Chemical conversion catalysts

By converting the unimodal ligand-metal precatalyst into a bimodal ligand-metal catalyst, the problem of difficulty in preparing bimodal polymers in a single reactor is solved, and efficient and simplified multimodal polymer preparation is achieved, improving operation and cost-effective.

CN115698105BActive Publication Date: 2024-11-08DOW GLOBAL TECHNOLOGIES LLC
View PDF 54 Cites 0 Cited by

Patent Information

Application Number
CN202180038123.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2021-04-01
Filing Date
2021-05-28
Publication Date
2024-11-08
Estimated Expiration
2041-05-28

AI Technical Summary

Technical Problem

The prior art is difficult to efficiently prepare bimodal polymers in a single polymerization reactor, and the use of multiple catalysts or reactor environmental methods is costly, complex and poorly operable.

Method used

Polymers with a wide molecular weight distribution are prepared using a single polymerization reactor by chemically converting the unimodal ligand-metal precatalyst to a bimodal ligand-metal catalyst under conditions of activator and modal increased organic compounds.

Benefits of technology

The efficient preparation of multimodal polymers with desired properties in a single reactor is achieved, simplifying the process flow, reducing costs, and improving operability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_4
    Figure SMS_4
  • Figure SMS_5
    Figure SMS_5
Patent Text Reader

Abstract

Embodiments of the present disclosure relate to converting a unimodal ligand-metal precatalyst into a bimodal ligand-metal catalyst. As an example, the present disclosure provides a method for chemically converting a unimodal ligand-metal precatalyst into a bimodal ligand-metal catalyst by combining, in any order, components consisting essentially of a first unimodal ligand-metal precatalyst, an effective amount of the activator, and an effective amount of the modality-enhanced organic compound under conditions effective for the activator and the modality-enhanced organic compound, chemically converting the first unimodal ligand-metal precatalyst into a bimodal ligand-metal catalyst, thereby preparing the bimodal ligand-metal catalyst, wherein the modality-enhanced organic compound has the formula (A 1 )、(B 1 ) or (C 1 ), as described in detail in this article.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] Olefin polymerization catalysts, processes and polyolefins prepared thereby. Background Art

[0002] The polymers can be used in many products, including films and pipes, as well as other types of products. Bimodal polymers have become increasingly important in the polyolefin industry, with many manufacturers offering this type of product. Polymers such as bimodal polymers with a broad molecular weight distribution can have improved physical and / or mechanical properties, such as stiffness, toughness, processability, and environmental stress crack resistance (ESCR), among others.

[0003] The comonomer content (i.e., the weight fraction amount of constituent units derived from 1-olefin in the copolymer) of most poly(ethylene-co-1-olefin) copolymers varies with the molecular weight of their constituent macromolecules. Basically, if the higher molecular weight fraction of the macromolecule has a lower weight % comonomer content, this is a normal comonomer distribution relative to the molecular weight. Normal comonomer distribution is also called normal short chain branching distribution (normal SCBD) or normal molecular weight comonomer distribution index (normal MWCDI). If the MWCDI is less than 0, there is a normal MWCDI or normal SCBD. If MWCDI=0, there is a flat MWCDI or flat SCBD. The MWCDI value is determined by a by plotting a linear regression of the comonomer content in weight percent (wt%) on the y-axis and Log (M) on the x-axis.

[0004] If the higher molecular weight fraction has a higher weight % comonomer content, this is a reverse comonomer distribution relative to the molecular weight. This is also called reverse short chain branching distribution (reverse SCBD), reverse molecular weight comonomer distribution index (reverse MWCDI) or broad-orthogonal composition distribution (BOCD). If the MWCDI is greater than 0, there is a reverse comonomer distribution or reverse SCBD. In addition, the MWCDI value quantifies the magnitude of the comonomer distribution.

[0005] The distribution of the content of these comonomers on molecular weight is shown by plotting the linear regression of the comonomer content in weight percent (wt%) on the y-axis and the Log (M) on the x-axis. The weight % comonomer content is determined by fast Fourier transform infrared (FT-IR) spectroscopy of the dissolved copolymer in a gel permeation chromatography (GPC) measurement using an infrared detector. M is a specific x-axis molecular weight point (10^[Log (M)]) of the Flory distribution of molecular weight, as measured by GPC. In such a figure, a normal comonomer distribution has a negative slope (i.e., a line (from left to right on the x-axis) fitted to the data points from a lower Log (M) value to a higher Log (M) value slopes downward). Summary of the invention

[0006] Bimodal polymers generally refer to polymers prepared using two or more different catalyst types or two or more different reactor environments (e.g., two or more polymerization reactors in series), so that the resulting polymer has a bimodal molecular weight distribution that typically includes a low molecular weight component and a high molecular weight component (having a molecular weight and / or molecular weight range that is relatively high than the low molecular weight component). However, the method using two or more different catalysts can lead to operability problems. For example, due to the different inherent initiation and / or decay kinetics of two or more catalysts, operability problems may occur. In addition, the method using two or more reactor environments may be costly, complicated and / or have other difficulties, such as those difficulties related to the difference in feed rate / position and / or the difference in reactor environment. In addition, in view of the industrial importance of this field, it is still necessary to provide an additional synthesis method for preparing a single reactor catalyst that can produce bimodal polymers in the absence of an additional catalyst.

[0007] Our technical solution to the above technical problem employs an effective amount of a modality-increasing organic compound to change the molecular structure of a unimodal ligand-metal precatalyst into a bimodal ligand-metal catalyst. The bimodal ligand-metal catalyst and / or a catalyst system comprising a bimodal ligand-metal catalyst (e.g., a bimodal catalyst system and / or a trimodal catalyst system) can be used in a single polymerization reactor to prepare a multimodal polymer having desired properties, such as a desired broad molecular weight distribution and / or a desired comonomer distribution between a high molecular weight polyethylene component and a low molecular weight polyethylene component of a bimodal polyethylene composition. This result is unpredictable. DETAILED DESCRIPTION

[0008] The entire content of the Summary section is incorporated herein by reference.Additional embodiments follow; some embodiments are numbered for ease of reference.

[0009] Aspect 1: A method for chemically converting a unimodal ligand-metal precatalyst to a bimodal ligand-metal catalyst, the method comprising combining, in any order, components consisting essentially of a first unimodal ligand-metal precatalyst, an effective amount of an activator, and an effective amount of a modality-enhanced organic compound under conditions effective for the activator and the modality-enhanced organic compound to chemically convert the first unimodal ligand-metal precatalyst to a bimodal ligand-metal catalyst, thereby preparing a bimodal ligand-metal catalyst; wherein the modality-enhanced organic compound has the formula (A 1 )、(B 1 ) or (C 1 ): R 5 -C≡CR 6 (A 1 )、(R 5 ) 2C=C=C(R 6 ) 2 (B 1 ) or (R 5 )(R 7 )C=C(R 6 )(R 7 )(C 1 );where R 5 and R 6 Each of which is independently H or R 7 ; and each R 7 Independently (C 1 -C 20 )alkyl, -C(=O)-O-(unsubstituted C 1 -C 20 ) alkyl), (C 1 -C 19 ) heteroalkyl or tri((C 1 -C 20 )alkyl)silyl, or two R 7 Combined to form (C 3 -C 8 ) alkylene; provided that each R 7 lacks a carbon-carbon double bond; each (C 1 -C 20 ) The hydrocarbon groups are independently unsubstituted or substituted by 1 to 4 groups R S Substituted; wherein each substituent group R S are independently selected from halogen (e.g., F), unsubstituted (C 1 -C 5 ) alkyl (e.g., CH 3 )、-C≡CH、-OH、(C 1 -C 5 )alkoxy, -C(=O)-(unsubstituted (C 1 -C 5 )alkyl), -NH 2 、-N(H)(unsubstituted(C 1 -C 5 ) alkyl), -N(unsubstituted(C 1 -C 5 )alkyl) 2 , -COOH, -C(=O)-NH 2 , -C(=O)-N(H)(unsubstituted(C 1 -C 5 ) alkyl), -C(=O)-N(unsubstituted (C 1 -C 5 )alkyl) 2 、-S-(unsubstituted(C 1 -C5 )alkyl), -S(=O) 2 -(Unsubstituted(C 1 -C 5 )alkyl), -S(=O) 2 -NH 2 、-S(=O) 2 -N(H)(Unsubstituted(C 1 -C 5 )alkyl), -S(=O) 2 -N(unsubstituted(C 1 -C 5 )alkyl) 2 , -C(=)S-(unsubstituted (C 1 -C 5 ) alkyl) and -COO (unsubstituted (C 1 -C 5 )alkyl).

[0010] In one or more embodiments, the modality-enhanced organic compound is described by any of limitations (i) to (vi): (i) having the formula (A 1 ) or (B 1 ); (ii) having the formula (A 1 ) or (C 1 ); (iii) having the formula (B 1 ) or (C 1 ); (iv) having the formula (A 1 ); (v) having the formula (B 1 ) or (vi) having the formula (C 1 Without being bound by theory, it is believed and has been found that: 1 ) and (B 1 ) produce ligands R (A) and (B) respectively, which are described herein as having a carbon-carbon double bond as a common structural feature between them. In some aspects, the organic compound with a modal increase consists of carbon and hydrogen atoms. In other aspects, the organic compound with a modal increase consists of carbon atoms, hydrogen atoms and at least one atom selected from halogen atoms, O, N and Si; alternatively, the organic compound with a modal increase consists of carbon atoms, hydrogen atoms and at least one atom selected from O, N and Si; alternatively O or N; alternatively O and Si; alternatively N and Si; alternatively O; alternatively N; alternatively Si.

[0011] Aspect 2: The method according to aspect 1, wherein the modal-enhanced organic compound has a formula (A 1 ): R 5 -C≡CR6 (A 1 ) is selected from phenylacetylene; (substituted phenyl)acetylene; diphenylacetylene; substituted diphenylacetylene; cycloalkylacetylene; a compound of the formula HC≡CSi(phenyl) h ((C 1 -C 20 )alkyl) 3-h Acetylene, wherein the subscript h is an integer from 0 to 3; and a compound of the formula HC≡C-(CH 2 ) m CH 3 wherein the subscript m is an integer from 1 to 15, alternatively from 1 to 10, alternatively from 2 to 15. In one or more embodiments, the modally increased organic compound has the formula (A 1 ): R 5 -C≡CR 6 (A 1 ), and formula (A 1 ) is selected from the group consisting of any one of MIC1 to MIC14: Modal increase of organic compound (1) ("MIC1"): phenylacetylene (ie, (C 6 H 5 )C≡CH); Modally increased organic compound (2) ("MIC2"): 4-methylphenyl-acetylene (i.e., (4-CH 3 -C 6 H 4 )C≡CH); Modally increased organic compound (3) ("MIC3"): 2,4,5-trimethylphenyl-acetylene (i.e., (2,4,5-(CH 3 ) 3 -C 6 H 2 )C≡CH); Modally increased organic compound (4) ("MIC4"): 1,3,5-triethynylbenzene (i.e., 1,3,5-tris(HC≡C) 3 (C 6 H 3 )); Modally increased organic compound (5) ("MIC5"): diphenylacetylene (i.e., (C 6 H 5 )C≡C(C 6 H 5 )); Modally increased organic compound (6) ("MIC6"): 3-fluorophenyl-acetylene (ie, (3-FC 6 H 4 )C≡CH); Modally increased organic compound (7) ("MIC7"): 4-fluorophenyl-acetylene (ie, (4-FC 6 H 4)C≡CH); Modally increased organic compound (8) ("MIC8"): 3,4-difluorophenyl-acetylene (i.e., (3,4-F 2 -C 6 H 3 )C≡CH); Modally increased organic compound (9) ("MIC9"): 3,5-difluorophenyl-acetylene (i.e., (3,5-F 2 -C 6 H 3 )C≡CH); Modally increased organic compound (10) ("MIC10"): cyclohexyl acetylene (i.e., C 6 H 11 C≡CH); Modally increased organic compound (11) ("MIC11"): phenyldimethylsilyl acetylene (i.e., (C 6 H 5 )(CH 3 ) 2 SiC≡CH); Modally increased organic compound (12) ("MIC12"): 1-pentyne (i.e., CH 3 (CH 2 ) 2 C≡CH); Modally increased organic compound (13) ("MIC13"): 1-octyne (i.e., CH 3 (CH 2 ) 5 C≡CH); and modally increased organic compounds (14) ("MIC14"): 1,7-octanediyne (i.e., HC≡C(CH 2 ) 4 C≡CH).

[0012] Aspect 3: The method according to aspect 1, wherein the modal-enhanced organic compound has a formula (B 1 )(R 5 ) 2 C=C=C(R 6 ) 2 (B 1 ), and is selected from the group consisting of cycloalkyl propadiene; alkyl propadiene; dialkyl propadiene; trialkyl propadiene; trialkylsilyl propadiene; vinylidene cycloalkanes; and alkyl esters of propadiene carboxylic acids. In one or more embodiments, formula (B 1 ) is selected from the group consisting of any one of MIC15 to MIC17: Modal-increased organic compound (15) ("MIC15"): cyclohexyl propadiene (i.e., (C 6 H 11 )C(H)=C=CH 2); Modally increased organic compound (16) ("MIC16"): ethyl 2,3-butadienoate (i.e., H2C=C=CH-C(=O)-O-CH 2 CH 3 ); and modally increased organic compound (17) ("MIC17"): 1,1-dimethylpropadiene (i.e., (CH 3 ) 2 C=C=CH 2 ).

[0013] Aspect 4: The method according to aspect 1, wherein the modal-enhanced organic compound has a formula (C 1 )(R 5 )(R 7 )C=C(R 6 )(R 7 )(C 1 ), and formula (C 1 ) is an internal olefin. Therefore, the internal olefin does not have a terminal carbon-carbon double bond or a terminal carbon-carbon triple bond. The internal olefin can be selected from MIC18 to MIC20: Modal-increased organic compound (18) ("MIC18"): 2-butene, modal-increased organic compound (19) ("MIC19"): 2-pentene, and modal-increased organic compound (20) ("MIC20"): 1,2-diphenylethylene.

[0014] Aspect 5: The method according to aspect 1, wherein the modality-enhanced organic compound is selected from the group consisting of: cyclohexylpropadiene; phenylacetylene; and 3,4-difluorophenylacetylene.

[0015] Aspect 6: A method according to any one of Aspects 1 to 5, wherein in the combining step, (i) the first unimodal ligand-metal precatalyst and the bimodal ligand-metal catalyst are unsupported (i.e., do not contain a support material); or (ii) the first unimodal ligand-metal precatalyst is unsupported, and the method further comprises, after the combining step, adding a support material to the bimodal ligand-metal catalyst so as to obtain a bimodal catalyst system comprising a support material and a bimodal ligand-metal catalyst.

[0016] Aspect 7: The method according to any one of aspects 1 to 5, wherein in the combining step, the first unimodal ligand-metal precatalyst and the bimodal ligand-metal catalyst are independently supported on a support material, so that the combining step is performed in the presence of the support material, and the method prepares a bimodal catalyst system comprising a support material and a bimodal ligand-metal catalyst. In one or more embodiments, wherein the first unimodal ligand-metal precatalyst is supported on a support material, so that the combining components are performed in the presence of the support material, and the method prepares a bimodal catalyst system comprising a support material and a bimodal ligand-metal catalyst. In one or more embodiments, wherein the first unimodal ligand-metal precatalyst is supported on a support material, so that the combining components are performed in the presence of the support material, and the method prepares a bimodal catalyst system consisting essentially of or consisting of a support material and a bimodal ligand-metal catalyst.

[0017] Aspect 8: A method according to any one of Aspects 1 to 5, comprising combining in any order components consisting essentially of a modally increased organic compound, an activator, and a bimodal pre-catalyst system, the bimodal pre-catalyst system essentially consisting of a first unimodal ligand-metal pre-catalyst, a second unimodal ligand-metal pre-catalyst having a ligand compositionally different from the first unimodal ligand-metal pre-catalyst, and a support material; wherein the method prepares a trimodal catalyst system, the trimodal catalyst system essentially consisting of a bimodal ligand-metal catalyst, a second unimodal ligand-metal catalyst (e.g., a metallocene-type catalyst) made of a second unimodal ligand-metal pre-catalyst and an activator, and a support material.

[0018] Aspect 9: The method according to any one of aspects 1 and 6 to 8 further comprises, during or after the combining step, contacting a bimodal ligand-metal catalyst (Aspect 1), a bimodal catalyst system (Aspect 6 or 7), or a trimodal catalyst system (Aspect 8) with ethylene and α-olefin in a polymerization reactor under steady-state polymerization conditions to produce a poly(ethylene-co-α-olefin) copolymer having a bimodal molecular weight distribution ("bimodal copolymer", Aspect 1, 6 or 7) or having a trimodal molecular weight distribution ("trimodal copolymer", Aspect 8) as determined by gel permeation chromatography (GPC). In one or more embodiments, the method according to any one of aspects 1 to 8 further comprises, during or after combining the components, contacting at least a bimodal ligand-metal catalyst with ethylene and α-olefin in a polymerization reactor under steady-state polymerization conditions to produce a poly(ethylene-co-α-olefin) copolymer having a multimodal molecular weight distribution as determined by GPC.

[0019] Aspect 10: A method according to aspect 9, wherein the comparative unimodal poly(ethylene-co-α-olefin) copolymer prepared by contacting a first unimodal ligand-metal catalyst prepared from a first unimodal ligand-metal precatalyst and an activator with ethylene and an α-olefin under the same steady-state polymerization conditions in the absence of a modality-enhancing organic compound has a normal short chain branching distribution per 1000 carbon atoms (normal SCBD / 1000C), and the bimodal copolymer or trimodal copolymer has a reduced normal SCBD / 1000C; wherein the comparative unimodal poly(ethylene-co-α-olefin) copolymer wherein the comparative unimodal poly(ethylene-co-α-olefin) copolymer has a normal SCBD / 1000C and the bimodal copolymer or trimodal copolymer has a flat SCBD / 1000C; wherein the comparative unimodal poly(ethylene-co-α-olefin) copolymer has a normal SCBD / 1000C and the bimodal copolymer or trimodal copolymer has a reverse SCBD / 1000C; or wherein the comparative unimodal poly(ethylene-co-α-olefin) copolymer has a reverse SCBD / 1000C and the bimodal copolymer or trimodal copolymer has an enhanced reverse SCBD / 1000C. In one or more embodiments, the method according to aspect 9 further includes wherein the comparative unimodal poly(ethylene-co-α-olefin) copolymer prepared by contacting a first unimodal ligand-metal catalyst prepared from a first unimodal ligand-metal precatalyst and an activator with ethylene and an α-olefin under the same steady-state polymerization conditions in the absence of a modality-enhanced organic compound has a normal short chain branching distribution per 1000 carbon atoms (normal SCBD / 1000C), and the multimodal copolymer has a reduced normal SCBD / 1000C, a flat SCBD / 1000C, a reverse SCBD / 1000C, or an enhanced reverse SCBD / 1000C.

[0020] Aspect 11: The method of aspect 9 or 10, wherein the comparative unimodal poly(ethylene-co-α-olefin) copolymer prepared by contacting a first unimodal ligand-metal catalyst prepared from a first unimodal ligand-metal precatalyst and an activator with ethylene and an α-olefin under the same steady-state polymerization conditions in the absence of a modality-increasing organic compound has a molecular weight distribution (M) of x. w / M n ), where M w is the weight average molecular weight and M n is the number average molecular weight as measured by GPC, and the bimodal or trimodal copolymer has an M of 1.1x to 5.0x. w / M n In one or more embodiments, a comparative unimodal poly(ethylene-co-α-olefin) copolymer may have an M of 3.2. w / M n(x=3.2), and the bimodal polymer or trimodal polymer prepared by this method may have an M of 6.7 w / M n (=2.1x). In one or more embodiments, the method according to aspect 10 may further include wherein the comparative unimodal poly(ethylene-co-α-olefin) copolymer has a molecular weight distribution (M w / M n ), where M w is the weight average molecular weight, and M n is the number average molecular weight as measured by GPC, and the multimodal copolymers have an M of 1.1x to 5.0x w / M n .

[0021] Aspect 12: The method according to any one of Aspects 1 to 11 comprises the following steps: converting the polymerization process carried out in a polymerization reactor from a process for preparing a unimodal poly(ethylene-co-α-olefin) copolymer to a process for preparing a bimodal or trimodal poly(ethylene-co-α-olefin) copolymer, the method further comprising, before the combining step, contacting a first unimodal ligand-metal catalyst made of a first unimodal ligand-metal precatalyst and an activator with ethylene and α-olefin in a polymerization reactor under steady-state polymerization conditions in the absence of a modality-increasing organic compound to prepare a poly(ethylene-co-α-olefin) copolymer having a unimodal molecular weight distribution as determined by GPC ("unimodal copolymer"); and after the combining step, contacting a bimodal ligand-metal catalyst (Aspect 1), a bimodal catalyst system (Aspect 6 or 7) or a trimodal catalyst system (Aspect 8) with ethylene and α-olefin in a polymerization reactor under steady-state polymerization conditions to prepare a poly(ethylene-co-α-olefin) copolymer having a bimodal or trimodal molecular weight distribution as determined by GPC. In one or more embodiments, the method according to any one of aspects 1 to 11 further comprises converting the polymerization process carried out in the polymerization reactor from a process for preparing a unimodal poly(ethylene-co-α-olefin) copolymer to a process for preparing a multimodal poly(ethylene-co-α-olefin) copolymer, the method further comprising contacting a first unimodal ligand-metal catalyst made of a first unimodal ligand-metal precatalyst and an activator with ethylene and an α-olefin in a polymerization reactor under steady-state polymerization conditions in the absence of a modality-increasing organic compound before combining the components so as to prepare a poly(ethylene-co-α-olefin) copolymer having a unimodal molecular weight distribution as determined by GPC ("unimodal copolymer"); and after the combining step, contacting at least a bimodal ligand-metal catalyst with ethylene and an α-olefin in a polymerization reactor under steady-state polymerization conditions so as to prepare a poly(ethylene-co-α-olefin) copolymer having a multimodal molecular weight distribution as determined by GPC. Converting the polymerization process carried out in the polymerization reactor from a process for preparing a unimodal poly(ethylene-co-α-olefin) copolymer to a process for preparing a multimodal polymer may be desirable for various different applications, such as preparing different polymers with different properties.

[0022] Aspect 13: A method according to any one of Aspects 1 to 12, wherein the order of the combining steps includes limiting any one of (i) to (iv): (i) combining a first unimodal ligand-metal precatalyst with an effective amount of an activator to obtain a first intermediate mixture that is free of a modally increased organic compound, and then combining the first intermediate mixture with a modally increased organic compound; (ii) combining a first unimodal ligand-metal precatalyst with an effective amount of a modally increased organic compound to obtain a second intermediate mixture, and then combining the second intermediate mixture with an effective amount of an activator; (iii) combining an effective amount of an activator with an effective amount of a modally increased organic compound to obtain a third intermediate mixture that is free of the first unimodal ligand-metal precatalyst, and then combining the third intermediate mixture with the first unimodal ligand-metal precatalyst; and (iv) simultaneously combining the first unimodal ligand-metal precatalyst, an effective amount of an activator, and an effective amount of a modally increased organic compound. In one or more embodiments, the first unimodal ligand-metal precatalyst can be free of substituted cyclopentadienyl ligands (e.g., propylcyclopentadienyl, pentamethylcyclopentadienyl, or 4,5,6,7-tetrahydroindenyl) and unsubstituted cyclopentadienyl ligands (i.e., C 5 H 5 The first unimodal ligand-metal precatalyst may be different from the metallocene-type precatalyst, and thus the bimodal ligand-metal catalyst prepared therefrom may be different from the metallocene-type catalyst. The second unimodal ligand-metal precatalyst having a ligand compositionally different from the ligand of the first unimodal ligand-metal precatalyst may be a metallocene-type precatalyst.

[0023] Aspect 14: The method according to any one of aspects 1 to 13, wherein the first unimodal ligand-metal precatalyst is a biphenylphenoxy-type (BPP-type) ligand-metal precatalyst of structural formula (I): Where L is CH 2 CH 2 , CH 2 CH 2 CH 2 , CH 2 CH 2 CH 2 CH 2 , CH 2 C(R L ) 2 CH 2 , CH 2 CH(R L )CH(R L )CH 2 , CH 2 Ge(RL ) 2 CH 2 or CH 2 Si(R L ) 2 CH 2 , where each R L are independently unsubstituted (C 1 -C 20 ) alkyl; M is Zr or Hf; R 1a and R 1b Each of which is independently F, (C 1 -C 20 )alkyl or Si(CH 3 ) 2 (CH 2 ) q CH 3 , wherein subscript q is an integer from 0 to 20; each subscript r is independently an integer from 0 to 3; R 2a and R 2b Each of which is independently H, F, Cl, (C 1 -C 5 ) alkyl groups such as CH 3 , or R 2a and R 2b may be bonded together to form an unsubstituted or substituted cycloalkyl group; each subscript s is independently an integer from 0 to 3; R 3a and R 3b Each of which is independently unsubstituted (C 1 -C 20 ) alkyl or (C 1 -C 20 ) alkoxy; each Ar 1a and Ar 1b is independently an unsubstituted or substituted aromatic group selected from the group consisting of phenyl, substituted phenyl, biphenyl, substituted biphenyl, anthracene, substituted anthracene, carbazolyl, and substituted carbazolyl, wherein each substituent in the substituted aromatic group is independently an alkyl group; and each X is independently a monodentate group or each X is a part of a multidentate (e.g., bidentate) group independently selected from the group consisting of a halogen atom; ((C 1 -C 20 )alkyl) 3-g -(phenyl) g Si-, where subscript g is 0, 1, 2 or 3; CH 3 ;(C 2 -C 20 )alkyl-CH 2 ;(C 6 -C 12 )Aryl-((C 0-C 10 )alkylene)-CH 2 (For example, benzyl, when (C 6 -C 12 ) aryl is phenyl and (C 0 -C 10 ) alkylene is (C 0 ) alkylene); (C 1 -C 6 )alkyl-substituted (C 6 -C 12 ) aryl; (C 1 -C 6 ) alkoxy-substituted (C 6 -C 12 ) aryl; (C 1 -C 6 ) alkoxy-substituted benzyl; and (C 1 -C 6 )alkyl-substituted benzyl; or one X is 4-(C 1 -C 20 )alkyl-substituted 1,3-butadiene molecules, and each of the remaining Xs, if any, is independently a monodentate group X.

[0024] In one or more embodiments, the first unimodal ligand-metal precatalyst is a biphenylphenoxy-type (BPP-type) ligand-metal precatalyst of formula (I) above; wherein in formula (A 1 )、(B 1 ) or (C 1 ), R 5 and R 6 Each of which is independently H or R 7 ; and each R 7 Independently (C 1 -C 20 )alkyl, -C(=O)-O-(unsubstituted C 1 -C 20 ) alkyl), (C 1 -C 19 ) heteroalkyl or tri((C 1 -C 20 )alkyl)silyl, or two R 7 Combined to form (C 3 -C 8 ) alkylene; provided that each R 7 lacks a carbon-carbon double bond; each (C 1 -C 20 ) The hydrocarbon groups are independently unsubstituted or substituted by 1 to 4 groups R S Substituted; wherein each substituent group RS are independently selected from halogen (e.g., F), unsubstituted (C 1 -C 5 ) alkyl (e.g., CH 3 )、-C≡CH、-OH、(C 1 -C 5 )alkoxy, -C(=O)-(unsubstituted (C 1 -C 5 )alkyl), -NH 2 、-N(H)(unsubstituted(C 1 -C 5 ) alkyl), -N(unsubstituted(C 1 -C 5 )alkyl) 2 , -COOH, -C(=O)-NH 2 , -C(=O)-N(H)(unsubstituted(C 1 -C 5 ) alkyl), -C(=O)-N(unsubstituted (C 1 -C 5 )alkyl) 2 、-S-(unsubstituted(C 1 -C 5 )alkyl), -S(=O) 2 -(Unsubstituted(C 1 -C 5 )alkyl), -S(=O) 2 -NH 2 、-S(=O) 2 -N(H)(Unsubstituted(C 1 -C 5 )alkyl), -S(=O) 2 -N(unsubstituted(C 1 -C 5 )alkyl) 2 , -C(=)S-(unsubstituted (C 1 -C 5 ) alkyl) and -COO (unsubstituted (C 1 -C 5 ) alkyl); and wherein in formula (I): L is CH 2 CH 2 , CH 2 CH 2 CH 2 , CH 2 CH 2 CH 2 CH 2 , CH 2 C(R L ) 2 CH2 , CH 2 CH(R L )CH(R L )CH 2 , CH 2 Ge(R L ) 2 CH 2 or CH 2 Si(R L ) 2 CH 2 , where each R L are independently unsubstituted (C 1 -C 20 ) alkyl; M is Ti, Zr or Hf; alternatively, M is Zr or Hf; R 1a and R 1b Each of the following is independently a halogen atom (eg, Cl or F, alternatively F), (C 1 -C 20 )alkyl or Si(CH 3 ) 2 (CH 2 ) q CH 3 , wherein subscript q is an integer from 0 to 20; each subscript r is independently an integer from 0 to 3; R 2a and R 2b Each of which is independently H, F, Cl, or R 2b are independently H, F, Cl, (C 1 -C 5 ) alkyl, or R 2a and R 2b may be bonded together to form an unsubstituted or substituted cycloalkyl group, alternatively H or CH 3 ; Each subscript s is independently an integer from 0 to 3; R 3a and R 3b Each of which is independently halogen, unsubstituted (C 1 -C 20 ) alkyl or (C 1 -C 20 )alkoxy, optionally unsubstituted (C 1 -C 20 ) alkyl or (C 1 -C 20 ) alkoxy; each Ar 1a and Ar 1bis independently an unsubstituted or substituted aromatic group selected from the group consisting of phenyl, substituted phenyl, biphenyl, substituted biphenyl, anthracene, substituted anthracene, carbazolyl, and substituted carbazolyl, wherein each substituent in the substituted aromatic group is independently an alkyl group; and each X is independently a monodentate group or each X is a part of a multidentate (e.g., bidentate) group independently selected from the group consisting of a halogen atom; ((C 1 -C 20 )alkyl) 3-g -(phenyl) g Si-, where subscript g is 0, 1, 2 or 3; CH 3 ;(C 2 -C 20 )alkyl-CH 2 ;(C 6 -C 12 )Aryl-((C 0 -C 10 )alkylene)-CH 2 (For example, benzyl, when (C 6 -C 12 ) aryl is phenyl and (C 0 -C 10 ) alkylene is (C 0 ) alkylene); (C 1 -C 6 )alkyl-substituted (C 6 -C 12 ) aryl; (C 1 -C 6 ) alkoxy-substituted (C 6 -C 12 ) aryl; (C 1 -C 6 ) alkoxy-substituted benzyl; and (C 1 -C 6 )alkyl-substituted benzyl; or one X is 4-(C 1 -C 20 )alkyl-substituted 1,3-butadiene molecules, and each of the remaining X, if any, is independently a monodentate group X. At least one group X acts as a leaving group during the activation step, and optionally, at least one group X acts as a leaving group during the combining step. In some embodiments, at least one X does not leave but remains coordinated to M. In some aspects, at least one X is (C 6 -C 12 )Aryl-((C 0 -C 10 )alkylene)-CH 2 (e.g., benzyl). In some aspects, each X is independently (C 6 -C12 )Aryl-((C 0 -C 10 )alkylene)-CH 2 Alternatively, one X is (C 6 -C 12 )Aryl-((C 0 -C 10 )alkylene)-CH 2 (e.g., benzyl), and the other X is F, Cl or methyl; alternatively, each X is benzyl. For the removal of all doubts, the monodentate group X does not contain a carbon-carbon double bond or a carbon-carbon triple bond, i.e., the monodentate group X is not an alkenyl group or an alkynyl group. In some aspects, each R 7 Independently (C 1 -C 20 ) hydrocarbon groups, which independently may be unsubstituted or substituted with 1 to 3 groups selected from halogen (e.g., F) and alkyl (e.g., CH 3 ) is substituted by a substituent group, provided that each R 7 Lacks carbon-carbon double bonds. In some embodiments, L is selected from CH 2 CH 2 , CH 2 CH 2 CH 2 , CH 2 CH 2 CH 2 CH 2 , CH 2 C(R L ) 2 CH 2 and CH 2 CH(R L )CH(R L )CH 2 , alternatively CH 2 CH 2 , CH 2 CH 2 CH 2 and CH 2 CH 2 CH 2 CH 2 , alternatively CH 2 C(R L ) 2 CH 2 and CH 2 CH(R L )CH(R L )CH 2 A carbon-bridging group, wherein each R L In some embodiments, L is selected from CH 2Ge(R L ) 2 CH 2 and CH 2 Si(R L ) 2 CH 2 , alternatively CH 2 Ge(R L ) 2 CH 2 , alternatively CH 2 Si(R L ) 2 CH 2 A heteroatom-containing bridging group; wherein each R L In some embodiments, L is selected from CH 2 C(R L ) 2 CH 2 , CH 2 CH(R L )CH(R L )CH 2 , CH 2 Ge(R L ) 2 CH 2 and CH 2 Si(R L ) 2 CH 2 R L -substituted bridging group; wherein each R L In some embodiments, M is Zr or Hf, and R 3a and R 3b Each of which is independently unsubstituted (C 1 -C 20 )alkyl.

[0025] The first unimodal ligand-metal precatalyst of formula (I) may be any one of those described in WO 2012 / 027448 A1, WO 2014 / 105411 A1, WO 2017 / 058981 A1 or WO 2018 / 022975 A1.

[0026] 15: The method according to aspect 14, wherein the BPP-type ligand-metal precatalyst of structural formula (I) is any one of compounds (1) to (2):

[0027] ("Precatalyst 1"); and ("Precatalyst 2"), wherein each Me is a methyl group.

[0028] The unimodal ligand-metal precatalyst structure (1) was synthesized according to the procedure of WO 2012 / 027448 A1. The unimodal ligand-metal precatalyst structure (2) was synthesized according to the procedure of WO2018170227 A1.

[0029] Aspect 16: A method according to any one of Aspects 1 to 15, wherein the metal of the first unimodal ligand-metal precatalyst is M, wherein the activator is an organoaluminum compound, and wherein the effective amount of the activator is an Al / M molar ratio of 0.5 to 10,000, alternatively 0.95 to 200, alternatively 1.0 to 150, alternatively 10 to 100; and / or wherein the effective amount of the modal-increased organic compound comprises a molar ratio of the modal-increased organic compound to the first unimodal ligand-metal precatalyst (MIOC / FUC molar ratio) of 0.5:1.0 to 50.0:1.0, alternatively 0.9:1.0 to 20.0:1.0, alternatively 0.9:1.0 to 11:1.0, alternatively 0.95:1.0 to 6:1.0.

[0030] Aspect 17: A method for preparing a poly(ethylene-co-α-olefin) copolymer ("bimodal copolymer") having a bimodal molecular weight distribution as determined by GPC, the method essentially consisting of the following steps: contacting ethylene and an α-olefin with a bimodal ligand-metal catalyst prepared by the method according to any one of Aspects 1 to 16 in a polymerization reactor under steady-state polymerization conditions to prepare a bimodal copolymer. In one or more embodiments, the method for preparing a poly(ethylene-co-α-olefin) copolymer may include contacting at least one 1-olefin monomer with a bimodal ligand-metal catalyst prepared by the method according to any one of Aspects 1 to 16 under slurry phase or gas phase polymerization conditions in a slurry phase or gas phase polymerization reactor containing a moving bed of a polyolefin resin, respectively, thereby preparing a poly(ethylene-co-α-olefin) copolymer. The moving bed may be a stirred bed or a fluidized bed. The at least one 1-olefin monomer may be ethylene, or a combination of ethylene and a comonomer selected from the group consisting of propylene, 1-butene, 1-hexene, and 1-octene. In some embodiments, the reactor is a first gas phase polymerization reactor and is under first gas phase polymerization conditions. Alternatively, the reactor may be a slurry phase polymerization reactor and the polymerization conditions may be slurry phase polymerization conditions. In some such embodiments, the method may further comprise transferring the active polymer particles prepared in the first gas phase polymerization reactor under first gas phase polymerization conditions or prepared in the slurry phase polymerization reactor under slurry phase polymerization conditions and in either case containing (in the particles) an active bimodal ligand-metal catalyst to a (second) gas phase polymerization reactor under (second) gas phase polymerization conditions (these gas phase polymerization conditions are different from the first gas phase polymerization conditions used in the first gas phase polymerization reactor or the slurry phase polymerization conditions used in the slurry phase polymerization reactor, as the case may be), thereby preparing a multimodal (e.g., bimodal or trimodal) polyolefin polymer (i.e., having a multimodal (e.g., bimodal or trimodal) molecular weight distribution (M) in the (second) gas phase polymerization reactor). w / M n ) of polyolefin polymers).

[0031] Aspect 18: A poly(ethylene-co-α-olefin) copolymer prepared by the method according to Aspect 17, wherein the poly(ethylene-co-α-olefin) copolymer has a BCDI greater than 4, a MWCDI>0, or both. Embodiments provide that the copolymer may have an Mn (number average molecular weight) of 10,000 to 250,000. Embodiments provide that the copolymer may have an Mw (weight average molecular weight) of 50,000 to 1,000,000. Embodiments provide that the copolymer may have an Mz (z-average molecular weight) of 500,000 to 5,000,000. Embodiments provide that the copolymer may have an Mz to Mw ratio in the range of 2.00 to 20.00. In some embodiments, the copolymer may have a value of the Mw to Mn ratio greater than 2.00, greater than 3.00, greater than 4.00, or greater than 5.00. Some embodiments provide that the copolymer may have a Mw to Mn ratio in the range of 5.00 to 75.00 or 5.00 to 50.00. Embodiments provide that the copolymer may have a Mz to Mw ratio that is less than the Mw to Mn ratio of the copolymer. Embodiments provide that the copolymer prepared using a gas phase polymerization reactor may have a melting temperature (Tm) of 110 degrees Celsius (° C.) to 135 degrees Celsius.

[0032] The copolymer may have a MWCDI of 0.9 to 25.0, such as MWCDI-1 and / or MWCDI-2. In some embodiments, the copolymer may have a MWCDI of a lower limit of 0.9, 1.0, 1.2, 1.5, or 1.6 to an upper limit of 25.0, 20.0, 16.0, 15.0, 14.0, 13.0, 12.0, 11.0, 10.0, 9.0, 8.0, 7.0, or 6.0. For example, the copolymer may have a MWCDI-1 of a lower limit of 0.9, 1.0, 1.2, 1.5, or 1.6 to an upper limit of 25.0, 20.0, 16.0, 15.0, 14.0, 13.0, 12.0, 11.0, 10.0, 9.0, 8.0, 7.0, or 6.0 and / or the copolymer may have a MWCDI-2 of a lower limit of 0.9, 1.0, 1.2, 1.5, or 1.6 to an upper limit of 25.0, 20.0, 16.0, 15.0, 14.0, 13.0, 12.0, 11.0, 10.0, 9.0, 8.0, 7.0, or 6.0.

[0033] The copolymer may have a BCDI greater than 4, greater than 5, or greater than 6. For example, the copolymer may have a BCDI of 4 to 500, 4 to 450, or 4 to 400.

[0034] Aspect 19: An article of manufacture made from the poly(ethylene-co-α-olefin) copolymer according to aspect 18.

[0035] Aspect 20: A multimodal catalyst system, the bimodal ligand-metal catalyst being prepared by the method according to any one of aspects 1 to 16.

[0036] A method for chemically converting a unimodal ligand-metal precatalyst to a bimodal ligand-metal catalyst. The method comprises combining, in any order, components consisting essentially of a first unimodal ligand-metal precatalyst, an effective amount of an activator, and an effective amount of an organic compound having an increased modality, under conditions effective for the activator and the organic compound having an increased modality, to chemically convert the first unimodal ligand-metal precatalyst to a bimodal ligand-metal catalyst, thereby preparing a bimodal ligand-metal catalyst. The organic compound having an increased modality may have the formula (A 1 )、(B 1 ) or (C 1 ). The first unimodal ligand-metal precatalyst can be a biphenylphenoxy-type (BPP-type) ligand-metal precatalyst of formula (I). In some embodiments, the metal M is Zr or Hf; alternatively, M is Zr or Ti; alternatively, M is Ti or Hf; alternatively, M is Zr; alternatively, M is Hf; alternatively, M is Ti.

[0037] The embodiment of the preparation method may include any one of Synthesis Schemes 1 to 13.

[0038] Synthesis Scheme 1: Step (a) unimodal ligand-metal precatalyst + excess activator → activated unimodal ligand-metal catalyst + intermediate mixture of remaining activator. Step (b) intermediate mixture + effective amount of modality-increasing compound → bimodal ligand-metal catalyst + remaining activator.

[0039] Synthesis Scheme 2: Step (a) unimodal ligand-metal precatalyst + effective amount of modality-increasing compound → intermediate unimodal ligand-metal precatalyst (unreacted mixture or reaction product of unimodal ligand-metal precatalyst + modality-increasing compound). Step (b) intermediate unimodal ligand-metal precatalyst + activator (e.g., alkylaluminoxane, such as methylaluminoxane ("MAO")) → bimodal ligand-metal catalyst.

[0040] Synthesis Scheme 3: Step (a) Unimodal ligand-metal precatalyst + activator (e.g., alkylaluminoxane, such as methylaluminoxane ("MAO")) → activated unimodal ligand-metal catalyst. Step (b) Unimodal ligand-metal catalyst + effective amount of modality-increasing compound → bimodal ligand-metal catalyst.

[0041] Synthesis Scheme 4: Step (a) Activator (e.g., alkylaluminoxane, such as methylaluminoxane ("MAO")) + effective amount of modality-increasing compound → intermediate mixture. Step (b) Intermediate mixture + unimodal ligand-metal precatalyst → bimodal ligand-metal catalyst.

[0042] Synthesis Scheme 5: Step (a) Activator → unimodal ligand-metal precatalyst ← effective amount of modality-increasing compound (activator and modality-increasing compound are added to unimodal ligand-metal precatalyst simultaneously but separately) → bimodal ligand-metal catalyst. Step (b): None.

[0043] Synthesis Scheme 6: Step (a) unimodal ligand-metal precatalyst + support material → supported unimodal ligand-metal precatalyst. Step (b) supported unimodal ligand-metal precatalyst + a certain amount of activator → the intermediate mixture of activated and supported unimodal ligand-metal catalyst + remaining activator is disposed on the support material (or balanced with the support material). Step (c) intermediate mixture + effective amount of mode-increasing compound → bimodal ligand-metal catalyst is disposed on the support material (or balanced with the support material). In some aspects, step (a) also includes an inert hydrocarbon solvent, and the deposition on the support material is performed by evaporating the solvent (alternatively by spray drying). The amount of the activator may be a stoichiometric amount relative to the metal M of the unimodal ligand-metal catalyst (e.g., a molar ratio of 1.0 to 1.0); alternatively, less than the stoichiometric amount relative to the metal M of the post-metallocene catalyst (e.g., a molar ratio of 0.1 to 0.94); alternatively, an excess amount relative to the metal M of the post-metallocene catalyst (e.g., a molar ratio of 1.1 to 10,000). Examples of the support material are alumina and hydrophobic fumed silica; alternatively, the hydrophobic fumed silica. The hydrophobic fumed silica can be prepared by surface treating untreated anhydrous fumed silica with an effective amount of a hydrophobic agent. The hydrophobic agent may be dimethyldichlorosilane, polydimethylsiloxane fluid, or hexamethyldisilazane; alternatively, dimethyldichlorosilane. The hydrophobic fumed silica prepared by surface-treating untreated anhydrous fumed silica with dimethyldichlorosilane may be CABOSIL TS-610, which is fumed silica surface-treated with dimethyldichlorosilane.

[0044] Synthesis Scheme 7: Step (a) unimodal ligand-metal precatalyst + effective amount of modality-increasing compound + on support material → intermediate mixture of unimodal ligand-metal precatalyst and modality-increasing compound is disposed on (or equilibrated with) a support material. Step (b) intermediate mixture + activator (e.g., alkylaluminoxane, such as methylaluminoxane ("MAO")) → bimodal ligand-metal catalyst is disposed on (or equilibrated with) a support material. In some aspects, step (a) further comprises an inert hydrocarbon solvent, and deposition on the support material is performed by evaporating the solvent (alternatively by spray drying).

[0045] Synthesis Scheme 8: Step (a) Unimodal ligand-metal precatalyst + support material + activator (e.g., alkylaluminoxane, such as methylaluminoxane ("MAO")) → the activated and supported unimodal ligand-metal catalyst is disposed on (or equilibrated with) a support material. Step (b) Supported activated unimodal ligand-metal catalyst + effective amount of modality-increasing compound → the bimodal ligand-metal catalyst is disposed on (or equilibrated with) a support material. In some aspects, step (a) further comprises an inert hydrocarbon solvent, and the deposition on the support material is performed by evaporating the solvent (alternatively by spray drying).

[0046] Synthesis Scheme 9: Step (a) Activator (e.g., alkylaluminoxane, such as methylaluminoxane ("MAO")) + effective amount of modality-increasing compound → intermediate solution. Step (b) Intermediate solution + unimodal ligand-metal precatalyst + support material → bimodal ligand-metal catalyst is disposed on (or equilibrated with) the support material. In some aspects, step (b) further comprises an inert hydrocarbon solvent, and the deposition on the support material is performed by evaporating the solvent (alternatively by spray drying).

[0047] Synthesis Scheme 10: Step (a) Activator → Unimodal ligand-metal precatalyst + support material ← effective amount of modality-increasing compound (adding activator and modality-increasing compound simultaneously but separately to the mixture of unimodal ligand-metal precatalyst + support material) → disposing bimodal ligand-metal catalyst on support material (or equilibrating with the support material). Step (b): None. In some aspects, step (a) further comprises an inert hydrocarbon solvent, and deposition on the support material is performed by evaporating the solvent (alternatively by spray drying).

[0048] Scheme 11: Step (a): activator (e.g., alkylaluminoxane, such as methylaluminoxane ("MAO")) + support material (e.g., hydrophobic fumed silica) + inert hydrocarbon solvent → a slurry of supported activator is disposed on (or equilibrated with) the support material. Step (b): spray-dried slurry of step (a) → the spray-dried supported activator is disposed on a support material in dry powder form (e.g., spray-dried MAO ("SDMAO" or "sdMAO") on hydrophobic fumed silica in dry powder form). Step (c): unimodal ligand-metal precatalyst + spray-dried supported activator of step (b) + inert hydrocarbon solvent are mixed → a suspension of supported unimodal ligand-metal catalyst is disposed on (or equilibrated with) the support material. Step (d): mixing the suspension from step (c) with an effective amount of a modality increasing compound → disposing the suspension of the supported bimodal ligand-metal catalyst on (or equilibrating with) a support material in an inert hydrocarbon solvent. Optional step (e): removing the inert hydrocarbon solvent from the suspension of the supported bimodal ligand-metal catalyst → the supported bimodal ligand-metal catalyst is disposed on the support material in the form of a dry powder. Step (e) may be performed by conventional evaporation of the inert hydrocarbon solvent from the suspension from step (d) or by spray drying the suspension from step (d).

[0049] Scheme 12: Preparation of a multimodal (bimodal) catalyst system, which comprises carrying out any of Schemes 1 to 11 and, when necessary (for example, when no support material is present), adding a certain amount of support material to obtain a bimodal catalyst system comprising a support material and a bimodal ligand-metal catalyst.

[0050] Scheme 13: Preparation of a multimodal (trimodal) catalyst system comprising a bimodal ligand-metal catalyst and a second unimodal ligand-metal catalyst (e.g., a metallocene-type catalyst), the second unimodal ligand-metal catalyst being made from a second unimodal ligand-metal precatalyst and an activator spray-dried on a silica support. Step (a) Unimodal ligand-metal precatalyst + support material + activator (e.g., alkylaluminoxane, such as methylaluminoxane ("MAO")) → the activated unimodal ligand-metal catalyst is disposed on (or equilibrated with) the support material. Step (b) Activated unimodal ligand-metal catalyst + an effective amount of a modality-increasing compound → the bimodal ligand-metal catalyst is disposed on (or equilibrated with) the support material. Step (c) The second unimodal ligand-metal catalyst is added to the bimodal ligand-metal catalyst disposed on (or equilibrated with) the support material to obtain a multimodal catalyst system. In some aspects, step (a) also includes an inert hydrocarbon solvent, and the deposition on the support material is performed by evaporating the solvent (alternatively by spray drying). For example, a slurry support material (e.g., fumed silica) and MAO in a solvent (e.g., toluene). Then add a unimodal ligand-metal precatalyst. Mix for a period of time (e.g., 1 hour). Then add a modal increase compound. Mix for another period of time (e.g., 1 hour). Then add a second catalyst (a second unimodal ligand-metal catalyst (e.g., a metallocene-type catalyst)). Spray dry the resulting mixture.

[0051] A multimodal catalyst system can be prepared to be fed into a gas phase polymerization reactor. If desired, an additional amount of a bimodal ligand-metal catalyst or an additional amount of a second catalyst (e.g., a metallocene catalyst) can be fed separately to the reactor as a solution thereof in an inert hydrocarbon solvent, where it contacts the multimodal catalyst system. Such separate catalyst solutions are sometimes referred to as fine-tuning catalysts. Alternatively, the multimodal catalyst system can be contacted with a fine-tuning catalyst feed in a feed line before entering the reactor. In other embodiments, a multimodal catalyst system, such as a trimodal catalyst system, can be prepared in situ in a gas phase polymerization reactor by adding a bimodal ligand-metal catalyst and at least one second catalyst separately to the reactor, where these catalysts contact each other, thereby preparing the multimodal catalyst system in situ in the reactor.

[0052] The method according to any of the above aspects may further comprise the step of transferring polymer particles produced in a gas phase or slurry phase polymerization reactor to a (second) gas phase polymerization reactor, and these polymer particles contain a fully active bimodal ligand-metal catalyst in the particles.

[0053] Organic compounds with increased modality. Formula (A 1 ) is the organic compound with the modal increase of R 5-C≡CR 6 (A 1 ). Formula (B 1 ) is the organic compound with a modal increase in (R 5 ) 2 C=C=C(R 6 ) 2 (B 1 ). Formula (C 1 ) is the organic compound with a modal increase in (R 5 )(R 7 )C=C(R 6 )(R 7 )(C 1 ). Formula (A 1 )、(B 1 ) or (C 1 ) has no deleterious effect on the monomodal ligand-metal catalyst, or may at most have a slight effect. 1 ) is an alkyne, formula (B 1 ) is propadiene, and the compound of formula (C 1 ) is an internal olefin. The modal-enhanced organic compound does not contain a vinyl functional group (i.e., lacks a olefin of the formula -C(H)=CH 2 In some embodiments, the modality-enhanced organic compound is as defined in any of the above numbered aspects. 1 )、(B 1 ) or (C 1 ) in some embodiments of the organic compound having a modal increase of 1 -C 20 ) The hydrocarbon group is (C 2 -C 6 ) alkyl, (C 3 -C 8 )cycloalkyl such as cyclohexyl or phenyl. In some embodiments, -C(=O)-O-(unsubstituted C 1 -C 20 )alkyl) is -C(=O)-O-(unsubstituted C 1 -C 5 )alkyl), alternatively -C(=O)-O-ethyl.

[0054] Bimodal ligand-metal catalyst. As described above, the first unimodal ligand-metal precatalyst can be chemically transformed to prepare the bimodal ligand-metal catalyst. Without being bound by theory, it is believed that the structure of the bimodal ligand-metal catalyst is similar to the structure of the first unimodal ligand-metal precatalyst and / or the first unimodal ligand-metal catalyst (made from the first unimodal ligand-metal precatalyst), for example, wherein one of the leaving groups X of the first unimodal ligand-metal precatalyst has been replaced by a leaving group R in the bimodal ligand-metal catalyst, wherein R is defined later and is derived from an organic compound with an increased modality. The leaving group R of the bimodal ligand-metal catalyst is structurally different from the leaving group X of the first unimodal ligand-metal precatalyst. In some embodiments, at least one X is ((C 1 -C 20 )alkyl) 3-g -(phenyl) g Si-, wherein the subscript g is 0, 1, 2 or 3, alternatively wherein g is 0 or 1, alternatively 0, alternatively 1. In some aspects, at least one X is (C 6 -C 12 )Aryl-((C 0 -C 10 )alkylene)-CH 2 (e.g., benzyl). In some aspects, each X is independently (C 6 -C 12 )Aryl-((C 0 -C 10 )alkylene)-CH 2 Alternatively, one X is (C 6 -C 12 )Aryl-((C 0 -C 10 )alkylene)-CH 2 (e.g., benzyl), and the other X is F, Cl or methyl; alternatively, each X is benzyl. In some aspects, each X is benzyl; alternatively, one X is benzyl and the other X is F, Cl or methyl. In some embodiments, at least one X, alternatively each X is (C 1 -C 6 ) alkoxy-substituted (C 6 -C 12 ) aryl, or (C 1 -C 6 ) alkoxy-substituted benzyl. The ligand in the bimodal ligand-metal catalyst derived from a modally increased organic compound may be a group R ("ligand R"). The ligand R may have the formula (A), (B) or (C): -C(R 5 )=C(X)R 6 (A), -C(R 5 ) 2-C(X)=C(R 6 ) 2 (B) or -C(R 5 )(R 7 )-C(X)(R 6 )(R 7 )(C); where X and R 5 To R 7 In some embodiments, R is a ligand of formula (A) or (B), alternatively R is a ligand of formula (A) or (C), alternatively R is a ligand of formula (B) or (C), alternatively R is a ligand of formula (A), alternatively R is a ligand of formula (B), alternatively R is a ligand of formula (C).

[0055] In the ligand R of formula (A), (B) or (C), R 5 and R 6 Each of which is independently H or R 7 , and each R 7 Independently (C 1 -C 20 ) alkyl or (C 1 -C 17 ) heteroalkyl, provided that each R 7 Lack of carbon-carbon double bonds. 1 -C 20 ) The hydrocarbon group may be unsubstituted and consist of carbon atoms and hydrogen atoms, or (C 1 -C 20 The hydrocarbon group may be substituted and consists of carbon atoms, hydrogen atoms and one or more halogen atoms. Each halogen atom is independently selected from F, Cl, Br and I; alternatively selected from F, Cl and Br; alternatively selected from F and Cl; alternatively selected from F; alternatively selected from Cl. Unsubstituted (C 1 -C 20 ) The hydrocarbon group may be unsubstituted (C 1 -C 20 ) alkyl, unsubstituted (C 3 -C 20 ) cycloalkyl such as cyclohexyl, unsubstituted (C 6 -C 12 )Aryl, unsubstituted ((C 1 -C 4 )alkyl) 1-3 -phenyl or unsubstituted (C 6 -C 12 )Aryl-(C 1 -C 6 ) alkyl. Substituted (C 1 -C 20 ) The hydrocarbon group may be the aforementioned unsubstituted (C 1 -C20 ) a mono- or di-fluoro derivative of a hydrocarbon group, such as 2-(3,4-difluorophenyl)-ethen-1-yl (having formula (A)).

[0056] R 5 To R 7 Each of the embodiments (C 1 -C 19 ) heteroalkyl contains the same heteroalkyl group, which may be unsubstituted and consists of carbon atoms, hydrogen atoms and at least one heteroatom selected from N and O, or (C 1 -C 17 ) heteroalkyl may be substituted and consists of carbon atoms, hydrogen atoms, at least one heteroatom selected from N and O, and one or more halogen atoms. 1 -C 17 ) heteroalkyl may be (C 1 -C 19 ) heteroalkyl, (C 3 -C 19 ) heterocycloalkyl, (C 6 -C 12 ) heteroaryl, ((C 1 -C 4 )alkoxy) 1-3 -phenyl or (C 6 -C 12 )heteroaryl-(C 1 -C 6 ) alkyl. Substituted (C 1 -C 17 ) heteroalkyl may be the above unsubstituted (C 1 -C 17 ) mono- or di-fluoro derivatives of heteroalkyl groups, such as 2-(3,4-dimethoxyphenyl)-ethen-1-yl (having formula (A)).

[0057] The structure of the ligand R is different from the structure of the ligand X of the unimodal ligand-metal precatalyst and, for that matter, is also different from the anion A of the unimodal ligand-metal catalyst formed from the unimodal ligand-metal precatalyst. - structure.

[0058] An effective amount of a modality increasing organic compound (MIC). An amount of a modality increasing organic compound (MIC) sufficient to prepare a bimodal ligand-metal catalyst. The effective amount of the MIC can be expressed as an absolute value compared to the amount of (pre)catalyst metal M or as a relative value compared to the bimodal performance or a combination thereof.

[0059] In some embodiments, the absolute value of the effective amount of the modality-enhancing organic compound can be expressed as a molar ratio of the number of moles of the modality-enhancing organic compound to the number of moles of the metal M (“MICmol / M mol ”), wherein M is the M of the unimodal ligand-metal precatalyst of formula (I), for example, M is a Group 4 metal. In some embodiments, an effective amount of MIC is represented by MIC mol / M mol ≥0.50 / 1.0, alternatively ≥0.9 / 1.0, alternatively ≥1.0 / 1.0, alternatively ≥1.5 / 1.0, alternatively ≥1.9 / 1.0, alternatively ≥3 / 1.0, alternatively ≥5 / 1.0, alternatively ≥6 / 1.0, alternatively ≥9 / 1.0, alternatively ≥10.0 / 1.0, alternatively ≤10.0 / 1.0, alternatively ≤20.0 / 1.0, alternatively ≤30.0 / 1.0, alternatively ≤40.0 / 1.0, alternatively ≤50.0 / 1.0. In other words, the foregoing embodiments can be expressed as the inverse molar ratio of the number of moles of the metal M to the number of moles of the modally increased organic compound (“MIC”). mol / MIC mol ”) are described as follows: ≤1.0 / 0.5, alternatively ≤1.0 / 0.9, alternatively ≤1.0 / 1.0, alternatively ≤1.0 / 1.5, alternatively ≤1.0 / 1.9, alternatively ≤1.0 / 3.0, alternatively ≤1.0 / 5.0, alternatively ≤1.0 / 6.0, alternatively ≤1.0 / 9.0, alternatively ≤1.0 / 10.0, alternatively ≤1.0 / 20.0, alternatively ≤1.0 / 30.0, alternatively ≤1.0 / 40.0, alternatively ≤1.0 / 50.0, respectively. In some embodiments, the MIC mol / M mol Limited to at most 40 / 1, alternatively at most 30 / 1, alternatively at most 20 / 1, alternatively at most 10.0, alternatively at most 6.0, alternatively at most 5.0.

[0060] With respect to multimodal performance; an effective amount of a modally enhanced organic compound (MIC) can provide a bimodal ligand-metal catalyst having (i) a bimodal molecular weight distribution; (ii) an improved (e.g., reversed) comonomer distribution; or both (i) and (ii). In some embodiments, the bimodal ligand-metal catalyst and the effective amount of the MIC are characterized by feature (i). In some embodiments, the bimodal ligand-metal catalyst and the effective amount of the MIC are characterized by feature (ii).

[0061] In some embodiments, the bimodal nature of the bimodal ligand-metal catalyst is characterized by GPC, Mw / Mn, or both. In some embodiments, the bimodal ligand-metal catalyst is a catalyst made from any of the previously described unimodal ligand-metal precatalysts (1) to (2).

[0062] Comparative examples or non-inventive examples do not contain any mode-increasing organic compound or contain less than an effective amount of a mode-increasing organic compound.

[0063] Catalyst Activity. All other things being equal, the catalyst activity of a bimodal ligand-metal catalyst, determined as the catalyst's activity / polymerization productivity (expressed as grams of dry polyolefin product produced / grams of catalyst added to the reactor per hour (gPE / gcat-hr)), may not be significantly less than the catalytic activity / polymerization productivity of a post-metallocene catalyst having a faster light-off, and in some embodiments may be greater than the catalyst activity / polymerization productivity of a unimodal ligand-metal precatalyst.

[0064] Catalyst Structure. Without being bound by theory, it is believed that the molecular structure of the unimodal ligand-metal catalyst (formed from the unimodal ligand-metal precatalyst of Formula I) and the molecular structure of the bimodal ligand-metal catalyst can be determined by conventional analytical methods such as nuclear magnetic resonance (NMR) spectroscopy or gas chromatography / mass spectrometry (GC / MS).

[0065] Activation step. In some embodiments, the method of preparing a bimodal ligand-metal catalyst further comprises an activation step as a preliminary step, which can be performed before the combining step begins. The activation step comprises contacting a unimodal ligand-metal precatalyst of formula (I) with an activator under effective activation conditions for preparing a unimodal ligand-metal catalyst or a bimodal ligand-metal catalyst. The activation step can be performed in the absence of a modally increasing organic compound.

[0066] Activator. The activator for activating the unimodal ligand-metal precatalyst of formula (I) may be an alkylaluminoxane, an organoborane compound, an organoborate compound or a trialkylaluminum compound. The activator may also be a combination of any two or more thereof. For example, the activator may include an alkylaluminoxane (such as methylaluminoxane) and an organoborate compound, such as an organoborate having the CAS name of bis(hydrogenated tallow alkyl)methyltetra(pentafluorophenyl)borate amine, bis(hydrogenated tallow alkyl)methyltetra(pentafluorophenyl)borate (1-)amine. The activator for activating the cyclopentadienyl-containing ligand-metal (Ti, Zr or Hf) complex to obtain a metallocene catalyst may be a trialkylaluminum compound.

[0067] Alkylaluminoxane: also known as alkylalumoxane. A partial hydrolysis product of a trialkylaluminum compound. The embodiment may be (C 1 -C 10 ) alkylaluminoxane, alternatively (C 1 -C 6 ) alkylaluminoxane, alternatively (C1 -C 4 ) alkylaluminoxane, alternatively (C 1 -C 3 ) alkylaluminoxane, alternatively (C 1 -C 2 ) alkylaluminoxane, alternatively methylaluminoxane (MAO), alternatively modified methylaluminoxane (MMAO). In some aspects, the alkylaluminoxane is MAO. In some embodiments, the alkylaluminoxane is supported on untreated silica (such as fumed silica). The alkylaluminoxane can be obtained from a commercial supplier or prepared by any suitable method. Suitable methods for preparing alkylaluminoxanes are well known. Examples of such preparation methods are described in U.S. Pat. 4,665,208 , 4,952,540 , 5,091,352 , 5,206, 199 , 5,204,419 , 4,874,734 , 4,924,018 , 4,908,463 , 4,968,827 , 5,308,815 , 5,329,032 , 5, 248,801 , 5,235,081 , 5,157,137 、5,103,031、 5,391,793 , 5,391,529 and 5,693,838 ; and European publications EP-A-0 561 476; EP-B1-0 279 586; and EP-A-0 594-218; and PCT publication WO 94 / 10180.

[0068] The maximum amount of alkylaluminoxane can be selected to be a 5,000-fold molar excess of the precatalyst based on the molar ratio of the number of moles of Al metal atoms in the aluminoxane to the number of moles of metal atoms M (e.g., Ti, Zr, or Hf) in the precatalyst. The minimum amount of activator to precatalyst can be a 1:1 molar ratio (Al / M). The maximum value of the molar ratio of Al / M can be 150, alternatively 124.

[0069] Organoborane compounds. Tri(fluoro-functional organo)borane compounds ((fluoro-organo) 3 B), such as tris(pentafluorophenyl)borane ((C 6 F 5 ) 3 B), tris[3,5-bis(trifluoromethyl)phenyl]borane ((3,5-(CF 3 ) 2 -C 6 H 3 ) 3B), or a mixture of any two or more thereof.

[0070] Organic borate compounds. Tetra(fluoro-functional organic) borate compounds ((fluoro-organic) 4 B), such as N,N-dimethylanilinium tetrakis(pentafluorophenyl)borate, triphenylcarbonium tetrakis(pentafluorophenyl)borate, N,N-dimethylanilinium tetrakis[3,5-bis(trifluoromethyl)phenyl]borate, or triphenylcarbonium tetrakis[3,5-bis(trifluoromethyl)phenyl]borate, or a mixture of any two or more thereof. The organic borate compound may be methyl di((C 2-tetrakis(pentafluorophenyl)borate) available from Boulder Scientific. 14 -C 18 ) alkyl) ammonium salts, or by long chain trialkylamine (Armeen TM M2HT, available from Akzo Nobel, Inc.) and HCl and Li[B(C 6 F 5 ) 4 ] by reaction. Such preparation is disclosed in Example 2 of US 5,919,983. The organic borate compound can be used herein without (further) purification. In addition, bis (hydrogenated tallow alkyl) methyl tetrakis (pentafluorophenyl) boric acid amine.

[0071] The trialkylaluminum compound can be used as an activator for the precatalyst (metallocene precatalyst) or as a scavenger to remove residual water from the polymerization reactor before start-up. Examples of suitable alkylaluminum compounds are trimethylaluminum, triethylaluminum, triisobutylaluminum, tri-n-hexylaluminum and tri-n-octylaluminum.

[0072] Activators, also called cocatalysts, can affect the molecular weight, degree of branching, comonomer content or other properties of polyolefin polymers. Activators can achieve coordination polymerization or cationic polymerization.

[0073] Without being bound by theory, it is believed that the choice of activator used to activate the unimodal ligand-metal precatalyst does not affect the structure of the bimodal ligand-metal catalyst made from the unimodal ligand-metal precatalyst. That is, the structure of the bimodal ligand-metal catalyst prepared using different activators is expected to be the same.

[0074] Effective conditions. The reactions described herein (e.g., combination steps, activation steps, polymerization) are independently carried out in a situation where the reaction is allowed to proceed. Examples of effective conditions are reaction temperature, atmosphere type (e.g., inert atmosphere), reactant purity, reactant stoichiometry, stirring / mixing of reactants, and reaction time period. The conditions effective for the activation step and polymerization step may be those conditions described in the art and well known to those of ordinary skill. For example, effective activation conditions may include techniques for manipulating catalysts, such as online mixers, catalyst preparation reactors, and polymerization reactors. The activation temperature may be 20°C to 800°C, alternatively 300°C to 650°C. The reaction time may be 10 minutes to 2 hours. Examples of gas phase polymerization conditions are described later herein. Effective conditions for the combination step of the preparation of a bimodal ligand-metal catalyst may include: a reaction temperature of -50°C to 80°C, alternatively 0°C to 50°C, alternatively -50°C to 50°C, alternatively -50°C to 30°C; an inert atmosphere (e.g., nitrogen, helium, or water-free and O 2 of argon); does not contain water and O 2 and reactants with a purity of 90% to 100%; an amount of reactants to minimize waste / maximize product yield; stirring or mixing the reactants; and a reaction time period of 1 minute to 24 hours.

[0075] Effective reaction conditions for preparing bimodal ligand-metal catalysts. Such conditions may include techniques for manipulating air sensitivity and / or moisture sensitivity reagents and reactants, such as Schlenk-line technology and inert gas atmosphere (e.g., nitrogen, helium or argon). Effective reaction conditions may also include sufficient reaction time, sufficient reaction temperature and sufficient reaction pressure. Each reaction temperature may be independently -78°C to 120°C, alternatively -30°C to 30°C. Each reaction pressure may be independently 95kPa to 105kPa, alternatively 99kPa to 103kPa. The progress of any particular reaction step may be monitored by analytical methods such as nuclear magnetic resonance (NMR) spectroscopy and mass spectrometry to determine the reaction time that effectively maximizes the yield of the desired product. Alternatively, each reaction time may be independently 30 minutes to 48 hours.

[0076] Unimodal ligand-metal precatalysts (e.g., unimodal ligand-metal precatalysts of formula (I)). Unimodal ligand-metal precatalysts can be synthesized according to methods known in the art, including those mentioned herein. Alternatively, unimodal ligand-metal precatalysts can be obtained from precatalyst suppliers such as Boulder Scientific.

[0077] The metallocene catalyst can be various types of metallocene catalysts, such as those described in WO2014149360A1. In some aspects, the unimodal ligand-metal precatalyst is selected from: bi(η5 -tetramethylcyclopentadienyl)zirconium dichloride; bis(η 5 -tetramethylcyclopentadienyl)zirconium dimethyl; bis(η 5 -pentamethylcyclopentadienyl)zirconium dichloride; bis(η 5 dimethyl zirconium; (1,3-dimethyl-4,5,6,7-tetrahydroindenyl)(1-methylcyclopentadienyl) dimethyl zirconium; bis(1-methyl-3-n-butylcyclopentadienyl) zirconium dichloride; bis(1-methyl-3-n-butylcyclopentadienyl) dimethyl zirconium; bis(n-propylcyclopentadienyl) hafnium dichloride; bis(n-propylcyclopentadienyl) dimethyl hafnium; bis(n-butylcyclopentadienyl) zirconium dichloride; (cyclopentadienyl)(1,5-dimethylindenyl) dimethyl zirconium; (methylcyclopentadienyl)(1,5-dimethylindenyl) dimethyl zirconium; (cyclopentadienyl)(1,4-dimethylindenyl) dimethyl zirconium; (methylcyclopentadienyl)(1,4-dimethylindenyl) dimethyl zirconium; and bis(n-butylcyclopentadienyl) dimethyl zirconium. In some aspects, the bimodal ligand-metal catalyst is the product of an activation reaction of an activator with any of the aforementioned unimodal ligand-metal precatalysts.

[0078] Prepare polyolefin polymer by polymerization method.When 1-olefin monomer is the combination of ethylene and propylene, the polyolefin polymer made therefrom is ethylene / propylene copolymer.When 1-olefin monomer is ethylene alone, the polyolefin polymer made therefrom is polyethylene homopolymer.When 1-olefin monomer is the combination of ethylene and 1-butene, 1-hexene or 1-octene, the polyolefin polymer made therefrom is poly(ethylene-to-1-butene) copolymer, poly(ethylene-to-1-hexene) copolymer or poly(ethylene-to-1-octene) copolymer.In some embodiments, the polyolefin polymer made therefrom by 1-olefin monomer is a vinyl polymer with following components: 50 weight percent to 100 weight percent (wt%) repeating units are derived from ethylene, and 50 weight % to 0 weight % repeating units are derived from 1-olefin monomer, and the 1-olefin monomer is selected from propylene, 1-butene, 1-hexene, 1-octene and any two or more combinations thereof.

[0079] In some embodiments, the polymerization process uses a 1-olefin monomer and a comonomer that is a diene monomer (e.g., 1,3-butadiene). When the 1-olefin monomer is a combination of ethylene and propylene, and the polymerization also uses a diene monomer, the polyolefin polymer is an ethylene / propylene / diene monomer (EPDM) copolymer. The EPDM copolymer can be an ethylene / propylene / 1,3-butadiene copolymer.

[0080] Multimodal (e.g., bimodal or trimodal) catalyst systems. The bimodal catalyst system comprises a bimodal ligand-metal catalyst. The trimodal catalyst system comprises a bimodal ligand-metal catalyst, a second unimodal ligand-metal catalyst (e.g., a metallocene-type catalyst) made from a second unimodal ligand-metal precatalyst and an activator. The multimodal catalyst system prepares a multimodal polyethylene composition comprising a HMW polyethylene component and a LMW polyethylene component in a single reactor.

[0081] The method for preparing the bimodal ligand-metal catalyst can be carried out in the presence of a metallocene catalyst or a metallocene precatalyst. When carried out in the presence of a metallocene precatalyst, the method for activating the precatalyst of formula (I) with an activator also includes activating the metallocene precatalyst with the same or different activators. Typically, the method for preparing the bimodal ligand-metal catalyst is carried out in the absence of a metallocene (pre)catalyst.

[0082] Unsupported or supported catalysts. The unimodal ligand-metal precatalyst, unimodal ligand-metal catalyst, bimodal ligand-metal catalyst and multimodal catalyst system of formula (I) can be independently unsupported or arranged on a solid particulate support material. When there is no support material, the unimodal ligand-metal precatalyst, unimodal ligand-metal catalyst, bimodal ligand-metal catalyst and multimodal catalyst system of formula (I) can be injected into a slurry phase or gas phase polymerization reactor as a solution in a hydrocarbon solvent. When the unimodal ligand-metal precatalyst, unimodal ligand-metal catalyst, bimodal ligand-metal catalyst and multimodal catalyst system of formula (I) are arranged on a support material, they can be injected into a slurry phase or gas phase polymerization reactor as a slurry suspended in a hydrocarbon solvent or as a dried powder (i.e., a dried particulate solid).

[0083] The unimodal ligand-metal catalyst (made from a unimodal ligand-metal precatalyst) and / or the bimodal ligand-metal catalyst can be preformed in the absence of a support material and subsequently disposed on the support material. Alternatively, the unimodal ligand-metal precatalyst or the unimodal ligand-metal catalyst can be disposed on the support material, and then the unimodal ligand-metal catalyst and / or the bimodal ligand-metal catalyst can be prepared in situ on the support material.

[0084] The unimodal ligand-metal precatalyst, unimodal ligand-metal catalyst and / or bimodal ligand-metal catalyst of formula (I) can be prepared by a concentration process by evaporating a hydrocarbon solvent from a suspension or solution of a support material in a solution of the unimodal ligand-metal precatalyst, unimodal ligand-metal catalyst and / or bimodal ligand-metal catalyst of formula (I) in a hydrocarbon solvent. Alternatively, the unimodal ligand-metal precatalyst, unimodal ligand-metal catalyst and / or bimodal ligand-metal catalyst of formula (I) can be prepared by a spray drying process by spray drying a suspension or solution. In some embodiments, a spray drying process is used.

[0085] Support material. The support material is a granular solid which may be non-porous, semi-porous or porous. The support material is a porous support material. Examples of support materials are talc, inorganic oxides, inorganic chlorides, zeolites, clays, resins and mixtures of any two or more thereof. Examples of suitable resins are polystyrene, functionalized or cross-linked organic supports such as polystyrene divinyl benzene polyolefins. The support material may independently be untreated silica, alternatively calcined untreated silica, alternatively silica treated with a hydrophobic agent, alternatively silica treated with a calcined and hydrophobic agent. The hydrophobic agent may be dichlorodimethylsilane.

[0086] Inorganic oxide support materials include Group 2, 3, 4, 5, 13 or 14 metal oxides. Preferred supports include dehydrated or non-dehydrated silica, fumed silica, alumina (see, e.g., PCT Publication WO 99 / 60033), silica-alumina, and mixtures thereof. Other useful supports include magnesium oxide, titanium dioxide, zirconium oxide, magnesium chloride (U.S. Pat. No. 5,965,477), montmorillonite (EP 0 511 665), phyllosilicates, zeolites, talc, clay (U.S. Pat. No. 6,034,187), and the like. In addition, combinations of these support materials may be used, such as silica-chromium, silica-alumina, silica-titania, and the like. Additional support materials may include those porous acrylic polymers described in EP 0 767 184, which is incorporated herein by reference. Other support materials include nanocomposites as disclosed in PCT Publication WO 99 / 47598, aerogels as disclosed in PCT Publication WO 99 / 48605, spheroids as disclosed in US Pat. No. 5,972,510, and polymer beads as disclosed in PCT Publication WO 99 / 50311.

[0087] The carrier material may have a thickness of about 10 m 2 / g to about 700m 2 Surface area in the range of / g, about 0.1cm 3 / g to about 4.0cm3 The carrier material may be silica (e.g., fumed silica), alumina, clay, or talc. The fumed silica may be hydrophilic (untreated), alternatively hydrophobic (treated). In some aspects, the carrier is a hydrophobic fumed silica, which may be prepared by treating untreated fumed silica with a hydrophobic agent such as dimethyldichlorosilane, polydimethylsiloxane fluid, or hexamethyldisilazane. In some aspects, the treating agent is dimethyldichlorosilane. In one embodiment, the carrier is Cabosil. TM TS-610.

[0088] The one or more precatalysts and / or one or more activators may be deposited on, contacted with, vaporized with, bonded with, incorporated into, adsorbed or absorbed into or onto one or more carrier or support materials.

[0089] The unimodal ligand-metal precatalyst may be spray dried according to the general method described in US5648310. The support for use with the bimodal ligand-metal catalyst may be functionalized as generally described in EP 0 802 203 or at least one substituent or leaving group may be selected as described in US5688880.

[0090] Solution phase polymerization and / or slurry phase polymerization of olefin monomers is well known. See, for example, US Pat. No. 8,291,115 B2.

[0091] Inert hydrocarbon solvent. Alkanes, aromatic hydrocarbons or alkyl aromatic hydrocarbons (i.e., aryl alkanes). Examples of inert hydrocarbon solvents are alkanes, such as mineral oil, pentane, hexane, heptane, octane, nonane, decane, undecane, dodecane, etc., and toluene and xylene. In one embodiment, the inert hydrocarbon solvent is an alkane or a mixture of alkanes, wherein each alkane independently has 5 to 20 carbon atoms, alternatively 5 to 12 carbon atoms, alternatively 5 to 10 carbon atoms. Each alkane can be independently acyclic or cyclic. Each noncyclic alkane can be independently straight or branched. Noncyclic alkane can be pentane, 1-methylbutane (isopentane), hexane, 1-methylpentane (isohexane), heptane, 1-methylhexane (isoheptane), octane, nonane, decane or any two or more mixtures thereof. The cyclic alkane can be cyclopentane, cyclohexane, cycloheptane, cyclooctane, cyclononane, cyclodecane, methylcyclopentane, methylcyclohexane, dimethylcyclopentane, or a mixture of any two or more thereof. Additional examples of suitable alkanes include Isopar-C, Isopar-E, and mineral oils such as paraffin oil. In some aspects, the inert hydrocarbon solvent does not contain mineral oil. The inert hydrocarbon solvent can be composed of one or more (C 5 -C 12 ) alkane composition.

[0092] Gas phase polymerization (GPP). Polymerization uses a GPP reactor, such as a stirred bed gas phase polymerization reactor (SB-GPP reactor) or a fluidized bed gas phase polymerization reactor (FB-GPP reactor). Such reactors and methods are generally well known. For example, FB-GPP reactors / methods can be as described in US 3,709,853, US 4,003,712, US 4,011,382, US 4,302,566, US 4,543,399, US 4,882,400, US 5,352,749, US 5,541,270, US 2018 / 0079836 A1, EP-A-0 802 202, and Belgian Patent No. 839,380. These SB-GPP and FB-GPP polymerization reactors and methods mechanically stir or fluidize the polymerization medium inside the reactor by the continuous flow of gaseous monomers and diluents, respectively. Other useful reactors / processes contemplated include tandem or multistage polymerization processes such as described in US 5,627,242, US 5,665,818, US 5,677,375, EP-A-0 794 200, EP-B1-0 649 992, EP-A-0 802 202, and EP-B-634 421.

[0093] Gas phase polymerization operating conditions are any variable or combination of variables that may affect the polymerization reaction in the GPP reactor or the composition or properties of the polyolefin polymer composition product produced therefrom. Variables may include: reactor design and size; precatalyst composition and amount; reactant composition and amount; molar ratio of two different reactants; feed gas (such as H 2 ), the molar ratio of feed gas to reactant, interfering materials (e.g., H 2 O and / or O 2 ), the absence or concentration of induced condensing agents (ICAs), the average polymer residence time in the reactor, the partial pressures of the components, the feed rate of the monomers, the reactor bed temperature (e.g., fluidized bed temperature), the nature or sequence of the process steps, the transition time periods between steps. Variables other than those variables described or varied by the process or use may be held constant.

[0094] In the GPP method, ethylene (“C 2 ”), hydrogen (“H 2 ”) and 1-hexene (“C 6 " or "C x ”, where x is 6) to maintain a fixed comonomer to ethylene monomer gas molar ratio or feed mass ratio (Cx / C 2 , for example C 6 / C 2 ), a constant hydrogen to ethylene gas molar ratio or feed mass ratio ("H 2 / C 2 ”), and a constant ethylene (“C 2 ") partial pressure. Gas concentrations were measured by online gas chromatography to understand and maintain the composition of the recycle gas stream. The reaction bed of growing polymer particles was maintained in a fluidized state by continuous flow of make-up feed and recycle gas through the reaction zone. A superficial gas velocity of 0.49 to 0.79 m / sec (1.6 to 2.6 ft / sec) was used. The reaction was carried out at a total pressure of about 2068 kilopascals (kPa) to about 2758 kilopascals (about 300 pounds per square inch-gauge (psig) to about 400 pounds per square inch-gauge) and And operate FB-GPP reactor under described first reactor bed temperature RBT.By extracting a part of bed at a rate equal to the production rate of polyolefin polymer composition in particle form, fluidized bed is maintained at constant height, and this production rate can be 5,000 kilograms / hour (kg / h) to 150,000 kg / h.Via a series of valves, product polyolefin polymer composition is semi-continuously moved into fixed volume chamber, wherein the multimodal (for example, bimodal or trimodal) ethylene-to-1-hexene copolymer composition of this removal is purged to remove entrained hydrocarbons and is purged with moist nitrogen (N 2 ) gas stream to deactivate any traces of residual catalyst.

[0095] The catalyst system can be fed into the polymerization reactor in "dry mode" or "wet mode", alternatively dry mode, alternatively wet mode. The dry mode is a dry powder or granules. The wet mode is a suspension in an inert liquid such as mineral oil.

[0096] Induced Condensing Agent (ICA). An inert liquid that can be used to cool materials in a GPP reactor. Its use is optional. ICA is (C 3 -C 20 ) alkane, alternatively (C 5 -C 20) alkane, such as 2-methylbutane (i.e., isopentane). See US 4,453,399, US 4,588,790, US 4,994,534, US 5,352,749, US 5,462,999, and US 6,489,408. The ICA concentration in the reactor may be 0.1 mol% to 25 mol%, alternatively 1 mol% to 16 mol%, alternatively 1 mol% to 10 mol%.

[0097] The GPP conditions may also include one or more additives such as chain transfer agents or promoters. Chain transfer agents are well known and may be metal alkyls such as diethyl zinc. Promoters are known such as those described in US 4,988,783 and may include chloroform, CFCl 3 , trichloroethane and difluorotetrachloroethane. A scavenger may be used to react with moisture before reactor startup, and a scavenger may be used to react with excess activator during reactor conversion. The scavenger may be a trialkylaluminum. The GPP may be operated without (not intentionally added) a scavenger. The GPP reactor / process may also include an amount (e.g., 0.5 ppm to 200 ppm based on all feeds entering the reactor) of one or more static control agents and / or one or more continuity additives, such as aluminum stearate or polyethyleneimine. Static control agents may be added to the FB-GPP reactor to inhibit the formation or accumulation of static charge therein.

[0098] The GPP reactor may be a commercial scale FB-GPP reactor, such as the UNIPOL 1000 reactor available from Univation Technologies, LLC, a subsidiary of The Dow Chemical Company, Midland, Michigan, USA. TM Reactor or UNIPOL TM II reactor.

[0099] 1-Olefin monomer. 1-Olefin monomer is a monomer of formula H 2 C=C(H)(CH 2 ) n R 8 The compound wherein the subscript n is an integer from 0 to 19, and the group R 8 H or CH 3 An example is ethylene (subscript n is 0 and R 8 H), propylene (subscript n is 0 and R 8 CH 3 ) and (C 4 -C 20)α-olefin (subscript n is an integer from 1 to 19 and R 8 H or CH 3 ). In some embodiments, the 1-olefin monomer is ethylene, propylene, 1-butene, 1-hexene, 1-octene, or a combination of any two or more thereof. In some embodiments, the 1-olefin monomer is a combination of ethylene and propylene. In other embodiments, the 1-olefin monomer is ethylene alone, or a combination of ethylene and 1-butene, 1-hexene, or 1-octene.

[0100] Polyolefin polymers. The product of polymerization of at least one 1-olefin monomer with a bimodal ligand-metal catalyst or a multimodal catalyst system. A macromolecule or a collection of macromolecules having constituent units derived from at least one 1-olefin monomer. For example, when at least one 1-olefin monomer consists of ethylene, the polyolefin polymer consists of a polyethylene homopolymer. When at least one 1-olefin monomer consists of ethylene and propylene, the polyolefin polymer consists of an ethylene / propylene copolymer. When at least one 1-olefin monomer consists of ethylene and a comonomer selected from 1-butene, 1-hexene and 1-octene, the polyolefin polymer is selected from poly(ethylene-to-1-butene) copolymers, poly(ethylene-to-1-hexene) copolymers and poly(ethylene-to-1-octene) copolymers, respectively.

[0101] The polyolefin polymer can be a homopolymer or a copolymer. The polyolefin polymer made by the multimodal catalyst system has a multimodal (e.g., bimodal or trimodal) molecular weight distribution, and comprises a higher molecular weight (HMW) polyolefin polymer component and a lower molecular weight (LMW) polyolefin polymer component. The HMW polyolefin polymer component and the LMW polyolefin polymer component can be prepared by a bimodal ligand-metal catalyst.

[0102] Any compound, composition, formulation, material, mixture or reaction product herein may not contain any one of the chemical elements selected from the group consisting of: H, Li, Be, B, C, N, O, F, Na, Mg, Al, Si, P, S, Cl, K, Ca, Sc, Ti, V, Cr, Mn, Fe, Co, Ni, Cu, Zn, Ga, Ge, As, Se, Br, Rb, Sr, Y, Zr, Nb, Mo, Tc, Ru, Rh, Pd, Ag, Cd, In, Sn, Sb, Te, I, Cs, Ba, Hf, Ta, W, Re, Os, Ir, Pt, Au, Hg, Tl, Pb, Bi, lanthanides and actinides; provided that the chemical elements required for the compound, composition, formulation, material, mixture or reaction product (e.g., Zr required for the zirconium compound, or C and H required for polyethylene, or C, H and O required for the alcohol) are not counted.

[0103] Alternatively, before different embodiments. ASTM is a standards organization, ASTM International, West Conshohocken, Pennsylvania, USA. Any comparative examples are for illustrative purposes only and should not be prior art. Containing or lacking means completely absent; or undetectable. IUPAC is the International Union of Pure and Applied Chemistry (IUPAC Secretariat, Research Triangle Park, North Carolina, USA). The periodic table is the IUPAC version released on May 1, 2018. Permitted options can be given, but not essential. Operability means functionally capable or effective. Optional (ground) means absence (or exclusion) or presence (or inclusion). Properties can be measured using standard test methods and conditions. Ranges include endpoints, subranges, and integers and / or fractional values ​​contained therein, except for integer ranges that do not include fractional values. Room temperature: 23°C ± 1°C

[0104] Unless otherwise indicated, the definitions of terms used herein are taken from the "IUPAC Compendium of Chemical Technology" ("Gold Book"), version 2.3.3, February 24, 2014. For convenience, some definitions are given below.

[0105] Example

[0106] Additional embodiments of the present invention are the aforementioned aspects and the claims described later, which describe a range of processing conditions and / or a range of material properties, wherein in the additional embodiments of the present invention, the end values ​​of the range of processing conditions and / or the end values ​​of the range of material properties are modified to any exemplary processing condition value and / or any exemplary material property value described below in this section for any example of the present invention, respectively.

[0107] The absence of exogenous organometallic compounds means that there is no external source of organic compounds containing metal atoms, such as an external source of a catalyst different from the first unimodal ligand-metal precatalyst, and there is no precatalyst different from the first precatalyst, i.e., there is no means of preparing the second unimodal ligand-metal catalyst in situ in the combining step. Prior to the combining step, the first unimodal ligand-metal precatalyst can be a component of a multimodal (e.g., bimodal) precatalyst system consisting essentially of the first unimodal ligand-metal precatalyst, a metallocene-type catalyst (an endogenous (pre-loaded, not exogenous) second unimodal ligand-metal catalyst), and an optional support material.

[0108] The catalyst system or polymerization process may optionally have at least one additive. At least one additive may be a flow aid for preventing agglomeration of dry catalyst particles; an antistatic compound for inhibiting the accumulation of charge on polyolefin particles in a floating bed gas phase polymerization reactor; or an antifouling compound such as a metal carboxylate for inhibiting reactor fouling.

[0109] Bimodal means a molecular weight distribution determined by GPC having two and only two peaks, wherein the two peaks may be in a head-shoulder configuration or in a double-head configuration with a local minimum (valley) therebetween. It may also refer to a catalyst that produces such a bimodal molecular weight distribution.

[0110] A bimodal ligand-metal catalyst means a catalyst made from a unimodal ligand-metal precatalyst, an activator, and a modality-enhancing organic compound, which produces polyolefins having a bimodal molecular weight distribution as determined by GPC in a single polymerization reactor in the absence of another catalyst. Activation of a unimodal ligand-metal precatalyst with an activator in the absence of a modality-enhancing organic compound will produce a unimodal ligand-metal catalyst.

[0111] Catalyst refers herein to a material that can polymerize monomers and optionally comonomers to prepare a polymer. The catalyst may be an olefin polymerization catalyst that can polymerize olefin monomers (e.g., ethylene) and optional olefin comonomers (e.g., propylene and / or (C 4 -C 20 )α-olefins) in order to prepare polyolefin homopolymers or optionally polyolefin copolymers, respectively.

[0112] Catalyst system A group of at least two chemical components and / or their reaction products, which together as a whole to increase the reaction rate, wherein at least one of the at least two chemical components is a catalyst. Other chemical components can be independently selected from different catalysts, support materials, excessive activators, catalyst additives such as antistatic agents, cocatalysts, carboxylic acid metal salts, dispersants for preventing the particles of the catalyst system from sticking together. The catalyst system can include a catalyst and a support material, wherein the catalyst is disposed on a support material, and the support material accommodates and provides a physical framework for increasing the distribution of the catalyst surface. The catalyst system does not include monomers, comonomers or modally increased organic compounds.

[0113] Chemical conversion. The bimodal ligand-metal catalyst is prepared by a chemical reaction. The chemical reaction occurs between a first unimodal ligand-metal precatalyst, an activator, and an organic compound with increased modality. That is, the bimodal ligand-metal catalyst is prepared by chemically converting the first unimodal ligand-metal precatalyst into a ligand-metal catalyst with functionality that produces a bimodal polymer. The bimodal ligand-metal catalyst is not prepared by a simple addition method that combines two different catalysts together, such as by mixing a first unimodal ligand-metal precatalyst and an activator with a second unimodal ligand-metal precatalyst. When the second unimodal ligand-metal precatalyst is present during the combining step (i.e., in the first bimodal catalyst system), the second unimodal ligand-metal precatalyst is a bystander in the chemical conversion that affects the modality. The organic compound with increased modality does not contain metal atoms. Therefore, it is quite surprising that the organic compound with increased modality can increase the modality of the catalyst prepared by the first unimodal ligand-metal precatalyst.

[0114] Essentially consisting of means free of exogenous organometallic compounds. The exogenous organometallic compound is compositionally different from the first unimodal ligand-metal precatalyst. The second precatalyst is compositionally different from the first precatalyst used to prepare the first unimodal ligand-metal precatalyst. Therefore, the process of the present invention cannot be achieved by adding an exogenous organometallic compound or a second precatalyst precursor thereof to the first unimodal ligand-metal precatalyst. Therefore, the contacting step of the process is carried out in the absence of an exogenous organometallic compound or a second precatalyst precursor thereof. The process of the present invention also cannot be achieved by removing a selective catalyst poison from a semi-poisoned bimodal ligand-metal catalyst. The first unimodal ligand-metal precatalyst and the second unimodal ligand-metal precatalyst are endogenous organometallic compounds and are not self-modifying, such that they cannot increase the modality of themselves or each other. In the absence of a modality-increasing organic compound, there is no modality increase.

[0115] Endogenous. Having an internal cause or origin, or pre-load.

[0116] Exogenous. Having an external cause or origin, or obtained from an external source.

[0117] Feed. The conveying or physical movement of material from outside a space (e.g., outside a polymerization reactor) to inside a space (inside a polymerization reactor).

[0118] The first unimodal ligand-metal precatalyst. It means a transition metal compound, when it does not contain (does not contact) the organic compound with increased modality, when contacted with an activator, a unimodal ligand-metal catalyst is produced. The first unimodal ligand-metal catalyst prepares a unimodal polymer, and therefore if a bimodal polymer is required, the first unimodal ligand-metal precatalyst needs to be chemically converted into a bimodal ligand-metal catalyst. The method of the present invention can advantageously achieve such a chemical conversion without using an exogenous organometallic compound to carry out the chemical conversion. This is carried out by contacting the first unimodal ligand-metal precatalyst with the first activator and the organic compound with increased modality, thereby preparing a bimodal ligand-metal catalyst.

[0119] GPC means gel permeation chromatography.

[0120] An internal olefin is an olefin that is not terminal, ie, the carbon-carbon π bond is not at the end of the carbon chain. That is, the internal olefin does not have a terminal carbon-carbon double bond or a terminal carbon-carbon triple bond.

[0121] Leaving group. A group that is bonded to the metal atom of the ligand-metal precatalyst and is captured by the activator during activation of the precatalyst to the ligand-metal catalyst. An example of a leaving group is the monodentate group X in formula (I). Each ligand-metal precatalyst described herein implicitly has at least one leaving group, and typically has two leaving groups.

[0122] Ligand. A monovalent, divalent, trivalent or tetravalent and di-, tri- or tetra-coordinated organic group having two, three or four coordination functional groups for bonding to the metal atom of the ligand-metal precatalyst, respectively. The ligand remains coordinated to the metal atom in the ligand-metal catalyst prepared by activating the precatalyst. Thus, a ligand represents a group in the ligand-metal precatalyst that is carried to the ligand-metal catalyst prepared by activating the precatalyst, and a leaving group represents an unstable group, at least one of which is captured by the activator during the activation of the precatalyst. An example of a ligand is a BPP-type ligand, which is a divalent tetra-coordinated organic group.

[0123] Metal atom means a base unit of any of the elements of Groups 1 to 13, rows 3 to 6 of Groups 14 to 16, rows 5 and 6 of Group 17, lanthanides, actinides, all of the Periodic Table of the Elements published by IUPAC on December 1, 2018.

[0124] "Modal addition" or "increasing modality" means transforming the molecular weight distribution of a polyolefin polymer prepared from an olefin polymerization catalyst by adding at least one, alternatively only one, mode to the polyolefin polymer. Examples of modal addition are adding one mode to a unimodal molecular weight distribution to obtain a bimodal molecular weight distribution; adding one mode to a bimodal molecular weight distribution to obtain a trimodal molecular weight distribution; or adding two modes to a unimodal molecular weight distribution to obtain a trimodal molecular weight distribution. Thus, an example of adding one mode to a unimodal ligand-metal catalyst to prepare a bimodal ligand-metal catalyst is adding one mode to an olefin polymerization catalyst for preparing a polyolefin polymer having a unimodal molecular weight distribution (i.e., the unimodal ligand-metal catalyst is a unimodal olefin polymerization catalyst) to obtain an olefin polymerization catalyst for preparing a polyolefin polymer having a bimodal molecular weight distribution (i.e., the bimodal ligand-metal catalyst is a bimodal olefin polymerization catalyst). Typical modal addition means adding one mode to a unimodal molecular weight distribution to obtain a bimodal molecular weight distribution.

[0125] The modality-enhanced organic compound means a non-catalytic, metal-free carbon-based molecule composed of carbon atoms, hydrogen atoms, optionally zero, one or more halogen atoms, and optionally zero, one or more heteroatoms independently selected from O, N, P and Si; wherein the molecule contains at least one internal carbon-carbon double bond (CC=CC), one olefinic group (C=C=C) or at least one carbon-carbon triple bond (HC≡CH, HC≡CC or CC≡CC), and serves to chemically transform the molecular structure of the first unimodal ligand-metal precatalyst into a bimodal ligand-metal catalyst. The modality-enhanced organic compound itself does not contain metal atoms. Because it is known that polymerizable olefin monomers such as ethylene, α-olefins such as propylene or (C 4 -C 20 )α-olefins, 1, #-dienes (where # is an integer of 3 or higher) do not increase the mode (whether unimodal, bimodal, trimodal) of the molecular weight distribution of the polyolefin polymer prepared by the olefin polymerization catalyst, and therefore, by definition, "modality-increasing organic compounds" do not include polymerizable olefin monomers (e.g., olefins with terminal carbon-carbon double bonds). The conversion can be advantageously completed in the absence of an exogenous organometallic compound and its second precatalyst precursor. The conversion can also be advantageously completed in the absence of a second activator.

[0126] Multimodal means a molecular weight distribution with two or more peaks as determined by GPC, wherein the two or more peaks may independently be a head-shoulder configuration or a double-headed or multi-headed configuration with a local minimum (valley) therebetween. Examples of multimodal are bimodal and trimodal. . It may also refer to a catalyst that produces such a multimodal molecular weight distribution.

[0127] An organic compound means a chemical entity consisting of carbon atoms, hydrogen atoms, optionally zero, one or more halogen atoms, and optionally zero, one or more heteroatoms independently selected from O, N, P and Si per molecule. The molecule does not have, i.e., does not contain, metal atoms (i.e., the chemical entity does not include an organometallic compound).

[0128] Reaction conditions, including polymerization conditions, are the environmental conditions under which a chemical transformation (eg, polymerization) is carried out, such as temperature, pressure, solvent, concentration of reactants, etc. All chemical transformations described herein are carried out under suitable and effective reaction conditions.

[0129] Short chain branching distribution per 1000 carbon atoms or SCBD / 1000C. Weight percent (wt%) of the bimodal copolymer. Change in comonomer content relative to the log (weight average molecular weight (M)) of the bimodal copolymer. w )) as measured by GPC. The comonomer content can be plotted on the y-axis against log(M) on the x-axis. w ) and plotted in log(M w )4 to log(M w )6 (i.e., M w 10,000 to M w 1,000,000) to visually detect by examining the slope of the graph. A normal SCBD / 1000C is indicated by a negative (downward trending) slope, which indicates that log(M w ) increases, the weight % of the comonomer content decreases. A decreasing normal SCBD / 1000C means that the degree of negative slope decreases (e.g., from a slope of -3 to a slope of -2). A flat SCBD / 1000C is represented by a zero slope (flat trend), which means that log(M w ) increases, the weight % of the comonomer content remains approximately the same. Reverse SCBD / 1000C is indicated by a positive (upward trending) slope, which indicates that log(M w ) increases, the weight % of the comonomer content increases. An enhanced reverse SCBD / 1000C means that the degree of the positive slope increases (e.g., from a slope of +2 to a slope of +3).

[0130] Support material refers to finely divided particulate inorganic solids capable of supporting the catalyst.

[0131] Trimodal means a molecular weight distribution as determined by GPC having three and only three peaks. It can also refer to a catalyst that produces such a trimodal molecular weight distribution.

[0132] Unimodal means a molecular weight distribution having one and only one peak as determined by GPC. It can also refer to the catalyst that produces such a unimodal molecular weight distribution.

[0133] A unimodal ligand-metal catalyst refers to a catalyst for preparing a polyolefin having a unimodal molecular weight distribution as determined by GPC. Therefore, if a bimodal polymer is desired, the first unimodal ligand-metal precatalyst needs to be chemically converted into a bimodal ligand-metal catalyst. The prior art will do this by adding a combination of a first unimodal ligand-metal precatalyst and an exogenous transition metal compound precatalyst in contact with an activator to prepare a bimodal catalyst comprising two or more different catalyst compounds. The method of the present invention can advantageously achieve such a chemical conversion without using an exogenous transition metal compound precatalyst. That is, the method of the present invention can advantageously achieve such a chemical conversion by: under conditions effective for an activator and an organic compound with increased modality, a component consisting essentially of a first unimodal ligand-metal precatalyst, an effective amount of an activator and an effective amount of an organic compound with increased modality and / or consisting of them is combined in any order to chemically convert the first unimodal ligand-metal precatalyst into a bimodal ligand-metal catalyst.

[0134] Unsupported means free of inorganic support material (eg, silica).

[0135] Methods for chemically converting a unimodal ligand-metal precatalyst into a bimodal ligand-metal catalyst are described herein. The bimodal ligand-metal catalyst and / or a catalyst system comprising at least a bimodal ligand-metal catalyst (e.g., a bimodal catalyst system and / or a trimodal catalyst system) can be used in a single polymerization reactor to prepare a multimodal polymer as described herein.

[0136] Formula (A) is provided as follows 1 )、(B 1 ) or (C 1 ) of organic compounds with modal increase: R 5 -C≡CR 6 (A 1 )、(R 5 ) 2 C=C=C(R 6 ) 2 (B 1 ) or (R 5 )(R 7 )C=C(R 6 )(R 7 )(C 1 ), as described in detail herein. The modal-increasing organic compound (MIC1) is commercially available from Sigma-Aldrich. The modal-increasing organic compound (MIC8) is commercially available from Sigma-Aldrich. The modal-increasing organic compound (MIC15) is commercially available from Sigma-Aldrich.

[0137] The monomodal ligand-metal precatalyst structure (1) was synthesized according to the procedure of WO 2012 / 027448 A1.

[0138]

[0139] The monomodal ligand-metal precatalyst structure (2) was synthesized according to WO2018170227 A1.

[0140]

[0141] The bimodal ligand-metal catalyst of Inventive Examples 1-3 (IE1-3) was prepared as follows. In a nitrogen purged glove box, an oven dried glass bottle was charged with 0.795 grams (g) of treated fumed silica (CABOSIL TS-610; available from WR Grace) slurried in 22.5 g of toluene (available from Aldrich) and stirred with a stir bar until fully dispersed. 6.6 g of 10 wt % methylaluminoxane (MAO) (available from WR Grace in the form of 10 wt % in toluene) was added to the bottle to form a mixture. The mixture was magnetically stirred for 15 minutes, then the unimodal ligand-metal catalyst of structure (1) (0.096 g) and the modally enhanced organic compound of structure (MIC15) (1 equivalent; 0.096 g) were added and the mixture was stirred for 30 minutes to 60 minutes. The mixture was spray dried using a Buchi Mini Spray Dryer B-290 with the following parameters to produce the dried and activated bimodal ligand-metal catalyst of Example 1: set temperature - 185°C, outlet temperature - 100°C (min), exhaust fan - 95 and pump speed - 150 rpm.

[0142] The unimodal ligand-metal catalyst of Comparative Example 4 (CE4) was prepared identically to the bimodal ligand-metal catalysts of IE1-3, with the change being the absence of the modality-enhancing organic compound (not present in any amount), as shown in Table 1.

[0143] Inventive embodiment 4-6 (IE4-6) was prepared identically to IE1-3, except that the organic compound at the modal addition of structure (MIC15) was present in 5 equivalents under the conditions shown in Table 1.

[0144] Inventive embodiment 7-9 (IE7-9) was prepared identically to IE1-3, except that the modal-increasing organic compound of structure (MIC8) was used in 5 equivalents under the conditions as shown in Table 1.

[0145] Inventive embodiment 10-11 (IE10-11) was prepared identically to IE1-3, except that the modal-increasing organic compound of structure (MIC1) was used in 5 equivalents under the conditions as shown in Table 1.

[0146] Inventive embodiment 12-13 (IE12-13) was prepared identically to IE1-3, except that the modal addition organic compound of structure (MIC1) was used in 10 equivalents under the conditions shown in Table 1.

[0147] Inventive Example 14 was prepared identically to Example 1, except that the unimodal ligand-metal precatalyst of structure (2) was used in five equivalents (molar equivalents) under the conditions as shown in Table 1.

[0148] The unimodal ligand-metal catalyst of Comparative Example 4 (CE4) was prepared identically to the bimodal ligand-metal catalysts of EX1-3 under the conditions as indicated in Table 1, except that a unimodal ligand-metal precatalyst of structure (2) was used and no modal increasing organic compound was present (not present in any amount).

[0149] The gas phase ethylene / 1-hexene copolymerization of the bimodal ligand-metal catalyst of IE1-14 and the unimodal ligand-metal catalyst of CE1-4 was carried out in the gas phase in a 2 liter (L) semi-batch autoclave polymerization reactor equipped with a mechanical stirrer as follows. The reactor was first dried for 1 hour, 200 g of sodium chloride (NaCl) was added, and dried by heating at 100° C. for 30 minutes under nitrogen. After drying, 5 g of silica-supported methylaluminoxane (SMAO) was introduced as a scavenger under nitrogen pressure. After the addition of SMAO, the reactor was sealed and the components were stirred. The reactor was then charged with hydrogen (H 2 preloaded as indicated below for each of Conditions 1, 2, and 3) and hexene (C 6 / C 2 Ratios, as indicated below for each of Conditions 1, 2, and 3) and then pressurized with ethylene at 100 pounds per square inch (psi). Once the system reached steady state, the type and amount of polymerization catalyst for each of IE1-14 and CE1-4 was charged into the reactor at 80°C to start polymerization of each of the catalysts for IE1-14 and CE1-4. The reactor temperature was brought to 90°C and set to that temperature throughout the 1 hour run. Runs were conducted under Conditions 1, 2, or 3, as identified in Table 1 and detailed below. At the end of the run, the reactor was cooled, vented, and opened. The resulting product mixture was washed with water and methanol and then dried.

[0150] The results for IE1-14 and CE1-4 are shown in Tables 1, 2 and 3.

[0151] For each batch reactor run, the catalyst activity / polymerization productivity was calculated as grams of dry polyolefin product produced / grams of catalyst added to the reactor per hour (gPE / gcat-hr). Higher values ​​of gPE / gcat-hr indicate higher catalyst activity / polymerization productivity.

[0152] The melting temperature (ie, Tm) can be determined via differential scanning calorimetry according to ASTM D 3418-08. For example, a scan rate of 10°C / min is used for a 10 mg sample and a second heating cycle is used.

[0153] Mw, Mn and Mw / Mn are determined by using a high temperature gel permeation chromatography (Polymer Laboratories) equipped with a differential refractive index detector (DRI). Three Polymer Laboratories PLgel 10 μm mixed-B columns are used. The nominal flow rate is 1.0 mL / min, and the nominal injection volume is 300 μL. Various transmission lines, columns and differential refractometers (DRI detectors) are contained in an oven maintained at 160°C. The solvent used for the experiment is prepared by dissolving 6 grams of butylated hydroxytoluene as an antioxidant in 4 liters of Aldrich reagent grade 1, 2, 4 trichlorobenzene (TCB). The TCB mixture is then filtered through a 0.1 μm Teflon filter. TCB is then degassed with an online degasser before entering the GPC instrument. By placing the dried polymer in a glass vial, adding the desired amount of TCB, the mixture is then heated at 160°C and continuously shaken for about 2 hours to prepare a polymer solution. All amounts are measured by gravimetric analysis. The injection concentration was 0.5 mg / ml-2.0 mg / ml, with lower concentrations used for higher molecular weight samples. Before running each sample, the DRI detector was cleaned. The flow rate in the device was then increased to 1.0 ml / min, and the DRI was allowed to stabilize for 8 hours before the first sample was injected. Molecular weights were determined by combining a universal calibration relationship with column calibration, which was performed with a series of monodisperse polystyrene (PS) standards. The MW was calculated at each elution volume using the following equation:

[0154]

[0155] The variables with the subscript "X" represent the test sample, while those with the subscript "PS" represent the PS. PS =0.67 and K PS =0.000175, and a X and K Xand are obtained from published literature. Specifically, for PE, a / K=0.695 / 0.000579, and for PP, a / K=0.705 / 0.0002288. Using the following equation, the baseline-subtracted DRI signal I DRI Calculate the concentration c at each point in the chromatogram: c = K DRI I DRI / (dn / dc)

[0156] Where K DRI is a constant determined by calibrating the DRI, and (dn / dc) is the refractive index increment of the system. Specifically, for polyethylene, dn / dc=0.109. The mass recovery is calculated from the ratio of the integrated area of ​​the concentration chromatogram to the elution volume and the injection mass, which is equal to the predetermined concentration multiplied by the injection loop volume.

[0157] Unless otherwise stated, all molecular weights are reported in g / mol. If a conflict occurs between the GPC-DRI procedure and "Fast GPC", the GPC-DRI procedure immediately above should be used. Further details on methods for determining Mw, Mn, MWD are described in US 2006 / 0173123, pages 24-25, paragraphs

[0334] to

[0341] .

[0158] Mp is the MW of the maximum, so the bimodal polymer Mp-1 and Mp-2 are the corresponding local maxima of the bimodal polymer (of the HMW and LMW peaks), and Mp-1>Mp-2. When the polymer is unimodal, or does not have two discrete local maxima, then Mp-1=Mp-2=Mp.

[0159] The distribution of a bimodal polymer is given by (Mp-1)–(Mp-2).

[0160] The short chain branching / comonomer content (wt% c6) is determined using GPC, wherein the comonomer content (wt%) incorporated into the polymer is determined by rapid FT-IR spectroscopy of the dissolved polymer in the GPC measurement. For example, the comonomer content is determined by using an infrared detector such as an IR5 detector in a gel permeation chromatography measurement to determine the polymer molecular weight, as described in "Toward Absolute Chemical Composition Distribution Measurement of Polyolefins by High-Temperature Liquid Chromatography Hyphenated with Infrared Absorbance and Light Scattering Detectors" by Dean Lee, Colin Li Pi Shan, David M. Meunier, John W. Lyons, Rongjuan Cong and A. Willem deGroot, Analytical Chemistry, 2014, 86(17), 8649-8656. Described in Analytical Chemistry, 2014, 86(17), 8649-8656.

[0161] Molecular Weight Comonomer Distribution Index (MWCDI) and Bimodal Comonomer Distribution Index (BCDI). Each of MWCDI-1, MWCDI-2, and BCDI provides a method of quantifying the type (eg, reverse) and extent of comonomer distribution.

[0162] Calculation of MWCDI-1: Using a GPC instrument also equipped with a precision detector (University of Massachusetts, Amherst, MA), Model 2040 2-angle laser light scattering detector, using the known short chain branching (SCB) frequency (by 13The IR5 detector ratio calibration was performed with at least ten ethylene polymer standards (polyethylene homopolymers and ethylene / octene copolymers; narrow molecular weight distribution and uniform comonomer distribution) measured by C NMR method, ranging from homopolymer (0 SCB / 1000 total C) to about 50 SCB / 1000 total C, where total C = carbon in the main chain + carbon in the branches. The weight average molecular weight of each standard was 36,000 g / mol to 126,000 g / mol, as determined by the GPC-LALS (LALS = laser assisted light scattering) processing method described above. The molecular weight distribution (Mw / Mn) of each standard was 2.0 to 2.5, as determined by the GPC-LALS processing method described above. The SCB standard terpolymer properties are shown in Table A.

[0163] Table A: SCB Standards .

[0164] Wt% comonomer IR5 Area Ratio SCB / 1000Total C M Mw / Mn 23.1 0.2411 28.9 37,300 2.22 14.0 0.2152 17.5 36,000 2.19 0.0 0.1809 0.0 38,400 2.20 35.9 0.2708 44.9 42,200 2.18 5.4 0.1959 6.8 37,400 2.16 8.6 0.2043 10.8 36,800 2.20 39.2 0.2770 49.0 125,600 2.22 1.1 0.1810 1.4 107,000 2.09 14.3 0.2161 17.9 103,600 2.20 9.4 0.2031 11.8 103,200 2.26

[0165] For MWCDI, for each of the “SCB” standards, the “IR5 Area Ratio” (or “IR5 Area Response”) was calculated as the “Baseline-Subtracted Area Response of the IR5 Methyl Channel Sensor” to the “Baseline-Subtracted Area Response of the IR5 Measurement Channel Sensor”. (甲基通道面积) / IR5 (测量通道面积) ”)” (Standard filters and filter wheels as supplied by PolymerChar: Part No. IR5_FWM01 included as part of the GPC-IR instrument). A linear fit of SCB frequency to “IR5 Area Ratio” was constructed in the form of the following Equation 4B: SCB / 1000 Total C = A 0 +[A 1 ×IR5 (甲基通道面积) / IR5 (测量通道面积) ](Equation 4B), where A 0 is the "SCB / 1000 total C" intercept at the "IR5 area ratio" of zero, and A 1 It is the slope of "SCB / 1000 total C" versus "IR5 area ratio" and represents the increase of "SCB / 1000 total C" as "IR5 area ratio" changes.

[0166] For MWCDI, a "series of linear baseline-subtracted chromatogram heights" of the chromatogram produced by the "IR5 methyl channel sensor" was established as a function of the column elution volume to produce a baseline-corrected chromatogram (methyl channel). A series of "linear baseline-subtracted chromatogram heights" of the chromatogram produced by the "IR5 measurement channel" was established as a function of the column elution volume to produce a baseline-corrected chromatogram (measurement channel).

[0167] For MWCDI, the "IR5 Height Ratio" of the "Baseline Corrected Chromatogram (Methyl Channel)" to the "Baseline Corrected Chromatogram (Measurement Channel)" was calculated at each column elution volume index (each equally spaced index represents 1 data point per second at 1 ml / min elution) at both ends of the sample integration limit. The "IR5 Height Ratio" was multiplied by the factor A. 1 , and the coefficient A 0 is added to this result to yield the predicted SCB frequency for the sample. The result is converted to mole percent comonomer as shown below in Equation 5B: Mole percent comonomer = {SCB f / [SCB f +((1000-SCB f * length of the comonomer) / 2)]}*100 (Equation 5B), where "SCB f "SCB per 1000 total C", also written as "SCB / 1000 TC" in the table below, and "Comonomer Length" = 8 (for octene), = 6 (for hexene), etc.

[0168] For MWCDI, each elution volume index was converted to a molecular weight value (Mw i ). Plot "Comonomer Weight Percent (y-axis)" as Log(Mw i ) and calculate the Mw of 15,000 g / mol i With Mw of 10,000,000 g / mol i The slope between Mwi of 15,000 to 150,000 g / mol (and including the end points) is calculated using Microsoft EXCEL linear regression. This slope is defined as the molecular weighted comonomer distribution index (MWCDI = molecular weighted comonomer distribution index).

[0169] Representative determination of MWCDI: Generate the measured "SCB per 1000 total C (= SCB f )" versus the observed "IR5 area ratio", and the intercept (A 0 ) and slope (A 1 ) was determined to be A 0 = -90.246 SCB / 1000 total C; and A 1 = 499.32 SCB / 1000 total C. Determine the "IR5 height ratio" and multiply by the coefficient A 1 At each elution volume index, the coefficient A0 is added to the result to generate the predicted SCB frequency (SCB) of the embodiment f ), as mentioned above (A 0 = -90.246 SCB / 1000 total C; and A 1 =499.32 SCB / 1000 total C). SCB f Plotted as a function of polyethylene equivalent molecular weight as measured using Equation 1. SCB f Converted to "molar percent comonomer" via Equation 5B. Plot "molar percent comonomer" as a function of polyethylene equivalent molecular weight (as determined using Equation 1B). The linear fit is from Mwi of 15,000 g / mol to Mwi of 150,000 g / mol, yielding a slope of "2.27 mole % comonomer x mol / g". Therefore, MWCDI = 2.27. EXCEL linear regression was used to calculate the slope between Mwi of 15,000 to 150,000 g / mol (and including the endpoints).

[0170] MWCDI-2 was calculated as described in WO 2019246069: MWCDI-2.

[0171] Calculation of BCDI: BCDI is the ratio of MWCDI-2 and MWCDI-1 and is weighted by the difference in weight % of the comonomer content of the high molecular weight component measured at HMW-Mw and the comonomer content of the low molecular weight component measured at LMW-Mw, and the molecular weight distribution (MWD) is given by Mw / Mn and is given by the following equation:

[0172] BCDI = [|(MWCDI-2)| / (MWCDI-1)]×|ΔC6|×MWD, where ΔC6 is the difference between the comonomer measured at HMW-Mw and the comonomer measured at LMW-Mw (described in WO2019246069), given as wt% C6. As described in detail herein, the BCDI value of the bimodal catalyst prepared with MIOC is greater than that of the unmodified precatalyst. For example, the modified precatalyst herein may have a resulting BCDI value of greater than 4, greater than 5, greater than 6, or greater than 8, while the unmodified catalyst (unimodal catalyst) may have a BCDI value of less than 4.

[0173] Condition 1 is as follows: injection temperature = 80°C; reaction temperature = 90°C; ethylene = 230 psi; H 2 / C 2 =0.0068; C 6 / C 2 =0.004.

[0174] Condition 2 is as follows: injection temperature = 80°C; reaction temperature = 90°C; ethylene = 115 psi; H 2 / C 2 =0.0011; C 6 / C 2 =0.016.

[0175] Condition 3 is as follows: injection temperature = 80°C; reaction temperature = 90°C; ethylene = 230 psi; H 2 / C 2 =0.0011; C 6 / C 2 =0.016.

[0176] Table 1

[0177]

[0178]

[0179] Table 2

[0180]

[0181] Table 3

[0182]

[0183]

[0184] Each of IE1-14 demonstrates a surprising and unexpected chemical conversion of a unimodal ligand-metal precatalyst into a bimodal ligand-metal catalyst using a method that employs a modality-enhanced organic compound. That is, the modality-enhanced organic compound (e.g., acetylene) is not null or deleterious to the catalyst (e.g., acting as a catalyst poison) as would be expected based on conventional knowledge of such compounds, but rather a surprising and unexpectedly improved catalyst modality is prepared in the presence of the modality-enhanced organic compound. That is, the multimodal polymer provided by the bimodal ligand-metal catalyst of IE1-14 is formed in a single polymerization reactor (e.g., a single gas phase polymerization reactor) without the aid of any other polymerization catalyst (i.e., in the absence of any other polymerization catalyst), in contrast to other methods that rely on multiple polymerization reactors and / or multiple polymerization catalysts to provide multimodal polymers, and in contrast to other polymerization catalysts that provide polymers having a unimodal distribution (such as CE1, CE1, CE3, and CE4).

[0185] In addition, each of IE1-14 demonstrates the presence of a desired (e.g., reverse) comonomer distribution. When MWCDI>0 and / or when BCDI is greater than 4, a reverse comonomer distribution can be defined. For example, when MWCDI-1 and MWCDI-2 are both>0, the polymer has a reverse comonomer distribution. In addition, the MWCDI value and the BCDI value quantify the magnitude of the comonomer distribution. For example, comparing two polymers with MWCDI>0, the polymer with a larger MWCDI value is defined as having a larger, i.e., increased BOCD; in other words, the polymer with a larger MWCDI value has a larger (enhanced) reverse comonomer distribution. For example, as reported in Table 1, compared to the polymers prepared with Comparative Examples 1-4 (e.g., MWCDI-1 wt % and MWCDI-2 wt % of CE1 are 0.96 and 1.18, respectively), the polymers prepared with IE1-14 provide an increased BOCD (with a larger MWCDI value). Polymers having a larger MWCDI may provide improved physical properties, such as improved film performance, compared to polymers having a relatively smaller MWCDI.

Claims

1. A method for chemically converting a unimodal ligand-metal precatalyst to a bimodal ligand-metal catalyst, the method comprising combining, in any order, components consisting essentially of a first unimodal ligand-metal precatalyst, an effective amount of the activator, and an effective amount of the modality-enhanced organic compound under conditions effective for the activator and the modality-enhanced organic compound, chemically converting the first unimodal ligand-metal precatalyst to a bimodal ligand-metal catalyst, thereby preparing the bimodal ligand-metal catalyst; wherein the modality-enhanced organic compound has the formula (A 1 ) or (B 1 ): R 5 -C≡CR 6 (A 1 )、(R 5 )2C=C=C(R 6 )2(B 1 );where R 5 and R 6 Each of which is independently H or R 7 ; and each R 7 Independently (C1-C 20 )alkyl, -C(=O)-O-(unsubstituted C1-C 20 )alkyl), (C1-C 19 ) heteroalkyl or tri((C1-C 20 )alkyl)silyl, or two R 7 together to form a (C3-C8) alkylene group; provided that each R 7 lacks carbon-carbon double bonds; each (C1-C 20 ) The hydrocarbon groups are independently unsubstituted or substituted by 1 to 4 groups R S Substituted; wherein each substituent group R S independently selected from halogen, unsubstituted (C1-C5) alkyl, -C≡CH, -OH, (C1-C5) alkoxy, -C(=O)-(unsubstituted (C1-C5) alkyl), -NH2, -N(H)(unsubstituted (C1-C5) alkyl), -N(unsubstituted (C1-C5) alkyl)2, -COOH, -C(=O)-NH2, -C(=O)-N(H)(unsubstituted (C1-C5) alkyl), -C(=O)-N(unsubstituted (C1-C5) alkyl)2, -S-(unsubstituted (C1-C5) alkyl), -S(=O)2-(unsubstituted (C1-C5) alkyl), -S(=O)2-NH2, -S(=O)2-N(H)(unsubstituted (C1-C5) alkyl), -S(=O)2-N(unsubstituted (C1-C5) alkyl)2, -C(=)S-(unsubstituted (C1-C5) alkyl) and -COO(unsubstituted (C1-C5) alkyl); and Wherein the first unimodal ligand-metal precatalyst is a biphenylphenoxy-type ligand-metal precatalyst having formula (I): Wherein L is CH2CH2, CH2CH2CH2, CH2CH2CH2CH2, CH2C(R L )2CH2、CH2CH(R L )CH(R L )CH2、CH2Ge(R L )2CH2 or CH2Si(R L )2CH2, where each R L are independently unsubstituted (C1-C 20 ) alkyl; M is Zr or Hf; R 1a and R 1b Each of the above is independently F, (C1-C 20 )alkyl or Si(CH3)2(CH2) q CH3, wherein subscript q is an integer from 0 to 20; each subscript r is independently an integer from 0 to 3; R 2a and R 2b Each of R is independently H, F, Cl, (C1-C5) alkyl, or R 2a and R 2b can be bonded together to form an unsubstituted or substituted cycloalkyl group; each subscript s is independently an integer from 0 to 3; R 3a and R 3b Each of which is independently unsubstituted (C1-C 20 )alkyl or (C1-C 20 ) alkoxy; each Ar 1a and Ar 1b is independently an unsubstituted or substituted aromatic group selected from the group consisting of phenyl, substituted phenyl, biphenyl, substituted biphenyl, anthracene, substituted anthracene, carbazolyl, and substituted carbazolyl, wherein each substituent in the substituted aromatic group is independently an alkyl group; and each X is independently a monodentate group or each X is a part of a multidentate group independently selected from the group consisting of a halogen atom; ((C1-C 20 )alkyl) 3-g -(phenyl) g Si-, where the subscript g is 0, 1, 2 or 3; CH3; (C2-C 20 )alkyl-CH2; (C6-C 12 )aryl-((C0-C 10 )alkylene)-CH2; (C1-C6)alkyl-substituted (C6-C 12 )aryl; (C1-C6)alkoxy-substituted (C6-C 12 )aryl; (C1-C6)alkoxy-substituted benzyl; and (C1-C6)alkyl-substituted benzyl; or one X is 4-(C1-C 20 )alkyl-substituted 1,3-butadiene molecule, and each of the remaining X, if present, is independently the monodentate group X.

2. The method of claim 1, wherein the modally enhanced organic compound has the formula: (A 1 ): R 5 -C≡CR 6 (A 1 ) is selected from phenylacetylene; (substituted phenyl)acetylene; diphenylacetylene; substituted diphenylacetylene; cycloalkylacetylene; a compound of the formula HC≡CSi(phenyl) h ((C1-C 20 )alkyl) 3-h Acetylene, wherein the subscript h is an integer from 0 to 3; and the formula HC≡C-(CH2) m CH3 acetylene, wherein the subscript m is an integer from 1 to 15; or (B 1 )(R 5 )2C=C=C(R 6 )2(B 1 ) and is selected from cycloalkyl propadiene; alkyl propadiene; dialkyl propadiene; trialkyl propadiene; trialkylsilyl propadiene; vinylidene cycloalkanes; and alkyl esters of propadiene carboxylic acids.

3. The method of claim 1, wherein the modality-enhanced organic compound is selected from the group consisting of: cyclohexylpropadiene; phenylacetylene; and 3,4-difluorophenylacetylene.

4. The method of claim 1, wherein in the combining step, (i) the first unimodal ligand-metal precatalyst and the bimodal ligand-metal catalyst are unsupported and do not contain a support material; or (ii) the first unimodal ligand-metal precatalyst is unsupported, and the method further comprises, after the combining step, adding a support material to the bimodal ligand-metal catalyst so as to obtain a bimodal catalyst system comprising the support material and the bimodal ligand-metal catalyst.

5. The method of claim 1 comprising combining, in any order, components consisting essentially of said modally increased organic compound, said activator, and a bimodal precatalyst system consisting essentially of said first unimodal ligand-metal precatalyst, a second unimodal ligand-metal precatalyst having ligands compositionally different from said first unimodal ligand-metal precatalyst, and a support material; wherein said method produces a trimodal catalyst system consisting essentially of said bimodal ligand-metal catalyst, a second unimodal ligand-metal catalyst made from said second unimodal ligand-metal precatalyst and said activator, and said support material.

6. The process of claim 5, wherein the second unimodal ligand-metal catalyst is a metallocene-type catalyst.

7. The method of claim 1 further comprising contacting the bimodal ligand-metal catalyst with ethylene and an α-olefin in a polymerization reactor under steady-state polymerization conditions during or after the combining step to produce a poly(ethylene-co-α-olefin) copolymer having a bimodal molecular weight distribution as determined by gel permeation chromatography (GPC).

8. The method of claim 4, further comprising contacting the bimodal catalyst system with ethylene and an α-olefin in a polymerization reactor under steady state polymerization conditions during or after the combining step to produce a poly(ethylene-co-α-olefin) copolymer having a bimodal molecular weight distribution as determined by gel permeation chromatography (GPC).

9. The method of claim 5, further comprising contacting the trimodal catalyst system with ethylene and an α-olefin in a polymerization reactor under steady-state polymerization conditions during or after the combining step to produce a poly(ethylene-co-α-olefin) copolymer having a trimodal molecular weight distribution as determined by gel permeation chromatography (GPC).

10. The method according to claim 1, comprising the steps of: The polymerization process carried out in a polymerization reactor is converted from a process for preparing a unimodal poly(ethylene-co-α-olefin) copolymer to a process for preparing a bimodal or trimodal poly(ethylene-co-α-olefin) copolymer, the method further comprising, before the combining step, contacting a first unimodal ligand-metal catalyst made of the first unimodal ligand-metal precatalyst and an activator with ethylene and α-olefin in a polymerization reactor under steady-state polymerization conditions in the absence of the modality-increasing organic compound so as to prepare a poly(ethylene-co-α-olefin) copolymer having a unimodal molecular weight distribution as determined by GPC; and after the combining step, contacting the bimodal ligand-metal catalyst with the ethylene and the α-olefin in the polymerization reactor under steady-state polymerization conditions so as to prepare a poly(ethylene-co-α-olefin) copolymer having a bimodal molecular weight distribution as determined by GPC.

11. The method according to claim 4, comprising the steps of: The polymerization process carried out in a polymerization reactor is converted from a process for preparing a unimodal poly(ethylene-co-α-olefin) copolymer to a process for preparing a bimodal or trimodal poly(ethylene-co-α-olefin) copolymer, the method further comprising, before the combining step, contacting a first unimodal ligand-metal catalyst made of the first unimodal ligand-metal precatalyst and an activator with ethylene and α-olefin in a polymerization reactor under steady-state polymerization conditions in the absence of the modality-increasing organic compound so as to prepare a poly(ethylene-co-α-olefin) copolymer having a unimodal molecular weight distribution as determined by GPC; and after the combining step, contacting the bimodal catalyst system with the ethylene and the α-olefin in the polymerization reactor under steady-state polymerization conditions so as to prepare a poly(ethylene-co-α-olefin) copolymer having a bimodal molecular weight distribution as determined by GPC.

12. The method according to claim 5, comprising the steps of: The polymerization process carried out in a polymerization reactor is converted from a process for preparing a unimodal poly(ethylene-co-α-olefin) copolymer to a process for preparing a bimodal or trimodal poly(ethylene-co-α-olefin) copolymer, the method further comprising, before the combining step, contacting the first unimodal ligand-metal catalyst made of the first unimodal ligand-metal precatalyst and the activator with ethylene and α-olefin in a polymerization reactor under steady-state polymerization conditions in the absence of the modality-increasing organic compound so as to prepare a poly(ethylene-co-α-olefin) copolymer having a unimodal molecular weight distribution as determined by GPC; and after the combining step, contacting the trimodal catalyst system with the ethylene and the α-olefin in the polymerization reactor under steady-state polymerization conditions so as to prepare a poly(ethylene-co-α-olefin) copolymer having a trimodal molecular weight distribution as determined by GPC.

13. The method of claim 1, wherein each X is independently a bidentate group; and / or Each X is benzyl.

14. The method according to claim 1, wherein the biphenylphenoxy-type ligand-metal precatalyst of structural formula (I) is any one of compounds (1) to (2): (2), wherein each Me is a methyl group.

15. The method of claim 1, wherein the metal of the first unimodal ligand-metal precatalyst is M, wherein the activator is an organoaluminum compound, and wherein the effective amount of the activator is an Al / M molar ratio of 0.5 to 10,000; and / or wherein the effective amount of the modal-enhanced organic compound comprises a molar ratio of modal-enhanced organic compound to first unimodal ligand-metal precatalyst of 0.5:1.0 to 50.0:1.

0.

16. The method of claim 15, wherein the effective amount of the activator is an Al / M molar ratio of 0.95 to 200; and / or wherein the effective amount of the modality-enhanced organic compound comprises a molar ratio of modality-enhanced organic compound to first unimodal ligand-metal precatalyst of 0.9:1.0 to 20.0:1.

0.

17. The method of claim 16, wherein the effective amount of the activator is an Al / M molar ratio of 1.0 to 150; and / or wherein the effective amount of the modality-enhanced organic compound comprises a molar ratio of modality-enhanced organic compound to first unimodal ligand-metal precatalyst of 0.9:1.0 to 11:1.

0.

18. The method of claim 17, wherein the effective amount of the activator is an Al / M molar ratio of 10 to 100; and / or wherein the effective amount of the modality-enhanced organic compound comprises a molar ratio of modality-enhanced organic compound to first unimodal ligand-metal precatalyst of 0.95:1.0 to 6:1.

0.

19. A poly(ethylene-co-α-olefin) copolymer prepared by the method of any one of claims 7-9, wherein the poly(ethylene-co-α-olefin) copolymer has a BCDI greater than 4, a MWCDI>0, or both.

20. An article of manufacture made from the poly(ethylene-co-alpha-olefin) copolymer of claim 19.

21. A multimodal catalyst system comprising a bimodal ligand-metal catalyst prepared by the method according to claim 1.

Citation Information

Patent Citations

  • Finely divided aluminoxane, process for producing same and its use

    EP0279586B1

  • Disc brake actuator

    EP0649992B1

  • Circuit breaker with handle locking device

    EP0839380A1

  • Modified polyethylene compositions

    US20060173123A1

  • Closed reactor transitions between metallocene catalysts

    US20180079836A1