A plant fiber modification method and modified plant fiber material
The hydrothermal reaction method is used to synthesize BiFeO3 nanocrystalline plant fibers and perform esterification treatment, which solves the problem of insufficient interface strength and easy combustion between plant fibers and polymers, significantly improves the mechanical and flame retardant properties of composite materials, and forms high-performance composite materials. Green composite materials.
Patent Information
- Application Number
- CN202211477146.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-11-23
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2042-11-23
AI Technical Summary
The interface strength between the plant fiber and the polymer matrix is insufficient, resulting in poor mechanical properties of the composite material. At the same time, the plant fiber composite material is easy to burn, posing safety risks.
The hydrothermal reaction method was used to synthesize BiFeO3 nanocrystalline plant fibers, and the polarity of the fiber surface was reduced through the esterification reaction to improve the interface strength and flame retardant properties of the fiber and polymer.
It significantly improves the mechanical properties and flame retardant properties of plant fibers, enhances the compatibility between fibers and polymers, forms high-performance plant fiber/polymer composite materials, and achieves green and environmentally friendly esterification modification.
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of plant fiber modification, and in particular relates to a plant fiber modification method and modified plant fiber materials. Background Art
[0002] Plant fibers come from natural plants and have the advantages of low cost, low density, renewable and degradable. Plant fibers are introduced into polymer matrices to prepare high-performance green composite materials, which have a wide range of application scenarios in engineering fields such as aerospace, automobiles, sports, packaging, medical care, and construction. However, the mechanical properties of composite materials depend not only on the properties of the fibers and the matrix themselves, but also on the strength of the interface between the two phases. There are a large number of hydroxyl groups on the surface of plant fibers, which have strong hydrophilicity, while polymer molecules are often low-polar or even non-polar substances. For example, polypropylene (PP), a meltblown cloth widely used as a filter material for masks, is a non-polar material, and polylactic acid (PLA), a bio-based polymer widely used in food packaging, is a low-polar material. This polarity difference makes it difficult for plant fibers to combine with polymers when blended with polymer materials, which has an adverse effect on the mechanical properties of composite materials.
[0003] In order to improve the interfacial strength between plant fibers and polymer matrices, different physical and chemical methods can be used to modify plant fibers and reduce the surface polarity of fibers. Physical modification methods include plasma treatment, corona treatment, ultraviolet treatment and heat treatment. Chemical modification methods include alkali treatment, silane treatment, acetylation treatment, benzoylation treatment, hydrogen peroxide treatment, potassium permanganate treatment and nanografting. Among them, alkali treatment and silane treatment have been widely used for surface modification of plants. Alkali treatment is to soak plant fibers for a long time with a high-quality concentration solution of a strong alkaline substance such as NaOH, Ca(OH)2, etc., which can effectively remove impurities such as lignin, hemicellulose, pectin and wax on the surface of plant fibers, increase the roughness of the fiber surface, and thus improve the mechanical lock strength between the fiber and the polymer matrix. The alkali treatment method only makes certain changes to the chemical composition and surface structure of plant fibers, and fails to change the strong hydrophilicity of the plant fibers themselves, so the effect of improving the interfacial strength between plant fibers and polymers is limited. Silane coupling agent can cover the micropores on the surface of the fiber as a surface coating and penetrate into the micropores. After hydrolysis, the silane coupling agent can obtain active hydroxyl groups, which can react with the hydroxyl groups on the surface of the plant fiber and the active groups in the matrix, respectively, to form a bridge between the plant fiber and the matrix. The interaction between the silane coupling agent and the surface of the plant fiber is usually achieved by hydrogen bonds, covalent bonds, etc. This force is often relatively weak. During the mixing process with the polymer, as the processing temperature rises to above 100 °C, weak interactions such as hydrogen bonds and covalent bonds will be destroyed, resulting in the deterioration of the compatibility between the plant fiber and the polymer matrix. Acylation treatment is to use acyl chloride chemicals to react with the hydroxyl groups on the surface of the plant fiber to generate ester substances, thereby reducing the hydrophilicity of the plant fiber. As a highly reactive esterifying agent, acyl chloride has the disadvantages of high toxicity, easy water absorption and inactivation, and easy degradation of the plant fiber during the reaction process. Although the method of using fatty acids plus co-reactants (such as trifluoroacetic anhydride, toluenesulfonyl chloride, etc.) can reduce the toxicity of the reaction aid to a certain extent, it still has the problem of not being green and environmentally friendly.
[0004] In addition, plant fiber composite materials are extremely flammable due to their organic properties. In a fire or under a high-intensity heat source, the composite materials will be thermally decomposed or burn violently, releasing a large amount of heat and smoke. Moreover, the thermal softening of the composite materials will cause the structure to buckle and break, leading to the deterioration or loss of mechanical properties, which will bring serious safety problems. Summary of the invention
[0005] The purpose of the present invention is to provide a method for modifying plant fibers.
[0006] Another object of the present invention is to provide a plant fiber material product modified by the above method.
[0007] The object of the present invention is achieved through the following scheme: A method for modifying plant fibers, comprising the following steps:
[0008] (1) Wash the plant fiber with deionized water for 3-5 times, dry it at 30-50 °C, and cut it into 5-10 mm segments;
[0009] (2) Add 7.00-11.00 parts by weight of the plant fiber segments obtained in step (1), 0.20-0.40 parts by weight of Fe(NO3)3·9H2O and 0.24-0.48 parts by weight of Bi(NO3)3·5H2O to 85.70-91.60 parts by weight of deionized water, stir evenly, and then add 1.00-2.50 parts by weight of 25 wt% KOH solution dropwise under strong stirring. After continuing to stir for 30-60 minutes, transfer the obtained mixed solution to a hydrothermal reactor. After sealing the hydrothermal reactor, react at 150-170 ° C for 6-12 hours. After the reaction is completed, cool naturally to room temperature to obtain a water dispersion of plant fibers loaded with BiFeO3 nanocrystalline;
[0010] (3) Add 2.00-3.00 parts by weight of long-chain fatty acid to the aqueous dispersion of plant fibers loaded with BiFeO3 nanocrystals obtained in step (2) and stir evenly. After sealing the hydrothermal reactor, react at 80-90°C for 4-8 hours. After the reaction is completed, cool naturally to room temperature, filter to obtain a solid substance, wash it repeatedly with ethanol and deionized water for 3 times, place it in a 60-80°C oven to dry for 10-12 hours, and recover the esterified modified plant fibers loaded with BiFeO3 nanocrystals.
[0011] The plant fiber in step (1) is one of flax fiber and ramie fiber or a mixture of the two.
[0012] In the step (2), the molar ratio of Fe(NO3)3·9H2O to Bi(NO3)3·5H2O is 1:1.
[0013] In step (3), the long-chain fatty acid is a saturated fatty acid, an unsaturated fatty acid, or a mixture of the two, having 12 to 18 carbon atoms.
[0014] On the other hand, the present invention provides a modified plant fiber material, namely, flax fiber loaded with BiFeO3 nanocrystal esterified modified flax fiber, ramie fiber loaded with BiFeO3 nanocrystal esterified modified ramie fiber, or a mixture of flax fiber loaded with BiFeO3 nanocrystal esterified modified ramie fiber and ramie fiber obtained by modifying one or a mixture of flax fiber and ramie fiber using the plant fiber modification method.
[0015] Compared with the existing plant fiber modification method, the present invention has the following advantages:
[0016] 1. The present invention adopts a hydrothermal reaction to synthesize plant fibers loaded with BiFeO3 nanocrystals in one step. The alkaline substance KOH in the reaction system acts as a reaction aid and reacts with Fe(NO3)3·9H2O and Bi(NO3)3·5H2O through a hydrothermal reaction to generate BiFeO3 nanocrystals. At the same time, the plant fibers in the reaction system are surface treated under hydrothermal conditions to increase the roughness of the plant fiber surface and obtain an effect similar to mercerization treatment.
[0017] 2. The BiFeO3 nanocrystals loaded on the plant fibers of the present invention are beneficial to enhancing the mechanical properties and flame retardant properties of the plant fibers on the one hand; on the other hand, the esterification reaction between long-chain fatty acids and the hydroxyl groups on the surface of the plant fibers is realized by utilizing their catalytic activity, which is green and environmentally friendly. Esterification modification is beneficial to reducing the surface polarity of the plant fibers, improving the interface strength between the plant fibers and the polymer matrix, and obtaining high-performance plant fiber / polymer composite materials. DETAILED DESCRIPTION
[0018] The technical solution of the present invention is further described below according to specific embodiments. The protection scope of the present invention is not limited to the following embodiments, which are listed only for illustrative purposes and do not limit the present invention in any way.
[0019] Example 1
[0020] A plant fiber is prepared according to the following steps:
[0021] (1) Wash the plant fiber flax fiber with deionized water three times, dry it at 30°C, and cut it into 5 mm small pieces;
[0022] (2) Add 7.00 parts by weight of the plant fiber segments obtained in step (1), 0.20 parts by weight of Fe(NO3)3·9H2O and 0.24 parts by weight of Bi(NO3)3·5H2O to 91.44 parts by weight of deionized water, stir evenly, and then add 1.12 parts by weight of 25 wt% KOH solution dropwise under strong stirring; continue stirring for 30 minutes, and then transfer the obtained mixed solution to a hydrothermal reactor; seal the hydrothermal reactor, react at 150°C for 12 hours, and naturally cool to room temperature after the reaction to obtain a water dispersion of plant fibers loaded with BiFeO3 nanocrystals;
[0023] (3) Add 2.00 parts by weight of long-chain fatty acid stearic acid to the aqueous dispersion of plant fibers loaded with BiFeO3 nanocrystals obtained in step (2) and stir evenly. After sealing the hydrothermal reactor, react at 80°C for 8 h; after the reaction is completed, naturally cool to room temperature, filter to obtain a solid substance, wash it repeatedly with ethanol and deionized water for 3 times, place it in a 60°C oven to dry for 12 h, and recover the esterified modified flax fiber loaded with BiFeO3 nanocrystals.
[0024] Example 2
[0025] A plant fiber is prepared according to the following steps:
[0026] (1) Wash plant fiber ramie fiber with deionized water for 5 times, dry it at 50 °C, and cut it into 10 mm small pieces;
[0027] (2) Add 11.00 parts by weight of the plant fiber segments obtained in step (1), 0.40 parts by weight of Fe(NO3)3·9H2O and 0.48 parts by weight of Bi(NO3)3·5H2O to 85.89 parts by weight of deionized water, stir evenly, and then add 2.23 parts by weight of 25 wt% KOH solution dropwise under strong stirring; continue stirring for 60 min, and then transfer the obtained mixed solution to a hydrothermal reactor. After sealing the hydrothermal reactor, react at 170 ° C for 6 h. After the reaction is completed, cool naturally to room temperature to obtain a water dispersion of plant fibers loaded with BiFeO3 nanocrystals;
[0028] (3) Add 3.00 parts by weight of lauric acid to the aqueous dispersion of plant fiber loaded with BiFeO3 nanocrystals obtained in step (2) and stir evenly. After sealing the hydrothermal reactor, react at 90°C for 4 h. After the reaction is completed, cool naturally to room temperature, filter to obtain a solid substance, wash it repeatedly with ethanol and deionized water for 3 times, place it in an oven at 80°C for 10 h, and recover the BiFeO3 nanocrystal-loaded lauric acid-modified ramie fiber material.
[0029] Example 3
[0030] A plant fiber is prepared according to the following steps:
[0031] (1) washing plant fibers with deionized water for 4 times, wherein the mixture of the plant fibers, flax fibers and ramie fibers, has a mass ratio of 1:1, is dried at 40° C., and cut into 8 mm small segments;
[0032] (2) Add 9.00 parts by weight of the plant fiber segments obtained in step (1), 0.30 parts by weight of Fe(NO3)3·9H2O and 0.36 parts by weight of Bi(NO3)3·5H2O to 88.66 parts by weight of deionized water, stir evenly, and then add 1.68 parts by weight of 25 wt% KOH solution dropwise under strong stirring; continue stirring for 45 minutes, and then transfer the obtained mixed solution to a hydrothermal reactor. After sealing the hydrothermal reactor, react at 160°C for 8 hours. After the reaction is completed, cool naturally to room temperature to obtain a water dispersion of plant fibers loaded with BiFeO3 nanocrystals;
[0033] (3) Add 2.50 parts by weight of oleic acid to the aqueous dispersion of plant fibers loaded with BiFeO3 nanocrystals obtained in step (2) and stir evenly. After sealing the hydrothermal reactor, react at 85°C for 6 h. After the reaction is completed, cool naturally to room temperature, filter to obtain a solid substance, wash it repeatedly with ethanol and deionized water for 3 times, place it in a 70°C oven to dry for 11 h, and recover the BiFeO3 nanocrystal-loaded oleic acid-esterified modified flax fiber and ramie fiber composite material.
[0034] Those skilled in the art should note that the embodiments described in the present invention are merely exemplary, and various other substitutions, changes and improvements may be made within the scope of the present invention. Therefore, the present invention is not limited to the above embodiments, but only to the claims.
Claims
1. A method for modifying plant fiber, characterized in that: The following steps are involved: (1) Wash the plant fiber with deionized water for 3-5 times, dry it at 30-50 °C, and cut it into 5-10 mm segments; (2) adding 7.00-11.00 parts by weight of the plant fiber segments obtained in step (1), 0.20-0.40 parts by weight of Fe(NO3)3·9H2O and 0.24-0.48 parts by weight of Bi(NO3)3·5H2O to 85.70-91.60 parts by weight of deionized water, stirring evenly, and then adding 1.00-2.50 parts by weight of a 25 wt% KOH solution dropwise under strong stirring; After continuing to stir for 30-60 min, the obtained mixed solution was transferred to a hydrothermal reactor; after sealing the hydrothermal reactor, the mixture was reacted at 150-170 °C for 6-12 h, and after the reaction was completed, the mixture was naturally cooled to room temperature to obtain a water dispersion of plant fibers loaded with BiFeO3 nanocrystalline; (3) adding 2.00-3.00 parts by weight of a long-chain fatty acid to the aqueous dispersion of the plant fiber loaded with BiFeO3 nanocrystals obtained in step (2) and stirring the mixture evenly; sealing the hydrothermal reactor and reacting the mixture at 80-90°C for 4-8 hours; cooling the mixture naturally to room temperature after the reaction, filtering the solid material, washing the solid material with ethanol and deionized water for three times, drying the solid material in an oven at 60-80°C for 10-12 hours, and recovering the esterified plant fiber loaded with BiFeO3 nanocrystals; The plant fiber in step (1) is one of flax fiber and ramie fiber or a mixture of both; In the step (2), the molar ratio of Fe(NO3)3·9H2O to Bi(NO3)3·5H2O is 1:
1.
2. The method for modifying plant fiber according to claim 1, characterized in that: In step (3), the long-chain fatty acid is a saturated fatty acid, an unsaturated fatty acid, or a mixture of the two, having 12 to 18 carbon atoms.
3. The method for modifying plant fiber according to any one of claims 1 to 2, characterized in that: Prepare as follows: (1) Wash the plant fiber flax fiber with deionized water three times, dry it at 30°C, and cut it into 5 mm small pieces; (2) Add 7.00 parts by weight of the plant fiber segments obtained in step (1), 0.20 parts by weight of Fe(NO3)3·9H2O and 0.24 parts by weight of Bi(NO3)3·5H2O to 91.44 parts by weight of deionized water, stir evenly, and then add 1.12 parts by weight of 25 wt% KOH solution dropwise under strong stirring; continue stirring for 30 minutes, and then transfer the obtained mixed solution to a hydrothermal reactor; seal the hydrothermal reactor, react at 150°C for 12 hours, and naturally cool to room temperature after the reaction to obtain a water dispersion of plant fibers loaded with BiFeO3 nanocrystals; (3) Add 2.00 parts by weight of long-chain fatty acid stearic acid to the aqueous dispersion of plant fibers loaded with BiFeO3 nanocrystals obtained in step (2), and stir evenly; seal the hydrothermal reactor, and react at 80°C for 8 h; after the reaction is completed, naturally cool to room temperature, filter to obtain a solid substance, wash it repeatedly with ethanol and deionized water for 3 times, place it in an oven at 60°C to dry it for 12 h, and recover the esterified modified flax fiber loaded with BiFeO3 nanocrystals.
4. The method for modifying plant fiber according to any one of claims 1 to 2, characterized in that: Prepare as follows: (1) Wash plant fiber ramie fiber with deionized water for 5 times, dry it at 50 °C, and cut it into 10 mm small pieces; (2) Add 11.00 parts by weight of the plant fiber segments obtained in step (1), 0.40 parts by weight of Fe(NO3)3·9H2O and 0.48 parts by weight of Bi(NO3)3·5H2O to 85.89 parts by weight of deionized water, stir evenly, and then add 2.23 parts by weight of 25 wt% KOH solution dropwise under strong stirring; continue stirring for 60 min, transfer the obtained mixed solution to a hydrothermal reactor, seal the hydrothermal reactor, react at 170°C for 6 h, and naturally cool to room temperature after the reaction to obtain a water dispersion of plant fibers loaded with BiFeO3 nanocrystals; (3) Add 3.00 parts by weight of lauric acid to the aqueous dispersion of plant fibers loaded with BiFeO3 nanocrystals obtained in step (2), and stir evenly; seal the hydrothermal reactor, and react at 90°C for 4 h; after the reaction is completed, naturally cool to room temperature, filter to obtain a solid substance, wash it repeatedly with ethanol and deionized water for 3 times, place it in an oven at 80°C for 10 h, and recover the BiFeO3 nanocrystal-loaded lauric acid-modified ramie fiber material.
5. The method for modifying plant fiber according to any one of claims 1 to 2, characterized in that: Prepare as follows: (1) washing plant fibers with deionized water for 4 times, wherein the mixture of the plant fibers, flax fibers and ramie fibers, has a mass ratio of 1:1, is dried at 40° C., and cut into 8 mm small segments; (2) Add 9.00 parts by weight of the plant fiber segments obtained in step (1), 0.30 parts by weight of Fe(NO3)3·9H2O and 0.36 parts by weight of Bi(NO3)3·5H2O to 88.66 parts by weight of deionized water, stir evenly, and then add 1.68 parts by weight of 25 wt% KOH solution dropwise under strong stirring; continue stirring for 45 min, transfer the obtained mixed solution to a hydrothermal reactor, seal the hydrothermal reactor, react at 160°C for 8 h, and naturally cool to room temperature after the reaction to obtain a water dispersion of plant fibers loaded with BiFeO3 nanocrystals; (3) Add 2.50 parts by weight of oleic acid to the aqueous dispersion of plant fibers loaded with BiFeO3 nanocrystals obtained in step (2), and stir evenly; seal the hydrothermal reactor, and react at 85°C for 6 h; after the reaction is completed, naturally cool to room temperature, filter to obtain a solid substance, wash it repeatedly with ethanol and deionized water for 3 times, and dry it in an oven at 70°C for 11 h to obtain a composite material of flax fiber and ramie fiber loaded with BiFeO3 nanocrystals oleic acid ester.
6. A plant fiber, characterized in that: The plant fiber loaded with BiFeO3 nanocrystals is esterified and modified by the modification method described in any one of claims 1 to 5.