A life assessment method for battery connection harness of energy storage system

By obtaining the relationship between thermal aging and thermal cycle life and temperature, combined with current impact testing, the problem of inaccurate life assessment of battery connection harnesses in energy storage systems is solved, and more accurate life assessment and processing quality assessment are achieved.

CN115684754BActive Publication Date: 2024-10-29SHENZHEN BYD LITHIUM BATTERY
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202110832411.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-07-22
Publication Date
2024-10-29
Estimated Expiration
2041-07-22

AI Technical Summary

Technical Problem

The existing technology cannot accurately evaluate the life of the battery connection harness of the energy storage system, mainly because it ignores the impact of the battery connection harness processing and the impact of current impact on the life.

Method used

By obtaining the corresponding relationship between thermal aging life and temperature, as well as the corresponding relationship between thermal cycle life and temperature, and combining the accelerated test method with the dual factors of temperature and current impact, the service life of the battery connection harness of the energy storage system is evaluated.

Benefits of technology

The accuracy of life assessment is improved, the failure conditions are closer to actual applications, the assessment results are more accurate, and the processing quality of the finished battery connection harness can be quickly evaluated, and the optimized processor or process can be selected.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115684754B_ABST
    Figure CN115684754B_ABST
Patent Text Reader

Abstract

The present application discloses a life assessment method for a battery connection harness of an energy storage system, the life assessment method comprising: obtaining a first correspondence between thermal aging life and temperature; obtaining the thermal aging life of the battery connection harness to be tested at an actual working temperature according to the first correspondence; obtaining a second correspondence between thermal cycle life and temperature; obtaining the thermal cycle life of the battery connection harness to be tested at an actual working temperature according to the second correspondence; and assessing the service life of the battery connection harness of the energy storage system according to the thermal aging life and the thermal cycle life. The life assessment method combines the accelerated testing method of the dual factors of temperature and current impact, and the test of the finished battery connection harness has a significant acceleration effect compared to the current simple thermal aging test.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of energy storage systems, and in particular to a life assessment method for a battery connection harness of an energy storage system. Background Art

[0002] With the rapid development of the energy storage industry, the capacity and power of energy storage systems are increasing, and the operating current and voltage are gradually increasing. Therefore, reliable connections within energy storage systems are becoming more and more important. Compared with other electrical equipment, energy storage systems have more stringent requirements on the reliability of battery connections, because the connection impedance of battery connection harnesses increases after aging, and a large amount of heat is generated under continuous high current, which can easily cause thermal runaway of the battery and cause fire accidents. Therefore, it is very important to accurately evaluate the service life of the battery connection harness.

[0003] At present, the evaluation of the service life of the battery connection harness mainly focuses on the plug-in life of the connector and the insulation life of the battery connection harness:

[0004] Usually, when evaluating the plug-in life of a connector, the number of times the connector can be reliably plugged in and out is evaluated through experience based on the plating material and plating thickness between the plug and socket, the matching tolerance, etc., or actual tests are performed to record the number of plug-in and plug-out times that reach the failure state (plug-in force, contact resistance, etc. reach the failure threshold);

[0005] Usually, when evaluating the insulation life of the battery connection harness, a thermal aging test is performed under high temperature conditions to accelerate the aging and failure of the insulation layer (elongation at break <50%, cable weight loss >10%). The insulation life of the battery connection harness under normal operating temperature is estimated using the aging model formula.

[0006] The current rapid life assessment method for battery connection harnesses is limited to the insulation layer and connector level, ignoring the impact of battery connection harness processing. Therefore, the life of the battery connection harness of the energy storage system cannot be accurately assessed according to the existing method.

[0007] Therefore, it is necessary to improve the current technical solution to avoid the above problems. Summary of the invention

[0008] In view of the problem of inaccurate life assessment of a battery connection harness of an energy storage system in the prior art, the present invention provides a life assessment method for a battery connection harness of an energy storage system, the life assessment method comprising:

[0009] Obtaining a first correspondence between thermal aging life and temperature;

[0010] Obtaining the thermal aging life of the battery connection harness to be tested at the actual working temperature according to the first corresponding relationship;

[0011] Obtaining a second corresponding relationship between thermal cycle life and temperature;

[0012] Obtaining the thermal cycle life of the battery connection harness to be tested at the actual working temperature according to the second corresponding relationship;

[0013] The service life of the battery connection harness of the energy storage system is evaluated according to the thermal aging life and the thermal cycle life.

[0014] Optionally, the method for obtaining the first corresponding relationship between the thermal aging life and the temperature includes:

[0015] Obtain the thermal aging failure time of the battery connection harness to be tested when it is heated to multiple different temperatures;

[0016] The relationship curve between the thermal aging life and temperature is determined according to the thermal aging failure time and the corresponding temperature to obtain the first corresponding relationship.

[0017] Optionally, the step of obtaining the thermal aging failure time of the battery connection harness to be tested when the harness itself is heated to a plurality of different temperatures includes:

[0018] Setting a plurality of different temperatures and calculating the current values ​​corresponding to heating the battery connection harness to be tested to the plurality of different temperatures;

[0019] adjusting the current to a current value corresponding to a set temperature and heating the battery connection harness to be tested based on the current so that the battery connection harness to be tested reaches a target temperature and lasts for a predetermined time to perform a thermal aging test;

[0020] The contact resistance change rate and / or the normal temperature temperature rise change value of the battery connection harness to be tested before and after the thermal aging test are compared to determine whether the battery connection harness to be tested has failed.

[0021] Optionally, determining whether the connection harness of the battery to be tested fails includes:

[0022] If the contact resistance change rate of the battery connection harness to be tested before and after the thermal aging test is greater than a set threshold, the battery connection harness to be tested fails; and / or

[0023] If the temperature rise change value of the battery connection harness to be tested before and after the thermal aging test is greater than a set threshold, the battery connection harness to be tested fails.

[0024] Optionally, if the connection harness of the battery to be tested fails, the thermal aging failure time is recorded;

[0025] If the battery connection harness to be tested has not failed, the thermal aging test is repeated until the battery connection harness to be tested fails, and the thermal aging failure time is recorded.

[0026] Optionally, the lifespan assessment method further includes:

[0027] Before the thermal aging test, performing a contact resistance test and / or a normal temperature temperature rise test on the battery connection harness to be tested;

[0028] After the heat aging test, the contact resistance test and / or the room temperature temperature rise test are performed again under the same test conditions.

[0029] Optionally, the method for obtaining the second corresponding relationship between the thermal cycle life and the temperature includes:

[0030] Obtain the number of thermal cycles to failure of the battery connection harness under test at multiple different temperatures;

[0031] A relationship curve between the number of failure thermal cycles and the temperature is determined according to the number of failure thermal cycles and the corresponding temperature to obtain the second corresponding relationship.

[0032] Optionally, obtaining the thermal cycle life of the battery connection harness to be tested at the actual working temperature according to the second corresponding relationship includes:

[0033] Determining the number of thermal cycles to failure at the actual operating temperature according to the second corresponding relationship and the actual operating temperature;

[0034] The thermal cycle life at the actual operating temperature is determined according to the number of failure thermal cycles at the actual operating temperature and the number of shutdowns and starts of the energy storage system within a fixed period.

[0035] Optionally, obtaining the number of thermal cycles of failure of the battery connection harness to be tested at multiple different temperatures includes:

[0036] Placing the connection harness of the battery to be tested in an incubator and adjusting the temperature of the incubator to a plurality of different set temperatures;

[0037] Cyclically adjusting the current value of the battery connection harness to be tested to a target current at a plurality of different temperatures and then disconnecting the current for a predetermined time to perform a thermal cycle test;

[0038] The contact resistance change rate and / or the normal temperature temperature rise change value of the battery connection harness to be tested before and after the thermal cycle test are compared to determine whether the battery connection harness to be tested has failed.

[0039] Optionally, determining whether the connection harness of the battery to be tested fails includes:

[0040] If the contact resistance change rate of the battery connection harness to be tested before and after the thermal cycle test is greater than a set threshold, the battery connection harness to be tested fails; and / or

[0041] If the temperature rise change value of the battery connection harness to be tested before and after the thermal cycle test is greater than a set threshold, the battery connection harness to be tested fails.

[0042] Optionally, if the connection harness of the battery to be tested fails, the number of thermal cycles to failure is recorded;

[0043] If the battery connection harness to be tested has not failed, the thermal cycle test is repeated until the battery connection harness to be tested fails, and the number of thermal cycles to failure is recorded.

[0044] Optionally, the lifespan assessment method comprises:

[0045] Before the thermal cycle test, performing a contact resistance test and / or a normal temperature temperature rise test on the battery connection harness to be tested;

[0046] After the thermal cycle test, the contact resistance test and / or the normal temperature temperature rise test are performed again under the same test conditions.

[0047] Optionally, evaluating the service life of the battery connection harness of the energy storage system according to the thermal aging life and the thermal cycle life includes:

[0048] The average values ​​of the thermal aging life and the thermal cycle life are determined to obtain the service life of the battery connection harness of the energy storage system.

[0049] Optionally, when acquiring the first corresponding relationship or the second corresponding relationship, the method includes:

[0050] Connect one end of the battery harness to be tested to the DC output terminal;

[0051] Connect the other end of the battery harness to be tested to the copper busbar.

[0052] Optionally, the number of the battery connection harnesses to be tested is greater than or equal to 2, and the battery connection harnesses to be tested are connected in series.

[0053] In order to solve the current technical problem of inaccurate life assessment of battery connection harnesses of energy storage systems, the present invention provides a life assessment method for battery connection harnesses of energy storage systems. The life assessment method combines the accelerated testing method of temperature and current impact dual factors, and uses the finished battery connection harness test, which has an obvious acceleration effect compared to the current simple thermal aging test.

[0054] The existing methods for evaluating the life of battery connection harnesses are all evaluated separately from the material level, such as through the plug-in life of the connector and the insulation life of the battery connection harness. The present invention has the following advantages over the prior art: the accelerated test model is improved, the failure conditions are closer to the actual application of the energy storage system, and the evaluation results are more accurate; the two factors of thermal aging and current shock are combined, the acceleration effect is obvious, and the evaluation results are more accurate; the influencing factors of the battery connection harness and connector are comprehensively considered from the level of the finished battery connection harness, and the results are more accurate than the conventional method of simply evaluating the life of the material level; the processing quality of the finished battery connection harness can be quickly evaluated, and the processor can be selected or the processing technology can be optimized based on this. BRIEF DESCRIPTION OF THE DRAWINGS

[0055] The following drawings of the present invention are used as part of the present invention for understanding the present invention. The drawings show embodiments of the present invention and their descriptions, and are used to explain the life evaluation method of the battery connection harness of the energy storage system of the present invention. In the drawings,

[0056] Figure 1 It is a schematic flow chart of a method for evaluating the life of a battery connection harness of an energy storage system in one embodiment of the present invention;

[0057] Figure 2 A flowchart of a method for evaluating the life of a battery connection harness of an energy storage system in another embodiment of the present invention;

[0058] Figure 3 A schematic diagram of a test bench structure for life evaluation of a battery connection harness of an energy storage system in another embodiment of the present invention;

[0059] Figure 4 It is a schematic diagram of a relationship curve between thermal aging life and temperature in a life assessment method for a battery connection harness of an energy storage system in one embodiment of the present invention;

[0060] Figure 5 It is a schematic diagram of a relationship curve between the number of failure thermal cycles and temperature in a life assessment method for a battery connection harness of an energy storage system in one embodiment of the present invention. DETAILED DESCRIPTION

[0061] In the following description, a large number of specific details are provided to provide a more thorough understanding of the present invention. However, it is apparent to those skilled in the art that the present invention can be implemented without one or more of these details. In other examples, in order to avoid confusion with the present invention, some technical features well known in the art are not described.

[0062] It should be understood that the present invention can be implemented in different forms and should not be construed as being limited to the embodiments presented herein. On the contrary, providing these embodiments will make the disclosure thorough and complete, and will fully convey the scope of the present invention to those skilled in the art. In the accompanying drawings, the sizes and relative sizes of layers and regions may be exaggerated for clarity.

[0063] The purpose of the terms used herein is only to describe specific embodiments and is not intended to be limiting of the present invention. When used herein, the singular forms "a", "an" and "said / the" are also intended to include plural forms, unless the context clearly indicates otherwise. It should also be understood that the terms "consisting of" and / or "comprising", when used in this specification, determine the presence of the features, integers, steps, operations, but do not exclude the presence or addition of one or more other features, integers, steps, operations and / or groups. When used herein, the term "and / or" includes any and all combinations of the relevant listed items.

[0064] In order to fully understand the present invention, a detailed structure will be presented in the following description to illustrate the technical solution proposed by the present invention. The preferred embodiments of the present invention are described in detail below, but in addition to these detailed descriptions, the present invention may also have other implementations.

[0065] At present, the evaluation of the service life of battery connection harnesses mainly focuses on the plug-in life of connectors and the insulation life. Evaluating the service life of battery connection harnesses by the plug-in life of connectors has the following disadvantages:

[0066] (1) If a dedicated test device is used for testing, the equipment needs to be customized, and the development cost is high;

[0067] (2) This method is only applicable to the life assessment of wiring harnesses that are frequently plugged and unplugged (the battery connection wiring harness is plugged and unplugged 1-2 times a year, so this method is not accurate in assessing the life span).

[0068] Evaluating the battery connection harness life by insulation life has the following disadvantages:

[0069] (1) The impact of current shock on the service life of the battery connection harness is not evaluated, which is not accurate enough for the battery connection harness;

[0070] (2) The impact of the crimping and welding quality of the battery connection harness terminals on the service life of the battery connection harness was not evaluated, and the processing quality assessment was not considered to be inaccurate;

[0071] (3) There is a lack of assessment of the impact of the increase in connector contact resistance due to aging on the life of the overall battery connection harness, and the assessment is not accurate enough.

[0072] The inventors have analyzed and tested the causes of the shortcomings in the above methods and found that the current rapid life assessment method for battery connection harnesses is limited to the material and connector levels, ignoring the impact of battery connection harness processing, and the failure indicators (cable tensile strength, elongation at break, breakdown voltage) are not applicable to energy storage systems. Usually, the material level of the battery connection harness has not aged, but the crimping or connector mating has failed (contact impedance, temperature rise exceeds the standard). Therefore, the existing method cannot accurately assess the life of the battery connection harness of the energy storage system.

[0073] In order to solve the problems existing in the current method, the present application provides a method for evaluating the life of a battery connection harness of an energy storage system, such as Figure 1 As shown, the life assessment method includes:

[0074] Step S1: obtaining a first corresponding relationship between thermal aging life and temperature;

[0075] Step S2: obtaining the thermal aging life of the battery connection harness to be tested at the actual working temperature according to the first corresponding relationship;

[0076] Step S3: obtaining a second corresponding relationship between thermal cycle life and temperature;

[0077] Step S4: obtaining the thermal cycle life of the battery connection harness to be tested at the actual working temperature according to the second corresponding relationship;

[0078] Step S5: evaluating the service life of the battery connection harness of the energy storage system according to the thermal aging life and the thermal cycle life.

[0079] The present invention provides a life assessment method for a battery connection harness of an energy storage system. The life assessment method combines an accelerated test method of temperature and current impact dual factors, and uses a finished battery connection harness test compared to the current simple thermal aging test, and the acceleration effect is obvious. Existing methods for assessing the life of a battery connection harness are all separate assessments from the material level, such as through the plug-in life of the connector and the insulation life of the battery connection harness. The present invention has the following advantages over the prior art: an improved accelerated test model, failure conditions are closer to the actual application of the energy storage system, and the assessment results are more accurate; the two factors of thermal aging and current impact are combined, the acceleration effect is obvious, and the assessment results are more accurate; the influencing factors of the battery connection harness and the connector are comprehensively considered from the level of the finished battery connection harness, and the results are more accurate than the conventional method of simply assessing the life of the material level; the processing quality of the finished battery connection harness can be quickly assessed, and the processor can be selected or the processing technology can be optimized based on this.

[0080] The following is a detailed description of the life evaluation method of the battery connection harness of the energy storage system described in this application in conjunction with the accompanying drawings, wherein Figure 1It is a schematic flow chart of a method for evaluating the life of a battery connection harness of an energy storage system in one embodiment of the present invention; Figure 2 A schematic flow chart of a method for evaluating the life of a battery connection harness of an energy storage system in another embodiment of the present invention; Figure 3 A schematic diagram of a test bench structure for life evaluation of a battery connection harness of an energy storage system in another embodiment of the present invention; Figure 4 It is a schematic diagram of a relationship curve between thermal aging life and temperature in a life assessment method for a battery connection harness of an energy storage system in one embodiment of the present invention; Figure 5 It is a schematic diagram of a relationship curve between the number of failure thermal cycles and temperature in a life assessment method for a battery connection harness of an energy storage system in one embodiment of the present invention.

[0081] In the present application, the first corresponding relationship can be a curve of the relationship between the thermal aging life and the temperature, or a list of the one-to-one correspondence between the thermal aging life and the temperature, and is not limited to a certain form. It can reflect the relationship between the two and can obtain the thermal aging life according to the actual working temperature. In the subsequent embodiments, the curve of the relationship between the thermal aging life and the temperature is used as an example for explanation and description, but it should be noted that it is not limited to this example. Similarly, the subsequent second corresponding relationship is a curve of the relationship between the number of failure thermal cycles and the temperature, but it is not limited to this example and will not be repeated later.

[0082] In this application, the thermal aging life is the time it takes for the battery connection harness to be tested to be affected by thermal factors and to age and fail. The thermal cycle life is the number of cycles in which the battery connection harness to be tested is affected by thermal factors and circulating current impact factors and to age and fail. Unless otherwise specified, the meanings of the thermal aging life and the thermal cycle life refer to this explanation.

[0083] In order to obtain the first corresponding relationship and the second corresponding relationship in the method described in the present application, the present application establishes an improved accelerated test model, combining the temperature and current impact, the most important aging factors of the battery connection harness, to simulate the actual working conditions of the battery connection harness to the greatest extent. The model is as follows:

[0084] The life τ is defined as the time when the battery connection harness reaches the failure state. The Arrhenius empirical formula is improved to establish the temperature acceleration test model:

[0085]

[0086] R: molar gas constant (8.314 J / (mol·K));

[0087] T: thermodynamic temperature (K);

[0088] Ea: activation energy (J / mol)

[0089] A: Pre-exponential factor (Arrhenius constant)

[0090] Among them, Ea and A are obtained from experiments. According to multiple groups of test data, a linear regression equation can be fitted to obtain the relationship curve between thermal aging life and temperature (such as Figure 4 as shown) and the relationship between the number of thermal cycles to failure and temperature (as shown Figure 5 As shown). The relationship curve is usually a straight line, where the slope of the straight line is Ea / R, and the intercept with the y-axis is lnA. The relationship curve between thermal aging life and temperature and the relationship curve between failure thermal cycle number and temperature have different acceleration factors, so the linear equations obtained are also different, and the specific values ​​of Ea and A will also be different.

[0091] From the equation, we can see that the logarithm of life is the inverse of temperature. It is a linear relationship. The equation curve can be seen in Figure 4 .

[0092] The number of current shocks N is defined as the number of times the battery connection harness reaches a failure state, and an improved current shock acceleration test model is established:

[0093]

[0094] From the equation, we can see that the logarithm of the number of current surges is the inverse of the temperature. It is a linear relationship. The equation curve can be seen in Figure 5 .

[0095] The life evaluation method described in this application can combine the test data of thermal aging and thermal cycling experiments to obtain a calculated life that is closer to the actual working conditions, as follows:

[0096] ① Calculate the thermal aging life: According to the failure time τ1, τ2, τ3 of the battery connection harness at three different temperatures T obtained from the test, draw Thermal aging life-temperature relationship curve, such as Figure 4 ; Linear fitting gives the univariate regression equation of the logarithm of life and the inverse of temperature:

[0097]

[0098] Substituting the actual operating temperature into the equation, the corresponding service life τ1 can be obtained.

[0099] ② Calculate thermal cycle life: According to the number of failure thermal cycles N1, N2, and N3 at three different temperatures T obtained from the test, plot Thermal cycle number-temperature relationship curve, such as Figure 5 ; Linear fitting gives the univariate regression equation of the logarithm of the number of thermal cycles and the inverse of temperature:

[0100]

[0101] Substituting the actual working temperature into the equation, the corresponding number of failure thermal cycles N can be obtained, and the service life τ2 can be calculated.

[0102] (n: the number of system starts and stops at a fixed cycle, for example, the number of system starts and stops per year)

[0103] ③ Comprehensive evaluation of lifespan

[0104] The estimated life of single thermal aging life and thermal cycle life has a large error with the actual life, so the theoretical life τ after combining the two is:

[0105]

[0106] The method is described in detail below in conjunction with steps S1-S5.

[0107] In the step S1, a first corresponding relationship between the thermal aging life and the temperature is obtained, wherein the corresponding relationship is a relationship curve between the thermal aging life and the temperature, and a method for obtaining the relationship curve between the thermal aging life and the temperature includes: obtaining the thermal aging failure time of the battery connection harness to be tested at multiple different temperatures; and determining the relationship curve between the thermal aging life and the temperature according to the thermal aging failure time and the temperature.

[0108] Among them, multiple different temperatures can be selected according to actual needs. The highest value of the set temperature can be the highest operating temperature of the battery connection harness, and then decreases with a fixed difference. For example, in one embodiment of the present application, 120°C is the highest operating temperature (working temperature -40°C ~ 125°C, wire diameter 4AWG) (to ensure that the temperature rise error does not exceed 125°C), and 100°C and 80°C are taken at a fixed difference interval of 20°C. It should be noted that the more the number of set temperatures, the more accurate the relationship curve between the thermal aging life and the temperature. Therefore, if there are enough test benches and samples, the test temperature can be increased and the fixed difference can be reduced to obtain more experimental data and improve accuracy.

[0109] In this application, the temperature of the battery connection harness is raised to a set temperature by adjusting the current. Figure 2 Provide a detailed description.

[0110] Specifically, first: build the test bench. The test bench topology is as shown in the attached Figure 3 The figure shows a DC high current test bench, which can provide a stable DC high current; the DC output terminal is connected in series to the battery connection harness 1 to be tested, wherein at least two harnesses are connected in series at each temperature to prevent accidental errors and improve measurement accuracy.

[0111] Among them, the battery connection harness 1 to be tested is connected by a copper busbar 4 to eliminate the abnormal temperature rise that interferes with the test data due to the small cross-sectional area of ​​the contact surface, thereby improving the accuracy of the evaluation result. In different embodiments of the present application, copper busbars 4 with different cross-sectional areas are selected for cables of different specifications. For example, a 4AWG cable uses a cross-sectional area of ​​50mm 2 The copper bar of the cable specification increases, and the cross-sectional area of ​​the copper bar increases accordingly. For example, the cross-sectional area of ​​2AWG cable is 70mm 2 Copper busbar, 1AWG cable with cross-sectional area of ​​100mm 2 of copper busbar.

[0112] The above setting not only evaluates the aging of the battery connection harness during the thermal aging life assessment, but also evaluates the crimping point 2 of the battery connection harness and the overlapping point 3 between the battery connection harness and the copper busbar, thereby simulating the actual working conditions of the battery connection harness to the greatest extent. This can effectively solve the shortcomings of the current conventional life assessment method, and the calculated life is more accurate.

[0113] Second: calculate the current values ​​corresponding to multiple different temperatures, and pass a large current to make the conductor of the battery connection harness reach the set temperature. In order to be closer to the actual failure environment, this application is different from the conventional high-temperature box heating aging. A large current is used to heat the battery connection harness. By using a large current for heating, the heating speed is fast and the energy consumption is low.

[0114] To ensure the accuracy of the test results, the thermal aging test is conducted at least at three different temperatures (the temperature reached by the internal part of the battery connection harness conductor through current heating). In one example, the three test temperatures are set to 120°C, 100°C, and 80°C (the temperature fluctuation range is controlled within 5°C).

[0115] According to the law of conservation of energy, the heat generation formula of the conductor in equilibrium state is as follows:

[0116] Q R =Q C +Q r

[0117] Q R : Heat generated by conductor resistance

[0118] Q C :Conductor heat removed by air convection (wind speed < 0.2m / s)

[0119] Q r :Thermal radiation heat dissipation of conductor

[0120] Q R =I 2 R

[0121] Q C=αF(θ W -θ0)

[0122]

[0123] α: Convection heat dissipation coefficient, α = 1.5 (θ W -θ0) 0.35

[0124] F: The heat dissipation area of ​​the conductor per unit length, determined by the conductor itself

[0125] ε: radiation coefficient of conductor material

[0126] θ W : The stable temperature of the conductor after a large current is passed

[0127] θ0: Initial ambient temperature

[0128] Combining the above equations, we can get the working current equation under different temperature rises:

[0129]

[0130] The calculation can be obtained:

[0131] Test currents I1, I2, and I3 when the battery connection harness conductor reaches 120°C, 100°C, and 80°C;

[0132] Third: before the thermal aging test, the battery connection harness to be tested is subjected to a contact resistance test and / or a normal temperature temperature rise test; after the thermal aging test, the contact resistance test and / or the normal temperature temperature rise test is performed again under the same test conditions.

[0133] Specifically, the contact resistance test and / or the normal temperature temperature rise test includes the following steps:

[0134] Contact resistance test: adjust the high current test bench to the rated current. After the current output is stable, use a high-precision multimeter to test the voltage (millivolts) at both ends of the cable, use a current clamp to test the current (A) flowing through, and calculate the on-resistance R=U / I.

[0135] Normal temperature temperature rise test: adjust the high current test bench to the rated current until the cable temperature is stable, record the data every 20 minutes, and observe the temperature data in real time. Test time: 4 hours. If the temperature rise of each point has not reached equilibrium after 4 hours of testing, it needs to be extended to 6 hours (temperature rise balance judgment: temperature rise does not exceed 1 degree Celsius within 1 hour) (performed at normal temperature of 25 degrees Celsius).

[0136] The contact resistance test and / or normal temperature temperature rise test are both tested at a rated working current of 80A, and the test data are recorded.

[0137] Fourth: Conduct a thermal aging test, starting from a rated working current of 80A and gradually increasing it to the current calculated in the second step until the conductor temperature of the battery connection harness reaches the set target temperature; turn off the power every 24 hours to cool to room temperature, then conduct a contact resistance test and a temperature rise test at a current of 80A, and record the data.

[0138] Fifth: comparing the contact resistance change rate and / or room temperature temperature rise change value of the battery connection harness to be tested before and after the thermal aging test to determine whether the battery connection harness to be tested is failed.

[0139] In one embodiment of the present application, if any one of the contact resistance change rate and the temperature rise change value at room temperature is abnormal, it is determined that the connection harness of the battery to be tested has failed.

[0140] Determining whether the connection harness of the battery to be tested fails includes:

[0141] If the contact resistance change rate of the battery connection harness to be tested before and after the thermal aging test is greater than a set threshold, the battery connection harness to be tested fails. The contact resistance change rate set threshold is 15%, that is, when the contact resistance change rate is greater than 15%, the battery connection harness to be tested fails, wherein the set threshold can be adjusted according to actual needs.

[0142] If the temperature rise change value of the battery connection harness under test before and after the thermal aging test is greater than the set threshold, the battery connection harness under test fails. The set threshold value of the temperature rise change value under test is 30K, that is, when the temperature rise is greater than 30K, the battery connection harness under test fails, wherein the set threshold value can be adjusted according to actual needs.

[0143] If the battery connection harness to be tested fails, the thermal aging failure times τ1, τ2, and τ3 at different temperatures are recorded; if the battery connection harness to be tested does not fail, the thermal aging test is repeated until the battery connection harness to be tested fails, and the thermal aging failure times τ1, τ2, and τ3 are recorded.

[0144] It should be noted that the thermal aging failure time does not include the static time of the battery connection harness to be tested, but only includes the time when the battery connection harness to be tested is heated to a preset temperature.

[0145] Sixth: Based on the failure times τ1, τ2, and τ3 of the battery connection harness at three different temperatures T obtained from the test, plot Life-temperature relationship curve, see Figure 4 ; Linear fitting gives the univariate regression equation of the logarithm of life and the inverse of temperature:

[0146]

[0147] In step S2, the actual operating temperature is substituted into the above-mentioned univariate regression equation, for example, 45°C, and the corresponding service life τ1 (45°C) can be obtained.

[0148] In step S3, a thermal cycle test is performed, which specifically includes the following steps:

[0149] First: Build the test bench. The test bench topology is as follows: Figure 3 As shown, unlike thermal aging test, thermal cycling test requires placing the test bench in a high temperature box to adjust the temperature.

[0150] Second: define the parameters of the test bench, set the current impact I to the rated working current of 80A, and define three test temperatures of 120℃, 100℃, and 80℃ (the temperature fluctuation range is controlled within 5℃).

[0151] Third: Conduct contact resistance test and / or normal temperature temperature rise test on the battery connection harness to be tested, test at rated working current of 80A, and record the test data.

[0152] Fourth: Thermal cycle test, adjust the temperature of the high temperature box to the target temperature, gradually increase the high current test bench from 0A to 80A, stabilize at 80A for at least 15 minutes, then cut off the power for 15 minutes before restarting the current.

[0153] In one embodiment of the present application, before the thermal cycle test, the battery connection harness to be tested is subjected to a contact resistance test and / or a normal temperature temperature rise test; after the thermal cycle test, the contact resistance test and / or the normal temperature temperature rise test is performed again under the same experimental conditions to obtain the contact resistance and normal temperature temperature rise before and after the thermal cycle test, and by calculating the difference in contact resistance before and after the thermal cycle test and the difference in temperature rise at normal temperature, the contact resistance change rate and the normal temperature temperature rise change value are obtained.

[0154] In order to improve the test efficiency, after repeating the charge-power-off operation 20 times, the high temperature box can be adjusted to room temperature, and a contact resistance test and / or a room temperature temperature rise test can be performed at a current of 80A, and the data can be recorded. The number of times is not limited to a certain numerical range, for example, any one of 1-20 can be selected, and after repeating the charge-power-off operation 20 times, a contact resistance test and / or a room temperature temperature rise test can be performed after each charge-power-off operation.

[0155] Fifth: judging whether the connection harness of the battery to be tested is failed includes:

[0156] If the initial contact resistance change rate of the battery connection harness to be tested before and after the thermal cycle test is greater than a set threshold, the battery connection harness to be tested fails. The contact resistance change rate set threshold is 15%, that is, when the contact resistance change rate is greater than 15%, the battery connection harness to be tested fails, wherein the set threshold can be adjusted according to actual needs.

[0157] If the temperature rise change value of the battery connection harness under test before and after the thermal cycle test is greater than the set threshold, the battery connection harness under test fails. The set threshold value of the temperature rise change value under test is 30K, that is, when the temperature rise is greater than 30K, the battery connection harness under test fails, wherein the set threshold value can be adjusted according to actual needs.

[0158] If the connection harness of the battery to be tested fails, the number of thermal cycles of failure N1, N2, N3 is recorded;

[0159] If the battery connection harness to be tested has not failed, the thermal cycle test is repeated until the battery connection harness to be tested fails, and the number of thermal cycles to fail N1, N2, and N3 are recorded.

[0160] According to the number of failure thermal cycles N1, N2, and N3 at three different temperatures T obtained from the test, plot Thermal cycle number-temperature relationship curve, see Figure 5 ; Linear fitting gives the univariate regression equation of the logarithm of the number of thermal cycles and the inverse of temperature:

[0161]

[0162] In step S4, obtaining the thermal cycle life at the actual working temperature according to the second corresponding relationship includes: obtaining the number of failure thermal cycles at the actual working temperature according to the second corresponding relationship, for example, substituting the actual working temperature into the above-mentioned univariate regression equation, for example, when the actual working temperature is 45°C, the corresponding number of failure thermal cycles N can be obtained.

[0163] Then, the thermal cycle life at the actual working temperature, for example, the thermal cycle life τ2, is calculated according to the number of failure thermal cycles at the actual working temperature and the number of shutdowns and starts of the energy storage system within a fixed period. (n: the number of system starts and stops in a fixed period, for example, the number of system starts and stops per year). In one embodiment of the present application, (The system is charged and discharged once a day).

[0164] It should be noted that the construction of the test bench in the thermal cycle test, the connection method of the battery connection harness, the selection of temperature, the specific method of the contact resistance test and / or the room temperature temperature rise test, and the drawing of the relationship curve can all refer to the relevant introduction in the thermal aging test. If there is no contradiction, the relevant instructions and explanations can be introduced into the thermal cycle test and will not be repeated here.

[0165] In step S5, the service life of the battery connection harness to be tested is comprehensively evaluated. In this application, the service life is estimated by combining thermal aging and thermal cycling, and the theoretical service life of the finished battery connection harness to be tested at the actual working temperature can be obtained. For example, when the actual working temperature is 45°C, the estimated service life is:

[0166]

[0167] The life assessment method described in this application uses the failure indicators of the battery connection harness to be tested (contact impedance, temperature rise exceeding the standard) instead of the currently commonly used failure indicators (cable tensile strength, elongation at break, breakdown voltage), which can effectively solve the shortcomings of the current conventional life assessment method and the calculated life is more accurate. The method combines the accelerated test method of temperature and current impact dual factors, uses the finished harness test, and has a significant acceleration effect compared to the current simple thermal aging test.

[0168] Compared with the prior art, the present invention has the following advantages: the accelerated test model is improved, the failure conditions are closer to the actual application of the energy storage system, and the evaluation results are more accurate; the two factors of thermal aging and current impact are combined, the acceleration effect is obvious, and the evaluation results are more accurate; the influencing factors of cables and connectors are comprehensively considered from the finished wire harness level, and the results are more accurate than the conventional method of simply evaluating the life of the material level; the processing quality of the finished wire harness can be quickly evaluated, and the processor can be selected or the processing technology can be optimized based on this.

[0169] Although example embodiments have been described herein with reference to the accompanying drawings, it should be understood that the above example embodiments are merely exemplary and are not intended to limit the scope of the present invention thereto. Various changes and modifications may be made therein by one of ordinary skill in the art without departing from the scope and spirit of the present invention. All such changes and modifications are intended to be included within the scope of the present invention as required by the appended claims.

[0170] In the description provided herein, a large number of specific details are described. However, it is understood that embodiments of the present invention can be practiced without these specific details. In some instances, well-known methods, structures and techniques are not shown in detail so as not to obscure the understanding of this description.

[0171] Similarly, it should be understood that in order to streamline the present invention and help understand one or more of the various inventive aspects, in the description of the exemplary embodiments of the present invention, the various features of the present invention are sometimes grouped together into a single embodiment, figure, or description thereof. However, the method of the present invention should not be interpreted as reflecting the following intention: the claimed invention requires more features than the features explicitly stated in each claim. More specifically, as reflected in the corresponding claims, the inventive point is that the corresponding technical problem can be solved with less than all the features of a single disclosed embodiment. Therefore, the claims following the specific embodiment are hereby expressly incorporated into the specific embodiment, wherein each claim itself serves as a separate embodiment of the present invention.

[0172] It will be understood by those skilled in the art that, except for mutually exclusive features, all features disclosed in this specification (including the accompanying claims, abstracts and drawings) and all processes or units of any method or device disclosed in this specification may be combined in any combination. Unless otherwise expressly stated, each feature disclosed in this specification (including the accompanying claims, abstracts and drawings) may be replaced by an alternative feature that provides the same, equivalent or similar purpose.

[0173] In addition, those skilled in the art will appreciate that, although some embodiments described herein include certain features included in other embodiments but not other features, the combination of features of different embodiments is meant to be within the scope of the present invention and form different embodiments. For example, in the claims, any one of the claimed embodiments may be used in any combination.

[0174] It should be noted that the above embodiments illustrate rather than limit the invention, and that those skilled in the art may devise alternative embodiments without departing from the scope of the appended claims. In the claims, any reference symbol between brackets shall not be construed as a limitation on the claims. The invention may be implemented by means of hardware comprising a number of different elements and by means of a suitably programmed computer. In a unit claim enumerating a number of means, several of these means may be embodied by the same hardware item. The use of the words first, second, and third, etc., does not indicate any order. These words may be interpreted as names.

Claims

1. A method for evaluating the life of a battery connection harness of an energy storage system, characterized in that: The life assessment method comprises: Obtaining a first correspondence between thermal aging life and temperature; Obtaining the thermal aging life of the battery connection harness to be tested at the actual working temperature according to the first corresponding relationship; Obtaining a second corresponding relationship between thermal cycle life and temperature; including: obtaining the number of failure thermal cycles of the battery connection harness to be tested at multiple different temperatures; determining a relationship curve between the number of failure thermal cycles and the temperature according to the number of failure thermal cycles and the corresponding temperature to obtain the second corresponding relationship; The thermal cycle life of the battery connection harness to be tested at the actual working temperature is obtained according to the second corresponding relationship; including: determining the number of failure thermal cycles at the actual working temperature according to the second corresponding relationship and the actual working temperature; determining the thermal cycle life at the actual working temperature according to the number of failure thermal cycles at the actual working temperature and the number of shutdowns and starts of the energy storage system within a fixed period; wherein, obtaining the number of failure thermal cycles of the battery connection harness to be tested at multiple different temperatures includes: placing the battery connection harness to be tested in an incubator and adjusting the temperature of the incubator to multiple different set temperatures; cyclically adjusting the current value of the battery connection harness to be tested to a target current at multiple different temperatures and then disconnecting the current for a predetermined time, so as to perform a thermal cycle test; comparing the contact resistance change rate and / or the normal temperature temperature rise change value of the battery connection harness to be tested before and after the thermal cycle test, so as to determine whether the battery connection harness to be tested has failed; The service life of the battery connection harness of the energy storage system is evaluated according to the thermal aging life and the thermal cycle life.

2. The life assessment method according to claim 1, characterized in that: The method of obtaining the first corresponding relationship between the thermal aging life and the temperature includes: Obtain the thermal aging failure time of the battery connection harness to be tested when it is heated to multiple different temperatures; The relationship curve between the thermal aging life and temperature is determined according to the thermal aging failure time and the corresponding temperature to obtain the first corresponding relationship.

3. The life assessment method according to claim 2, characterized in that: The step of obtaining the thermal aging failure time of the battery connection harness to be tested when the harness is heated to a plurality of different temperatures includes: Setting a plurality of different temperatures and calculating current values ​​corresponding to heating the battery connection harness to be tested to the plurality of different temperatures; adjusting the current to a current value corresponding to a set temperature and heating the battery connection harness to be tested based on the current so that the battery connection harness to be tested reaches a target temperature and lasts for a predetermined time to perform a thermal aging test; The contact resistance change rate and / or the normal temperature temperature rise change value of the battery connection harness to be tested before and after the thermal aging test are compared to determine whether the battery connection harness to be tested has failed.

4. The life assessment method according to claim 3, characterized in that: Determining whether the connection harness of the battery to be tested fails includes: If the contact resistance change rate of the battery connection harness to be tested before and after the thermal aging test is greater than a set threshold, the battery connection harness to be tested fails; and / or If the temperature rise change value of the battery connection harness to be tested before and after the thermal aging test is greater than a set threshold, the battery connection harness to be tested fails.

5. The life assessment method according to claim 4, characterized in that: If the connection harness of the battery to be tested fails, the thermal aging failure time is recorded; If the battery connection harness to be tested has not failed, the thermal aging test is repeated until the battery connection harness to be tested fails, and the thermal aging failure time is recorded.

6. The life assessment method according to claim 3, characterized in that: The life assessment method further comprises: Before the thermal aging test, performing a contact resistance test and / or a normal temperature temperature rise test on the battery connection harness to be tested; After the heat aging test, the contact resistance test and / or the room temperature temperature rise test are performed again under the same test conditions.

7. The life assessment method according to claim 1, characterized in that: Determining whether the connection harness of the battery to be tested fails includes: If the contact resistance change rate of the battery connection harness to be tested before and after the thermal cycle test is greater than a set threshold, the battery connection harness to be tested fails; and / or If the temperature rise change value of the battery connection harness to be tested before and after the thermal cycle test is greater than a set threshold, the battery connection harness to be tested fails.

8. The life assessment method according to claim 7, characterized in that: If the connection harness of the battery to be tested fails, the number of thermal cycles to failure is recorded; If the battery connection harness to be tested has not failed, the thermal cycle test is repeated until the battery connection harness to be tested fails, and the number of thermal cycles to failure is recorded.

9. The life assessment method according to claim 1, characterized in that: The life assessment method comprises: Before the thermal cycle test, performing a contact resistance test and / or a normal temperature temperature rise test on the battery connection harness to be tested; After the thermal cycle test, the contact resistance test and / or the normal temperature temperature rise test are performed again under the same test conditions.

10. The life assessment method according to claim 1, characterized in that: Evaluating the service life of the battery connection harness of the energy storage system according to the thermal aging life and the thermal cycle life includes: The average values ​​of the thermal aging life and the thermal cycle life are determined to obtain the service life of the battery connection harness of the energy storage system.

11. The life assessment method according to any one of claims 1 to 10, characterized in that: When acquiring the first corresponding relationship or the second corresponding relationship, it includes: Connect one end of the battery harness to be tested to the DC output terminal; Connect the other end of the battery harness to be tested to the copper busbar.

12. The life assessment method according to claim 11, characterized in that: The number of the battery connection harnesses to be tested is greater than or equal to 2, and the battery connection harnesses to be tested are connected in series.

Citation Information

Patent Citations

  • Method for testing service life of medium-voltage solid insulation power cable

    CN101738572A

  • Traffic cable aging life evaluation system

    CN112964951A