Method for improving synthesis efficiency of silicon carbide powder

By adding doped powders with high thermal conductivity during the synthesis of silicon carbide powder, the radial temperature gradient in the crucible is reduced, the problem of low synthesis efficiency and yield impact of silicon carbide powder is solved, and high-purity β-phase silicon carbide powder is achieved efficient synthesis.

CN115676833BActive Publication Date: 2024-10-25BEIJING NAURA MICROELECTRONICS EQUIP CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202110857956.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-07-28
Publication Date
2024-10-25
Estimated Expiration
2041-07-28

AI Technical Summary

Technical Problem

In the existing silicon carbide powder synthesis process, as the diameter of the crucible increases, the radial temperature gradient is too large, causing serious carbonization of the edge powder, reducing the synthesis efficiency, and the mixture of α-phase silicon carbide and β-phase generated in the center is not conducive to the Screening affects yield.

Method used

Add doping powders with higher thermal conductivity, such as diamond powder, to carbon powder and silicon powder. Through the preset mixing and filling methods, the radial temperature gradient of the raw materials in the crucible is reduced, and the self-propagation method is used for carbonization. Silicon synthesis.

Benefits of technology

By increasing the thermal conductivity of the mixed powder, reducing the carbonization of the edge powder, improving the synthesis efficiency of silicon carbide powder, ensuring the generation of high-purity β-phase silicon carbide powder in the center, increasing the adaptability of the crucible size and reducing the temperature Gradient to improve heating efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115676833B_ABST
    Figure CN115676833B_ABST
Patent Text Reader

Abstract

The present invention discloses a method for improving the synthesis efficiency of silicon carbide powder, comprising: providing doped powder, carbon powder and silicon powder, wherein the doped powder is a material that does not pollute the silicon carbide powder, and the thermal conductivity of the doped powder is greater than that of the carbon powder; the carbon powder, silicon powder and doped powder are loaded into a crucible according to a preset mixing method and a preset filling method, and the doped powder is used to reduce the radial temperature gradient in the process of synthesizing silicon carbide powder from raw materials in the crucible; the crucible is placed in a silicon carbide synthesis device, and a silicon carbide synthesis process is performed based on a self-propagating method. The radial temperature gradient in the process of synthesizing silicon carbide powder from raw materials in the crucible is reduced, and the synthesis efficiency of silicon carbide powder is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of semiconductor material manufacturing, and more specifically, to a method for improving the synthesis efficiency of silicon carbide powder. Background Art

[0002] With the expansion of the application fields of third-generation semiconductor materials, silicon carbide single crystal materials, as the representative materials of third-generation semiconductors, have broad application prospects in many fields due to their characteristics such as large bandgap, high thermal conductivity, high saturated electron drift rate and high breakdown field strength. In particular, the fields of electric vehicles (xEV), rail transportation (Rail) and motor driving (Motordriving) are growing rapidly and their share is gradually expanding.

[0003] Silicon carbide single crystal materials are generally grown by PVT (physical vapor transport) method. In the PVT method, silicon carbide raw materials are used as raw materials for growing single crystals, which plays an important role in the sublimation method of growing semiconductor SiC single crystals. There are usually three methods for synthesizing silicon carbide powder: Acheson method, organic synthesis method and self-propagating method. In the Acheson method, SiO2 is reduced by C under high temperature and strong electric field, first generating β-SiC, and then transforming into α-SiC at high temperature. The SiC powder synthesized by this method requires crushing, pickling and other processes, and has a high impurity content, and its purity cannot reach the level of growing semiconductor single crystals. The organic synthesis method is mainly used to prepare nano-scale SiC powder. There are many impurity elements in the synthesized raw materials. Although high-purity SiC powder with high purity can be obtained through subsequent treatment, the subsequent treatment process is complicated, the micro powder is difficult to collect, and it is not suitable for mass production and use, and it is easy to produce substances harmful to the human body. In addition, the particle size of the SiC powder synthesized by this method is too small, which seriously affects the crystallization quality of SiC single crystals. The high temperature self-propagating method uses the self-conduction effect of the heat of the reaction of the substance to cause a chemical reaction between the substances, forming a high temperature synthesis reaction of the compound in a very short time. The self-propagating method is a method in which C powder and Si powder directly contact and react to produce SiC. At present, this method has been widely used in the preparation of high-purity SiC powder.

[0004] The existing method of synthesizing silicon carbide powder based on the self-propagating method uses high-purity carbon (C) powder and silicon (Si) powder to react directly, without adding additives, and controls external heating to make Si powder and C powder react continuously to generate high-purity SiC powder. With the increasing demand for the synthesis capacity of silicon carbide powder, the diameter of the crucible used is also getting larger; however, in order to ensure that the powder at the center can reach the synthesis temperature process window of silicon carbide powder, the temperature gradient between the edge and the center will be 1 to 3 times larger than that of a small-sized crucible; it will cause severe carbonization in the edge area, and the volume of the carbonized area will account for 1 / 2 of the raw material volume, seriously affecting the output; however, if only the raw materials at the edge are guaranteed to be within the high-purity β-phase silicon carbide raw material synthesis process temperature range (β-phase is the desired phase), other α-phase silicon carbide and silicon mixtures will be generated in the center (polluting the entire furnace raw materials, which is not conducive to screening).

[0005] In addition, as the diameter of the crucible increases, the temperature gradient becomes too large, and the powder at the edge of the crucible will be carbonized. The increased carbonization of the powder at the edge of the crucible will continuously reduce the synthesis efficiency of silicon carbide powder. For example, the weight of carbon silicon powder is 40kg, but only 20kg of silicon carbide powder is obtained. Summary of the invention

[0006] The purpose of the present invention is to provide a method for improving the synthesis efficiency of silicon carbide powder, thereby reducing the radial temperature gradient during the process of synthesizing silicon carbide powder from raw materials in the crucible and improving the synthesis efficiency of silicon carbide powder.

[0007] To achieve the above object, the present invention proposes a method for improving the synthesis efficiency of silicon carbide powder, comprising:

[0008] Providing doping powder, carbon powder and silicon powder, wherein the doping powder is a material that does not contaminate silicon carbide powder, and the thermal conductivity of the doping powder is greater than the thermal conductivity of the carbon powder;

[0009] The carbon powder, the silicon powder and the doped powder are loaded into a crucible according to a preset mixing method and a preset filling method, wherein the doped powder is used to reduce the radial temperature gradient during the process of synthesizing silicon carbide powder from the raw materials in the crucible;

[0010] The crucible is placed in a silicon carbide synthesis device, and a silicon carbide synthesis process is performed based on a self-propagating method.

[0011] Optionally, the step of loading the carbon powder, the silicon powder and the doping powder into the crucible according to a preset mixing method and a preset filling method comprises:

[0012] Fully mixing the carbon powder, the silicon powder and the doping powder to form a first raw material;

[0013] The first raw material is loaded into the crucible.

[0014] Optionally, the step of loading the carbon powder, the silicon powder and the doping powder into the crucible according to a preset mixing method and a preset filling method comprises:

[0015] Fully mixing the carbon powder, the silicon powder and the doping powder to form a first raw material;

[0016] Fully mixing the carbon powder and the silicon powder to form a second raw material;

[0017] The second raw material is loaded into a central area of ​​the crucible, and the first raw material is loaded into a peripheral area of ​​the second raw material in the crucible.

[0018] Optionally, the molar ratio of the carbon powder to the silicon powder in the first raw material is 1:1, and the weight of the doped powder is greater than or equal to 1% of the total weight of the carbon powder and the silicon powder.

[0019] Optionally, the molar ratio of the carbon powder to the silicon powder in the second raw material is 1:1.

[0020] Optionally, the doped powder includes at least one of diamond powder, silicon carbide powder, graphene powder, carbon nanotube powder and carbon 60 powder.

[0021] Optionally, the particle size of diamond in the diamond powder is less than or equal to 1000 μm.

[0022] Optionally, placing the crucible into a silicon carbide synthesis device comprises:

[0023] The crucible is placed in a synthetic thermal field system and put into a growth chamber of a single crystal furnace heated by medium frequency induction.

[0024] Optionally, the silicon carbide synthesis process based on the self-propagation method includes:

[0025] evacuating the growth chamber to a preset pressure;

[0026] Raising the temperature in the growth chamber to a first preset temperature;

[0027] Injecting argon gas into the growth chamber and continuing heating to raise the temperature in the growth chamber to a second preset temperature;

[0028] Maintaining the second preset temperature until the set reaction time;

[0029] The temperature in the growth chamber is lowered to room temperature to obtain synthesized silicon carbide powder.

[0030] Optionally, the preset pressure is less than 0.0001 Pa; the first preset temperature is 1000° C., the second preset temperature is 2000° C.-2100° C.; and the set reaction time is 10 hours.

[0031] The beneficial effects of the present invention are:

[0032] The present invention changes the composition of the raw materials for synthesizing silicon carbide powder and adds doping powder with higher thermal conductivity and no contamination to the carbon powder and silicon powder, thereby increasing the thermal conductivity of the mixed powder of carbon powder and silicon powder, thereby reducing the radial temperature gradient of the mixed powder, reducing the carbonization of the edge powder, and improving the synthesis efficiency.

[0033] The method of the present invention has other characteristics and advantages, which will be apparent from the accompanying drawings and subsequent detailed descriptions incorporated herein, or will be described in detail in the accompanying drawings and subsequent detailed descriptions incorporated herein, which together serve to explain the specific principles of the present invention. BRIEF DESCRIPTION OF THE DRAWINGS

[0034] The above and other objects, features and advantages of the present invention will become more apparent through a more detailed description of exemplary embodiments of the present invention in conjunction with the accompanying drawings, in which like reference numerals generally represent like components.

[0035] Figure 1 The schematic diagram shows the structure of a crucible in an existing silicon carbide synthesis method.

[0036] Figure 2 A flow chart showing the steps of a method for improving the synthesis efficiency of silicon carbide powder according to Example 1 of the present invention.

[0037] Figure 3 A schematic diagram of powder filling in different zones in a method for improving synthesis efficiency of silicon carbide powder according to Example 2 of the present invention is shown.

[0038] Figure 4 A curve comparison of the radial Wendy gradient distribution of silicon carbide powder synthesized by the method for improving the synthesis efficiency of silicon carbide powder according to embodiments 1 and 2 of the present invention and the conventional filler method is shown. DETAILED DESCRIPTION

[0039] In an existing method for synthesizing silicon carbide using a self-propagating method, the following method is used: Figure 1The crucible shown is used to synthesize silicon carbide, and the crucible includes: a chamber 1, a first wall 2, a second wall 3, a cover 4, a first opening 5, a cavity 6, an inner bottom corner 7 of the first wall, an outer bottom corner 8 of the first wall, an inner bottom corner 9 of the second wall, an outer bottom corner 10 of the second wall, a material 11, and a second opening 12. The method can suppress the carbonization of powder, improve the synthesis efficiency, and reduce the cost by using a crucible with a double-layer chamber wall, a double-layer chamber wall side wall provided with openings, and a chamber wall bottom corner designed in an arc shape. The double-layer chamber wall design inside and outside the crucible can realize that the second wall 3, i.e., the outer wall, generates heat and radiates heat inward, and the first wall 2, i.e., the inner wall, is evenly heated, so that the temperature field in the powder area in the chamber is more uniform, stable and orderly, thereby improving the purity and consistency of the powder size; and the first wall (i.e., the inner wall) of the crucible itself does not generate heat but only receives heat, and its relative temperature is relatively low, which can effectively inhibit the high-temperature carbonization of the contact surface between the first wall, i.e., the inner wall, and the powder, thereby improving the quality of silicon carbide powder and the synthesis efficiency.

[0040] However, the prior art has the following disadvantages:

[0041] 1. Since the thermal conductivity of carbon silicon powder is too small, a small amount of carbonization occurs when a small-sized crucible (less than 6 inches in diameter) is used to synthesize the raw material according to this method. However, the use of a large-radius crucible will result in serious carbonization (the radius of the crucible determines the output of the synthetic silicon carbide raw material). It is not easy to expand the crucible size to a diameter of more than 300 mm.

[0042] 2. If the crucible size is expanded to a diameter of more than 380 mm, the thermal conductivity of carbon powder and silicon powder is used for synthesis. The temperature gradient between the center and the edge is large. In order to ensure that the powder temperature at the center reaches the synthesis temperature, the temperature near the edge of the graphite crucible will still produce carbonization, and the carbonization area will be greater than 50%.

[0043] The present invention changes the powder composition, adds a proper amount of doping powder, increases the thermal conductivity of the mixed powder of carbon powder and silicon powder, thereby reducing the radial temperature gradient of the powder, reducing the carbonization of the edge powder, and improving the synthesis efficiency.

[0044] The present invention will be described in more detail below with reference to the accompanying drawings. Although preferred embodiments of the present invention are shown in the accompanying drawings, it should be understood that the present invention can be implemented in various forms and should not be limited by the embodiments set forth herein. On the contrary, these embodiments are provided to make the present invention more thorough and complete, and to fully convey the scope of the present invention to those skilled in the art.

[0045] Example 1

[0046] Figure 2 A flow chart showing the steps of a method for improving the synthesis efficiency of silicon carbide powder according to the present invention.

[0047] like Figure 2As shown, the method for improving the synthesis efficiency of silicon carbide powder comprises:

[0048] S101: providing doping powder, carbon powder and silicon powder, wherein the doping powder is a material that does not pollute the silicon carbide powder, and the thermal conductivity of the doping powder is greater than the thermal conductivity of the carbon powder;

[0049] Specifically, the doped powder includes at least one of diamond powder, silicon carbide powder, graphene powder, carbon nanotube powder, and carbon 60 powder. In this embodiment, the doped powder is preferably diamond powder. The thermal conductivity of the material is determined by the lattice structure of the material itself. At room temperature, the thermal conductivity of diamond (2000W / m*k)> the thermal conductivity of graphite (150W / m*k)> the thermal conductivity of silicon (130W / m*k) (diamond is the material with the best thermal conductivity in nature). In addition, diamond powder, as an allotrope of graphite, can undergo phase change at high temperatures above 2000°C, mainly transforming into a graphite phase. Therefore, diamond powder is used as a thermal conductive additive to reduce the radial temperature gradient of the powder inside the crucible without introducing new impurity elements, and a high-purity silicon carbide product can be obtained.

[0050] In other embodiments, the doped powder can also be a material with high thermal conductivity and no contamination to the silicon carbide powder, such as silicon carbide powder, graphene powder, carbon nanotube powder, C60 powder, etc. The doped powder can be one or multiple materials in any proportion.

[0051] In this step, diamond powder with a particle size of no more than 1000 μm is preferably used, and is prepared for use after screening, washing, drying and other steps.

[0052] S102: Carbon powder, silicon powder and doped powder are loaded into the crucible according to a preset mixing method and a preset filling method. The doped powder is used to reduce the radial temperature gradient during the process of synthesizing silicon carbide powder from the raw materials in the crucible.

[0053] Specifically, in this step, preferably, carbon powder and silicon powder are weighed in a molar ratio of 1:1 and loaded into a container; then, diamond powder is weighed according to 3.5% of the total weight of the carbon powder and silicon powder and loaded into the container; then, the weighed carbon powder, silicon powder and diamond powder are fully mixed to form a first raw material, and finally the mixed first raw material is loaded into the containing cavity of the crucible, and the crucible is preferably a high-purity crucible. It should be noted that the doping ratio of the diamond powder needs to be greater than or equal to 1% of the total weight of the carbon powder and silicon powder, preferably 3.5%.

[0054] S103: placing the crucible into a silicon carbide synthesis device, and performing a silicon carbide synthesis process based on a self-propagating method.

[0055] Specifically, a crucible is placed in a synthetic thermal field system and in a single crystal furnace with medium frequency induction heating; then, a raw material synthesis process is carried out according to certain synthesis parameters, wherein the growth chamber of the single crystal furnace is evacuated to less than 0.0001 Pa, and after heating for about 60 minutes, the temperature is raised to about 1000°C; then, high-purity argon gas (volume fraction > 99.999%) is filled into the growth chamber, and then heating is continued to raise the temperature in the growth chamber to 2000°C-2100°C, the synthesis reaction time is controlled to be about 10 hours, and finally the temperature is lowered to room temperature to obtain silicon carbide powder.

[0056] Example 2

[0057] The difference between this embodiment and implementation 1 is that in step S102, this embodiment adopts a partition mixing scheme, specifically:

[0058] First, carbon powder, silicon powder and doping powder are fully mixed to form a first raw material; the doping powder is preferably diamond powder with a particle size of no more than 1000 μm, and the mixing ratio is the same as in Example 1;

[0059] Then, the carbon powder and the silicon powder are weighed in a molar ratio of 1:1 and mixed thoroughly to form a second raw material;

[0060] Afterwards, the second raw material is loaded into the central area of ​​the crucible, and the first raw material is loaded into the edge area of ​​the crucible around the second raw material.

[0061] This step is as follows Figure 3 As shown, the crucible includes a crucible body and a crucible cover. The crucible body has a cylindrical accommodating cavity inside. During the powder filling process, a prefabricated isolation piece can be used for partition filling. The isolation piece is in the shape of a cylinder with open ends. The diameter of the isolation piece is set according to the specific raw material partition ratio. First, the isolation piece is placed in the central area of ​​the accommodating cavity and the bottom of the isolation piece is in contact with the bottom wall of the crucible body. The second raw material is filled inside the isolation piece, and then the first raw material is filled in the annular space formed between the outside of the isolation piece and the side wall of the crucible. After the filling is completed, it is necessary to ensure that the first raw material and the second raw material are filled to the same height, and a certain gap is left between the top of the raw materials and the crucible cover. Then the isolation piece is taken out vertically to form a Figure 3 The filling effect shown.

[0062] The other steps of this embodiment are the same as those of Embodiment 1 and will not be described again here.

[0063] This embodiment adopts a partitioned mixing solution, which reduces the use of diamond powder and can reduce costs (high-purity diamond powder is very expensive), and can also achieve similar effects as the solution in Example 1.

[0064] Figure 4A curve comparison of the radial Wendy gradient distribution of silicon carbide powder synthesized by the method for improving the synthesis efficiency of silicon carbide powder according to embodiments 1 and 2 of the present invention and the existing conventional filler method is shown.

[0065] like Figure 4 As shown, it can be seen that the existing conventional charging method: the radial temperature gradient difference of the synthetic raw material in the crucible is 29.55°C; the charging method of the embodiment 1 scheme is adopted: the radial temperature gradient difference of the synthetic raw material in the crucible is 10.08°C; the filling method of the embodiment 2 scheme is adopted: using different proportions of partitioned charging methods, the radial temperature gradient difference of the synthetic raw material in the crucible is distributed as 12.45°C and 18.9 degrees Celsius; and, the larger the proportion of the doped diamond powder partition, the smaller the temperature gradient.

[0066] In summary, the present invention has the following beneficial effects:

[0067] 1) Compared with the existing process, by adding diamond powder or the like as a thermal conductor, the thermal conductivity of the raw materials inside the crucible is improved, and the radial temperature gradient of the powder in the crucible is reduced (more uniform temperature can ensure the quality of the raw materials synthesized into high-quality β-phase silicon carbide powder. The structure of silicon carbide synthesized at different temperatures is different. Within the appropriate temperature window, the more uniform the temperature, the better). The temperature of the edge and center of the raw materials in the large-sized crucible is reduced from 30 degrees to 10 degrees, and the temperature gradient is reduced by 3 times, thereby improving the heating efficiency;

[0068] 2) Solved the problem of severe edge carbonization during the synthesis of silicon carbide raw materials caused by excessive radial temperature gradient, and reduced graphitization near the edge of the crucible;

[0069] 3) Cost saving, can be applied to large-sized crucibles (crucible diameter is greater than 380 mm), using the method of the present invention, 40 kg of silicon carbide powder can be synthesized in only one time, greatly improving the synthesis efficiency;

[0070] 4) The charging method of Example 2 of the present invention can reduce the amount of diamond powder used, save costs and achieve an effect similar to that of Example 1.

[0071] The embodiments of the present invention have been described above, and the above description is exemplary, not exhaustive, and is not limited to the disclosed embodiments. Many modifications and changes will be apparent to those skilled in the art without departing from the scope and spirit of the described embodiments.

Claims

1. A method for improving the synthesis efficiency of silicon carbide powder, characterized in that: include: Providing doping powder, carbon powder and silicon powder, wherein the doping powder is a material that does not contaminate silicon carbide powder, and the thermal conductivity of the doping powder is greater than the thermal conductivity of the carbon powder; The carbon powder, the silicon powder and the doped powder are loaded into a crucible according to a preset mixing method and a preset filling method, wherein the doped powder is used to reduce the radial temperature gradient during the process of synthesizing silicon carbide powder from the raw materials in the crucible; The crucible is placed in a silicon carbide synthesis device, and a silicon carbide synthesis process is performed based on a self-propagating method; The step of loading the carbon powder, the silicon powder and the doping powder into the crucible according to a preset mixing method and a preset filling method comprises: Fully mixing the carbon powder, the silicon powder and the doping powder to form a first raw material; placing the first raw material into the crucible; The doped powder includes at least one of diamond powder, graphene powder, carbon nanotube powder and carbon 60 powder, and the weight of the doped powder is greater than or equal to 1% of the total weight of the carbon powder and the silicon powder, and less than or equal to 3.5% of the total weight of the carbon powder and the silicon powder; The molar ratio of the carbon powder to the silicon powder in the first raw material is 1:

1.

2. The method for improving the synthesis efficiency of silicon carbide powder according to claim 1, characterized in that: The step of loading the carbon powder, the silicon powder and the doping powder into the crucible according to a preset mixing method and a preset filling method comprises: Fully mixing the carbon powder, the silicon powder and the doping powder to form a first raw material; Fully mixing the carbon powder and the silicon powder to form a second raw material; The second raw material is loaded into a central area of ​​the crucible, and the first raw material is loaded into a peripheral area of ​​the second raw material in the crucible.

3. The method for improving the synthesis efficiency of silicon carbide powder according to claim 2, characterized in that: The molar ratio of the carbon powder to the silicon powder in the second raw material is 1:

1.

4. The method for improving the synthesis efficiency of silicon carbide powder according to claim 1, characterized in that: The particle size of diamond in the diamond powder is less than or equal to 1000 μm.

5. The method for improving the synthesis efficiency of silicon carbide powder according to claim 1, characterized in that: Placing the crucible into the silicon carbide synthesis device comprises: The crucible is placed in a synthetic thermal field system and put into a growth chamber of a single crystal furnace heated by medium frequency induction.

6. The method for improving the synthesis efficiency of silicon carbide powder according to claim 5, characterized in that: The silicon carbide synthesis process based on the self-propagation method comprises: evacuating the growth chamber to a preset pressure; Raising the temperature in the growth chamber to a first preset temperature; Injecting argon gas into the growth chamber and continuing heating to raise the temperature in the growth chamber to a second preset temperature; Maintaining the second preset temperature until the set reaction time; The temperature in the growth chamber is lowered to room temperature to obtain synthesized silicon carbide powder.

7. The method for improving the synthesis efficiency of silicon carbide powder according to claim 6, characterized in that: The preset pressure is less than 0.0001 Pa; the first preset temperature is 1000° C., and the second preset temperature is 2000° C.-2100° C.; and the set reaction time is 10 hours.