution is 75%, ultrasonic cleaning is performed for 5 minutes, the temperature of the vacuum drying oven is 90-100° C., and the drying time is 2-5 minutes;

[0022] In step S2, the temperature of the drying oven is 90-100°C, and the drying time is 2-5 minutes;

[0023] In step S7, after removing the aluminum foil and the constraining layer, the mixture is placed in an ultrasonic cleaning machine containing an alcohol solution with a volume concentration of 75% for 5 minutes, and then placed in a drying oven at 100° C. for drying for 2 to 5 minutes.

[0024] The method for improving the efficiency of laser shock spraying described in the present invention is, as a preferred embodiment, that in steps S3 and S6, the constrained layer is a light-transmitting material with a light transmittance higher than 90%, and the light-transmitting material includes water and K9 glass.

[0025] In the method for improving the efficiency of laser shock spraying described in the present invention, as a preferred embodiment, the laser generator used for laser shock spraying in steps S4 and S6 is a Nd:YaG laser generator.

[0026] The method for improving the efficiency of laser shock spraying described in the present invention is, as a preferred embodiment, in step S5, the material of the pressed sheet is tungsten steel.

[0027] The technical solution is as follows:

[0028] Step 1. Grind and polish the surface of the base material sample, then ultrasonically clean it in an alcohol solution, and finally place it in a vacuum drying oven for use;

[0029] Step 2. Place pretreated particles of the same nature with a diameter twice that of the spray material into a beaker filled with an alcohol solution with a volume concentration of 75%, stir thoroughly, and before the particles settle, use a dropper to absorb the suspension and apply it on the surface of the substrate to be sprayed. The mixed suspension containing the pretreated particles is dispersed and spread on the surface of the sample. Place the sample in a 100°C drying oven for 3 minutes to dry it and evaporate and remove the surface alcohol.

[0030] Step 3. Cover the surface of the sample with aluminum foil to prevent the sample surface from being damaged during the laser shock spraying process during the pretreatment process.

[0031] Step 4. Place K9 optical glass with a light transmittance greater than 90% on the aluminum foil layer as a constraint layer to reflect the reflected shock wave back to the sample surface to increase the impact efficiency.

[0032] Step 5. Fix the sample on a movable processing platform, calculate the laser parameters through the Fabrro pressure model according to the hugoniot elastic limit (HEL) of the base material, make its pressure load 2 times higher than the material HEL (60% to 80%), and perform a single impact. (During pre-processing, there is no spraying material on the surface, and it is not normal processing.)

[0033] Step 6. The surface of the substrate sample obtained from the above test forms an uneven boundary deposition area, and due to the existence of residual stress, a small amount of particles are embedded in this concave area of ​​the substrate. At this time, the aluminum-based particles to be sprayed (generally micron-sized) are fixed to the boundary deposition area on the surface of the substrate sample with a tungsten steel press.

[0034] Step 7. Cover the coating surface with aluminum foil and K9 glass layer by layer and fix them on a movable processing platform. Adjust the laser parameters again to make its power density 2.5 times higher than that of the material HEL. Perform a single laser impact processing on the coating area. After processing, remove the aluminum foil and glass on the surface. Place the sample in an ultrasonic cleaner containing a 75% alcohol solution by volume for 5 minutes, take it out and place it in a 100°C drying oven for three minutes to dry.

[0035] The present invention is mainly based on the mechanical self-locking principle of coating particles. It uses laser shock waves to spray pre-treated particles that are larger than the coating particles onto the surface of the substrate at high speed, forming a large degree of plastic deformation on the surface of the substrate, and the boundary layer formed by partially deposited pre-treated particles is isotropic with the spraying material. Subsequent processing can more efficiently form effective deposition at this interface. The recessed area formed by the deformation can effectively reduce the rebound effect of the coating particles during the experiment. The compressive stress generated by the surface pretreatment is used to achieve mechanical self-locking of the coating and improve processing efficiency.

[0036] The present invention has the following advantages:

[0037] The present invention uses a method for laser shock coating pre-treated particles and a method for high-speed impact of pre-treated particles on a substrate. On the one hand, plastic deformation can be formed on the substrate surface to generate a large residual compressive stress. When laser shock spraying is performed, the spraying material offsets most of the substrate rebound effect under the action of the laser normal shock wave. On the other hand, due to the erosion effect on the substrate surface during the high-speed impact of the pre-treated particles, some high-speed pre-treated particles are deposited on the substrate surface, causing the substrate surface to undergo varying degrees of morphological changes. When laser shock spraying is performed, the spraying material effectively offsets most of the diffusion effect of the tangential shock wave in this area, and the boundary layer formed by the partially deposited pre-treated particles is isotropic with the spraying material. Subsequent processing can more efficiently form effective deposition at this interface. Therefore, this solution can greatly improve the efficiency of laser shock coating preparation, make the coating and the substrate more compact, improve the coating quality, and reduce the processing frequency and processing cost. BRIEF DESCRIPTION OF THE DRAWINGS

[0038] Figure 1 A flow chart of a method for improving the efficiency of laser shock spraying;

[0039] Figure 2 Schematic diagram of steps S3 and S4 of a method for improving laser shock spraying efficiency;

[0040] Figure 3 A 3D topography image after step S4 of a method for improving laser shock spraying efficiency;

[0041] Figure 4 A partial enlarged view of the 3D morphology after step S4 of a method for improving laser shock spraying efficiency;

[0042] Figure 5 This is a method for improving the efficiency of laser impact spraying, showing the actual effect of the surface after pretreatment;

[0043] Figure 6a Surface effect diagram of Example 3 of a method for improving laser shock spraying efficiency;

[0044] Figure 6b This is a comparative surface effect diagram of Example 3 of a method for improving laser impact spraying efficiency. DETAILED DESCRIPTION

[0045] The technical solutions in the embodiments of the present invention will be described clearly and completely below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all the embodiments.

[0046] Example 1

[0047] like Figure 1 As shown, a method for improving the efficiency of laser shock spraying comprises the following steps:

[0048] S1. After grinding and polishing the surface of the substrate, ultrasonically clean it in an alcohol solution, and then dry it in a vacuum drying oven for later use. Prepare pre-treated particles and spraying materials. The pre-treated particles are used to impact the substrate at high speed by laser impact to form a barrier deposition area. The spraying material is used for laser impact spraying. The pre-treated particles have the same composition as the spraying material but different particle sizes. The particle size of the pre-treated particles is larger than that of the spraying material.

[0049] The particle sizes of the spraying material and pre-treated particles are both in the micron range, and the particle size of the pre-treated particles is more than twice that of the spraying material;

[0050] The materials of the spraying material and the pre-treated particles are any of the following: aluminum-based particles, titanium alloy particles and copper alloy particles; the material of the substrate is a metal material;

[0051] The material of the substrate is any one of the following: martensitic steel, stainless steel, copper, pure titanium and titanium alloy, nickel-based alloy and copper-based alloy; the volume concentration of the alcohol solution is 75%, ultrasonic cleaning is performed for 5 minutes, the temperature of the vacuum drying oven is 90-100°C, and the drying time is 2-5 minutes;

[0052] S2, placing the pretreated particles in a beaker containing an alcohol solution and stirring, using a dropper to absorb the suspension droplets before the pretreated particles have settled and applying them on the surface of the substrate to disperse and spread the suspension on the surface of the substrate, and then placing the sample in a drying oven to evaporate and remove the surface alcohol to obtain a pretreated particle layer attached to the surface of the substrate; taking out the sample, and continuing to absorb the suspension droplets and applying them on the surface of the substrate until the thickness of the pretreated particle layer reaches more than twice the particle size of the pretreated particles, to obtain a sample to be pretreated, and the thickness of the pretreated particle layer on the surface of the sample to be pretreated is 60-100 μm; the temperature of the drying oven is 90-100° C., and the drying time is 2-5 minutes;

[0053] S3, such as Figure 2 As shown, aluminum foil is covered on the surface of the sample to be pretreated, and then a constraint layer is placed on the aluminum foil layer and fixed on a movable processing platform;

[0054] The constraining layer is a light-transmitting material with a light transmittance higher than 90%, and the light-transmitting material includes water and K9 glass;

[0055] S4. According to the Hugo Neo elastic limit of the matrix material, the laser parameters are calculated by the Fabrro pressure model, and a laser with a pressure load more than 2 times higher than the pre-treated particles HEL is used for a single impact. The pre-treated particles collide with the matrix at high speed under the action of the laser impact, causing the surface of the matrix to produce plastic deformation to the boundary deposition area. Some pre-treated particles are embedded in the matrix to form deposition. The boundary deposition area is a spray pre-treatment area with compressive stress and an uneven surface. The floating powder remaining on the surface of the matrix is ​​cleaned to obtain a pre-treated sample, and the pre-treatment is completed; the laser generator used for laser impact is a Nd:YaG laser generator;

[0056] The 3D topography of the boundary deposition area is shown in Figure 3 , Figure 4 As shown, it can be seen that the surface of the barrier deposition area is uneven;

[0057] S5. Fix the spraying material on the surface of the boundary deposition area by using a pressing sheet to obtain a sample to be sprayed, wherein the material of the pressing sheet is tungsten steel;

[0058] S6. After covering the surface of the sample to be sprayed with aluminum foil and the constraint layer, fix it on a movable processing platform, adjust the laser parameters, and use a laser with a pressure load 2 to 5 times higher than the HEL of the spray material for single impact processing. The spray material partially offsets the rebound caused by the laser normal shock wave under the action of the compressive stress, and at the same time partially offsets the diffusion effect caused by the laser tangential shock wave under the action of the spray pretreatment area, so that the spray material and the boundary deposition area form a mechanical self-locking and combination;

[0059] The constrained layer is any one of the following: quartz glass, K9 glass and quartz glass after coating treatment;

[0060] The laser generator used for laser shock is a Nd:YaG laser generator;

[0061] S7, after removing the aluminum foil and the constraint layer, clean and dry, put it into an ultrasonic cleaner containing a 75% alcohol solution by volume for 5 minutes, and then put it into a drying oven at 100°C for 2 to 5 minutes, and the laser impact spraying is completed.

[0062] Example 2

[0063] like Figure 1 As shown, a method for improving the efficiency of laser shock spraying comprises the following steps:

[0064] Step 1: Grind and polish the surface of the base material sample, then ultrasonically clean it in an alcohol solution, and finally place it in a vacuum drying oven for standby use;

[0065] Step 2: Place aluminum-based particles of the same nature with a diameter twice that of the spraying material into a beaker filled with an alcohol solution with a volume concentration of 75%, stir thoroughly, and before the particles settle, use a dropper to draw the suspension and apply it on the surface of the substrate material to be sprayed. The mixed suspension containing the pretreated particles is dispersed and spread on the surface of the sample. Place the sample in a 100°C drying oven for 3 minutes to dry it and evaporate and remove the surface alcohol.

[0066] Step 3: Figure 2 As shown, the surface of the sample is covered with aluminum foil, the main purpose of which is to prevent the sample surface from being damaged during the laser shock spraying process during the pretreatment process.

[0067] Step 4: Place K9 optical glass with a light transmittance greater than 90% on the aluminum foil layer as a constraint layer to reflect the reflected shock wave back to the sample surface to increase the impact efficiency.

[0068] Step 5: Fix the sample on a movable processing platform, calculate the laser parameters through the Fabrro pressure model according to the hugoniot elastic limit (HEL) of the base material, make its pressure load 2 times higher than the material HEL (60% to 80%), and perform a single impact. (During pre-processing, there is no powder on the surface, and it is not normal processing,), the pre-processing is completed; the 3D morphology of the boundary deposition area is as follows Figure 3 , Figure 4 As shown, it can be seen that the surface of the barrier deposition area is uneven;

[0069] Step 6. An uneven boundary deposition area is formed on the surface of the substrate sample obtained from the above test, and due to the existence of residual stress, a small amount of particles are embedded in this concave area of ​​the substrate. At this time, the aluminum-based particles to be sprayed (generally micrometer scale) are fixed to the boundary deposition area on the surface of the substrate sample with a tungsten steel press.

[0070] Step 7: Cover the coating surface with aluminum foil and K9 glass layer by layer and fix them on a movable processing platform. Adjust the laser parameters again to make its power density 2 to 5 times higher than that of the material HEL. Perform subsequent processing on the coating area until the laser shock spraying is completed.

[0071] Example 3

[0072] like Figure 1 As shown, a method for improving the efficiency of laser shock spraying comprises the following steps:

[0073] In this example, the substrate material is T3 copper (10mm×10mm×3mm), which is mechanically polished and ultrasonically cleaned in an alcohol solution. The spraying particles are 1061 aluminum-based particles with a diameter of 20 to 30 μm, and the pre-treated particles are 1061 aluminum-based particles with a diameter of 50 to 60 μm;

[0074] This example is carried out in the following steps:

[0075] (1) Place the pretreated aluminum-based particles in a beaker filled with a 75% alcohol solution by volume, stir thoroughly, and use a dropper to draw the suspension droplets and apply them on the surface of the T3 copper substrate, spread them on the surface of the sample, and place the sample in a 100°C drying oven for 3 minutes to evaporate and remove the surface alcohol. After the alcohol evaporates, repeat the operation until the thickness reaches 60 to 80 μm.

[0076] (2) Figure 2 As shown, aluminum foil is covered on the surface of T3 copper, and K9 optical glass is placed on the aluminum foil layer, which is fixed on a KUKA (KR~8~R1640) manipulator. The main purpose of the aluminum foil is to prevent the sample surface from being damaged during the laser shock spraying process during the pretreatment process. The optical glass acts as a constraint layer to reflect the reflected shock wave back to the sample surface to increase the shock efficiency.

[0077] (3) According to the HEL of T3 copper of about 656MPa, the Fabrro pressure model was used to calculate the laser energy of 1J, the spot diameter of 3mm, and the pulse width of 15ns to perform a single impact on its surface. The surface of the sample was formed with pits formed by the impact of the pre-treated particles, and residual stress was preformed on the copper surface. A small amount of particles would be embedded in the copper matrix. At this time, the surface powder was cleaned.

[0078] The 3D topography of the boundary deposition area is shown in Figure 3 , Figure 4 As shown, it can be seen that the surface of the boundary deposition area is uneven.

[0079] (4) The aluminum-based sprayed particles are fixed on the surface of the T3 copper substrate with surface pretreatment using a tungsten steel press, and aluminum foil and K9 glass are covered layer by layer on the coating surface and fixed on a movable processing platform.

[0080] (5) Adjust the laser energy to 1.5 J, keep the spot diameter and pulse width unchanged, and perform impact spraying. After processing, remove the aluminum foil and glass on the surface, put the sample into an ultrasonic cleaning machine containing a 75% alcohol solution by volume for 5 minutes, take it out and place it in a drying oven at 100°C for three minutes to dry it.

[0081] In this embodiment, the coating density can be increased to 90% in a single processing. Figure 6a ;

[0082] The comparative example is to use only steps (4) and (5) for laser shock spraying. The surface image of the spraying is shown in FIG. Figure 6b The surface porosity is 60%, and it needs to be repeated 5 to 7 times to achieve the same coating density.

[0083] Example 4

[0084] like Figure 1 As shown, a method for improving the efficiency of laser shock spraying comprises the following steps:

[0085] In this example, the base material is 40Cr steel (10mm×10mm×3mm), which is mechanically polished and ultrasonically cleaned in an alcohol solution. The spraying particles are 1061 pure aluminum particles with a diameter of 20-30μm, and the pre-treated particles are 1061 pure aluminum particles with a diameter of 50-60μm;

[0086] This example is carried out in the following steps:

[0087] (1) Place the pretreated pure aluminum particles in a beaker filled with an alcohol solution with a volume concentration of 75%, stir thoroughly, and use a dropper to draw drops of the suspension and apply them to the surface of a 40Cr steel substrate. Spread the solution on the surface of the sample and place the sample in a drying oven at 100°C for 3 minutes to dry the sample and evaporate the alcohol on the surface.

[0088] (2) Figure 2 As shown, the surface of 40Cr steel is covered with aluminum foil, K9 optical glass is placed on the aluminum foil layer, and it is fixed on a KUKA (KR~8~R1640) robot.

[0089] (3) According to the HEL of 40Cr steel of about 1.46 GPa, the Fabrro pressure model was used to calculate the residual stress on the surface of 40Cr steel by single impact with laser energy of 3 J, spot diameter of 3 mm and pulse width of 15 ns.

[0090] (4) The pure aluminum spray particles are fixed on the surface of the pre-treated 40Cr steel substrate with a tungsten steel press, and aluminum foil and K9 glass are covered layer by layer on the coating surface and fixed on a movable processing platform.

[0091] (5) Adjust the laser energy to 5J, keep the spot diameter and pulse width unchanged, and perform impact spraying. After processing, remove the aluminum foil and glass on the surface, put the sample into an ultrasonic cleaning machine containing a 75% alcohol solution by volume for 5 minutes, take it out and place it in a drying oven at 100°C for three minutes to dry it.

[0092] In this embodiment, the coating density can be increased to more than 87% in a single processing;

[0093] In the comparative example, only steps (4) and (5) are used for laser impact spraying, which needs to be repeated 6 to 8 times to achieve the same coating density.

[0094] Example 5

[0095] like Figure 1 As shown, a method for improving the efficiency of laser shock spraying comprises the following steps:

[0096] In this example, the substrate material is TC11 titanium alloy (10mm×10mm×3mm), which is mechanically polished and ultrasonically cleaned in an alcohol solution. The sprayed particles are 7075 aluminum-based particles with a diameter of 20-30μm, and the pre-treated particles are 7075 aluminum-based particles with a diameter of 50-60μm.

[0097] This example is carried out in the following steps:

[0098] (1) Place the pretreated aluminum-based particles in a beaker filled with an alcohol solution with a volume concentration of 75%, stir thoroughly, use a dropper to draw drops of the suspension and apply them to the surface of the titanium alloy substrate, spread them on the surface of the sample, and place the sample in a drying oven at 100°C for 3 minutes to dry and evaporate the surface alcohol.

[0099] (2) Figure 2 As shown, aluminum foil is covered on the surface of the titanium alloy, and K9 optical glass is placed on the aluminum foil layer, which is fixed on a KUKA (KR~8~R1640) robot.

[0100] (3) According to the HEL of titanium alloy of about 900 MPa, the Fabrro pressure model was used to calculate the surface of the titanium alloy by single impact with a laser energy of 4.5 J, a spot diameter of 3 mm, and a pulse width of 15 ns to preform residual stress on the surface of the titanium alloy.

[0101] (4) The aluminum-based spray particles are fixed on the surface of the pre-treated titanium alloy substrate with a tungsten steel press, and aluminum foil and K9 glass are covered layer by layer on the coating surface and fixed on a movable processing platform.

[0102] (5) Adjust the laser energy to 7J, keep the spot diameter and pulse width unchanged, and perform impact spraying. After processing, remove the aluminum foil and glass on the surface, put the sample into an ultrasonic cleaning machine containing a 75% alcohol solution by volume for 5 minutes, take it out and place it in a drying oven at 100°C for three minutes to dry it.

[0103] In this embodiment, the coating density can be increased to more than 87% in a single processing;

[0104] In the comparative example, only steps (4) and (5) are used for laser impact spraying, which needs to be repeated 5 to 7 times to achieve the same coating density.

[0105] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.

Claims

1. A method for improving the efficiency of laser shock spraying, Features: The following steps are involved: S1. After grinding and polishing the surface of the substrate, ultrasonically clean it in an alcohol solution, and then dry it in a vacuum drying oven for later use. Prepare pre-treated particles and spraying materials. The pre-treated particles are used to impact the substrate at high speed by laser impact to form a barrier deposition area. The spraying material is used for laser impact spraying. The pre-treated particles have the same composition as the spraying material but different particle sizes. S2, placing the pretreated particles in a beaker containing an alcohol solution and stirring, using a dropper to absorb the suspension and apply it to the surface of the substrate before the pretreated particles have settled, and spreading the suspension on the surface of the substrate, and then placing the sample in a drying oven to evaporate and remove the surface alcohol to obtain a pretreated particle layer attached to the surface of the substrate; taking out the sample, and continuing to absorb the suspension and apply it to the surface of the substrate until the thickness of the pretreated particle layer reaches more than 2 times the particle size of the pretreated particles, to obtain a sample to be pretreated; S3, covering the surface of the sample to be pretreated with aluminum foil, placing a constraint layer on the aluminum foil layer and fixing it on a movable processing platform; S4. According to the Hugo Neo elastic limit of the matrix material, the laser parameters are calculated by the Fabrro pressure model, and a laser with a pressure load more than 2 times higher than the HEL of the pre-treated particles is used for a single impact. Under the action of the laser impact, the pre-treated particles hit the matrix at high speed to cause the surface of the matrix to be plastically deformed to the boundary deposition area. Some of the pre-treated particles are embedded in the matrix to form deposition. The boundary deposition area is a spray pre-treatment area with compressive stress and an uneven surface. The floating powder remaining on the surface of the matrix is ​​cleaned to obtain a pre-treated sample, and the pre-treatment is completed. S5, fixing the spraying material on the surface of the boundary deposition area by using a pressing sheet to obtain a sample to be sprayed; S6, after covering the surface of the sample to be sprayed with aluminum foil and the constraint layer, fix it on a movable processing platform, adjust the laser parameters, and use a laser with a pressure load 2 to 5 times higher than the HEL of the spray material for single impact processing, so that the spray material partially offsets the rebound caused by the laser normal shock wave under the action of the compressive stress, and at the same time partially offsets the diffusion effect caused by the laser tangential shock wave under the action of the spray pretreatment area, so that the spray material and the boundary deposition area form a mechanical self-locking and combination; S7, after removing the aluminum foil and the constraining layer, cleaning and drying are performed, and the laser shock spraying is completed.

2. A method for improving laser shock spraying efficiency according to claim 1, Features: In step S1, the particle size of the pre-treated particles is larger than the particle size of the spraying material.

3. A method for improving laser shock spraying efficiency according to claim 2, Features: The particle sizes of the spraying material and the pre-treated particles are both in the micron level, and the particle size of the pre-treated particles is more than twice the particle size of the spraying material; In step S2, the thickness of the pretreated particle layer on the surface of the sample to be pretreated is 60-100 μm.

4. A method for improving laser shock spraying efficiency according to claim 1, Features: In step S1, the materials of the spraying material and the pre-treated particles are any one of the following: aluminum-based particles, titanium alloy particles and copper alloy particles.

5. A method for improving laser shock spraying efficiency according to claim 1, Features: In step S1, the material of the substrate is a metal material.

6. A method for improving laser shock spraying efficiency according to claim 5, Features: The material of the substrate is any one of the following: martensitic steel, stainless steel, copper, pure titanium and titanium alloy, nickel-based alloy and copper-based alloy.

7. A method for improving laser shock spraying efficiency according to claim 1, Features: In step S1, the volume concentration of the alcohol solution is 75%, ultrasonic cleaning is performed for 5 minutes, the temperature of the vacuum drying oven is 90-100° C., and the drying time is 2-5 minutes; In step S2, the temperature of the drying oven is 90-100°C, and the drying time is 2-5 minutes; In step S7, after removing the aluminum foil and the constraining layer, the mixture is placed in an ultrasonic cleaning machine containing an alcohol solution with a volume concentration of 75% for 5 minutes, and then placed in a drying oven at 100° C. for drying for 2 to 5 minutes.

8. A method for improving laser shock spraying efficiency according to claim 1, Features: In steps S3 and S6, the constraining layer is a light-transmitting material with a light transmittance higher than 90%, and the light-transmitting material includes water and K9 glass.

9. A method for improving laser shock spraying efficiency according to claim 1, Features: The laser generator used for laser shock in steps S4 and S6 is a Nd:YaG laser generator.

10. A method for improving laser shock spraying efficiency according to claim 1, Features: In step S5, the material of the pressing sheet is tungsten steel.

Citation Information

Patent Citations

  • Method for preparing laser thermal composite induction nanoparticle reinforcement laminated film

    CN103103523A

  • Method for preparing compound coatings through laser shock induced chemical reaction

    CN103726046A

  • Novel thermal barrier coating structure and preparation method thereof

    CN113718188A

  • Surface strengthening method by laser shock on graphene or graphene oxide coating