A kind of hydrogen barrier composite coating and preparation method thereof
By preparing micron TiN/nanoTiC composite coating on the surface of stainless steel, the problems of low density and many defects of hydrogen resistance coating in the prior art are solved, which significantly improves hydrogen resistance performance and enhances the safety of stainless steel high-pressure hydrogen storage system and performance stability.
Patent Information
- Application Number
- CN202110914621.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-08-10
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2041-08-10
AI Technical Summary
The hydrogen embrittlement problem in existing stainless steel high-pressure hydrogen storage systems leads to reduced material plasticity and accelerated fatigue cracks. The hydrogen-resistance coating has low density and many defects, and insufficient hydrogen resistance performance, making it difficult to effectively prevent hydrogen penetration.
The composite coating structure of the micron TiN outer layer and the nano-TiC inner layer is prepared by chemical vapor deposition method to enhance the density and binding force of the coating, forming a block micron TiN outer layer and a conical nano-TiC inner layer to enhance resistance Hydrogen performance.
It significantly improves hydrogen resistance, reduces the energy barrier for hydrogen atom permeability, and effectively blocks hydrogen atoms. It is suitable for use in stainless steel high-pressure hydrogen storage systems, improving the safety and performance stability of the system.
Smart Images

Figure CN115704090B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of hydrogen barrier coatings, and in particular to a hydrogen barrier composite coating and a preparation method thereof. Background Art
[0002] Hydrogen energy has the advantages of being pollution-free, widely available, high in calorific value, and renewable and cyclic. It is the safest, cleanest, and highest in calorific value hydrogen fuel in the future, and plays a very important role in the nuclear power, petroleum, chemical, energy and other industries. Therefore, the preparation, processing, storage and transportation of hydrogen are crucial to the industrial development of hydrogen energy. Stainless steel is currently the main material for hydrogen storage systems, and high-pressure hydrogen storage is the main method for various stainless steel hydrogen storage systems. However, a high-pressure hydrogen environment can easily lead to a series of hydrogen embrittlement problems such as reduced plasticity of stainless steel materials and accelerated fatigue crack propagation, which is a huge challenge facing the safety of stainless steel high-pressure hydrogen systems.
[0003] Hydrogen barrier coating is an effective way to solve the hydrogen embrittlement problem of stainless steel hydrogen storage system. By preparing hydrogen barrier coating on the surface of metal materials, hydrogen penetration into the material is prevented or delayed, thereby preventing and reducing the occurrence of hydrogen embrittlement. The following types of hydrogen barrier coatings have been developed: oxide coatings such as chromium oxide and zirconium oxide; silicide coatings such as silicon carbide and silicon nitride; titanium nitride and titanium carbide coatings; aluminide coatings such as iron-aluminum alloy. Commonly used hydrogen barrier coating preparation processes include vapor deposition, plasma spraying, embedded aluminization, sol-gel method, micro-arc oxidation, etc.
[0004] Studies have shown that the hydrogen barrier effect of a single-layer hydrogen barrier coating is very limited, and a composite coating with a hydrogen barrier layer / hydrogen storage layer composite structure has better hydrogen barrier performance. However, the hydrogen barrier performance of a composite coating with a hydrogen barrier layer / hydrogen storage layer structure is often limited by factors such as the grain size, density, number of defects of the hydrogen barrier layer and the hydrogen storage layer, and the bonding strength between the coating and the stainless steel substrate. At the same time, preparation methods such as plasma spraying, embedded aluminization, and sol-gel methods have a series of problems such as low coating density, many defects, and uneven particle size distribution, resulting in the hydrogen barrier performance of the composite coating is still limited.
[0005] Therefore, in response to the hydrogen embrittlement problem currently faced by stainless steel high-pressure hydrogen storage systems, the field urgently needs to develop a hydrogen barrier composite coating with high density, few defects, and good hydrogen barrier / hydrogen storage composite functions, so as to overcome the shortcomings of existing hydrogen barrier coatings such as low density, many defects, and weak hydrogen barrier performance, and improve the safety of stainless steel high-pressure hydrogen storage systems. Summary of the invention
[0006] In order to solve the problems existing in the prior art, the present invention provides a hydrogen barrier composite coating and a preparation method thereof, which adopts a composite coating structure design to significantly enhance the hydrogen barrier capability of the composite coating.
[0007] To achieve the above objectives, the present invention provides the following technical solutions: a hydrogen barrier composite coating, comprising a micron TiN outer layer and a nano TiC inner layer, wherein the micron TiN outer layer is composed of micron-sized blocky TiN grains, and the nano TiC inner layer is composed of nano-sized conical TiC grains.
[0008] Furthermore, the particle size of the micron-sized block TiN grains is 1 μm-3 μm; the particle size of the cone-shaped TiC grains is 40 nm-300 nm, and the thickness of the composite coating is 3-8 μm.
[0009] The present invention also provides a method for preparing a hydrogen barrier composite coating.
[0010] S1 provides a substrate;
[0011] S2 deposits TiC on the surface of the substrate by chemical vapor deposition in the presence of a carbon source and a titanium source under an auxiliary gas to obtain a nano-TiC inner layer;
[0012] S3 deposits TiN on the TiC inner layer by chemical vapor deposition in the presence of a nitrogen source and a titanium source under an auxiliary gas to obtain a micron TiN outer layer, thereby forming a hydrogen barrier composite coating.
[0013] Furthermore, in step S1, the surface roughness of the substrate is 0.05-0.2, the substrate is preheated to 1000°C-1030°C, and the heating rate is 5°C / min-8°C / min.
[0014] Furthermore, in step S2, the flow rate of the carbon source is 600-1000 sccm, and the carbon source is at least one of methane, ethane, acetylene and propylene.
[0015] Furthermore, in step S2, the temperature is raised to 1000°C-1030°C at a heating rate of 5°C / min-8°C / min for deposition, and the deposition time is 120min-540min.
[0016] Furthermore, in steps S2 and S3, the titanium source is introduced into the reaction system with an auxiliary gas as a carrier, the flow rate of the auxiliary gas is 800-1500 sccm, and the titanium source is at least one of butyl titanate, titanium tetrachloride, titanium trichloride, titanium dichloride, titanium chloride, and titanium powder.
[0017] Furthermore, in step S3, the nitrogen source flow rate is 1500-2000 sccm, and the nitrogen source is at least one of nitric oxide, nitrogen dioxide, nitrogen and ammonia.
[0018] Furthermore, in step S3, the temperature is raised to 1010-1050°C at a heating rate of 5°C / min-8°C / min for deposition, and the deposition time is 120min-540min.
[0019] Furthermore, the obtained hydrogen barrier composite coating is cooled in two stages. In the first stage, the titanium source is stopped, the nitrogen source flow rate is reduced to 500 sccm-1000 sccm, the cooling rate is 5°C / min-8°C / min, and the temperature is reduced to 700°C-750°C;
[0020] In the second stage, the nitrogen source flow rate is reduced to 200-500 sccm, and the cooling rate is 5-8°C / min. When the temperature drops to 100-200°C, the nitrogen source is stopped and cooled to room temperature.
[0021] Compared with the prior art, the present invention has at least the following beneficial effects:
[0022] The invention provides a hydrogen barrier composite coating, which contains a blocky micron TiN outer layer and a conical nano TiC inner layer or is composed of the structural coating. The micron outer layer / nano inner layer structural design of the composite coating can realize hydrogen barrier + hydrogen storage function, thereby obtaining excellent hydrogen barrier function; the outer micron TiN coating is a "hydrogen barrier layer", which has high density, few defects, and high energy barrier required for hydrogen atom diffusion and penetration, thereby effectively blocking the penetration of hydrogen atoms; the inner nano TiC coating is a "hydrogen storage layer", which has many grain boundaries and few defects, and higher energy barrier for hydrogen atom diffusion and penetration, and can capture and store a small amount of hydrogen atoms passing through the "hydrogen barrier layer".
[0023] The micron TiN / nano TiC hydrogen barrier composite coating prepared by the chemical vapor deposition method can effectively regulate the coating structure and grain size, enhance the film-base bonding force, the density of the coating and reduce defects, and improve the hydrogen barrier performance of the composite coating.
[0024] The hydrogen barrier composite coating of the present invention is prepared on a metal substrate by chemical vapor deposition, which has little effect on the dimensional accuracy of the substrate and has good adaptability to the substrate shape, and is suitable for the fields of new energy, nuclear power, hydrogen energy storage and transportation, etc. At the same time, the coating has low production cost, simple process, strong controllability, and is suitable for industrial production.
[0025] Furthermore, the present invention performs two-stage cooling on the hydrogen barrier composite coating, which can prevent the coating from cracking and reducing the coating performance due to the interface stress caused by the mismatch of thermal expansion coefficients between the coating and the substrate and the increase of internal stress in the coating, thereby ensuring the stable performance of the hydrogen barrier composite coating. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] Figure 1 Schematic diagram of the structure of the micron TiN / nano TiC hydrogen barrier composite coating prepared in Example 1 and composited on the surface of 316L stainless steel.
[0027] Figure 2This is the XRD test diagram of the micron TiN / nano TiC hydrogen barrier composite coating prepared in Example 1 and composited on the surface of 316L stainless steel.
[0028] Figure 3 This is a SEM test image of the micron TiN outer layer of the micron TiN / nano-TiC hydrogen barrier composite coating prepared in Example 1 and composited on the surface of 316L stainless steel.
[0029] Figure 4 This is a SEM test image of the nano-TiC inner layer of the micron-TiN / nano-TiC hydrogen barrier composite coating composited on the surface of 316L stainless steel prepared in Example 1.
[0030] Figure 5 This is a cross-sectional SEM test image of the micron TiN / nano-TiC hydrogen barrier composite coating prepared in Example 1 and composited on the surface of 316L stainless steel. DETAILED DESCRIPTION
[0031] The invention will be further described below in conjunction with the accompanying drawings and specific embodiments. It should be understood that these embodiments are only used to illustrate the present invention and are not intended to limit the scope of the present invention. The experimental methods in the following examples without specifying specific conditions are usually carried out under conventional conditions or under conditions recommended by the manufacturer. Unless otherwise specified, percentages and parts are calculated by weight.
[0032] the term
[0033] Unless defined otherwise, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which this invention belongs.
[0034] As used herein, the term "coating" and "micron-TiN / nano-TiC hydrogen barrier composite coating on stainless steel surface" are interchangeable.
[0035] As used herein, the terms "include", "comprises", and "comprising" are interchangeable and include not only closed definitions, but also semi-closed and open definitions. In other words, the terms include "consisting of", "consisting essentially of".
[0036] As used herein, the term "316L stainless steel" is a stainless steel material grade, the US grade is AISI 316L, the Japanese grade is sus 316L. my country's unified digital code is S31603, the standard grade is 022Cr17Ni12Mo2, the three are interchangeable, and the corresponding national standard is GB / T 20878-2007.
[0037] As used herein, the term "CVD furnace" refers to a chemical vapor deposition furnace.
[0038] As used herein, the term "micrometer" is a unit of length that refers to the grain size of a coating, where 1 micrometer = 10 -6 m.
[0039] As used herein, the term "nanometer" is a unit of length that refers to the grain size of a coating, where 1 nanometer = 10 -9 m.
[0040] As used herein, the term "carbon source" refers to a raw material that provides carbon elements in a coating.
[0041] As used herein, the term "nitrogen source" refers to a raw material that provides nitrogen in a coating.
[0042] As used herein, the term "titanium source" refers to a raw material that provides the titanium element in the coating.
[0043] As used herein, the term "sccm" is a unit of volume flow, ie, standard-state cubic centimeter per minute.
[0044] As used herein, the term "PRF" is a hydrogen permeation reduction factor, which represents the ratio of the substrate permeability to the coating permeability.
[0045] As used herein, the term "assistant gas" refers to a gas having a purity of 99.99%.
[0046] The invention provides a surface micron TiN / nano TiC hydrogen barrier composite coating, wherein the hydrogen barrier composite coating contains a blocky micron TiN outer layer and a conical nano TiC inner layer or is composed only of a blocky micron TiN outer layer and a conical nano TiC inner layer, the thickness of the hydrogen barrier composite coating is 3-8 μm, and the hydrogen permeation reduction factor PRF at 300° C. is 550-700.
[0047] The bulk micron TiN outer layer is composed of micron-sized bulk TiN grains, and the size of the micron-sized bulk TiN grains is 1-3 μm, preferably 1-1.5 μm.
[0048] The conical nano-TiC inner layer is composed of nano-scale conical TiC grains; the size of the conical TiC grains is 40-300nm, preferably 60-150nm;
[0049] Preferably, the thickness of the hydrogen barrier composite coating is 4-6 μm;
[0050] Preferably, the hydrogen permeation reduction factor PRF at 300° C. is 550-700, preferably 600-650. The lower the permeability factor value, the better the hydrogen barrier performance of the hydrogen barrier composite coating of the present invention.
[0051] The present invention also provides a method for preparing a micron TiN / nano TiC hydrogen barrier composite coating, the specific steps of which are as follows:
[0052] (1) A substrate is provided, and the surface of the substrate is cleaned, sandblasted, re-cleaned, and polished in sequence, and the surface roughness of the substrate is Ra<0.2. Preferably, Ra is between 0.05-0.2. After the surface polishing is completed, in order to prevent residual sand particles on the surface of the substrate, and then prevent spots, local shedding, pitting defects and other problems from occurring during the coating preparation process, the surface of the substrate needs to be ultrasonically cleaned, and after drying at 70-90° C. for 3-5 hours, a hydrogen + argon mixed gas of 500-800 sccm is introduced under a vacuum degree of 0.01-0.02 MPa to heat the substrate and the reaction chamber cavity, and the heating rate is 5-8° C. / min, and the heating temperature is 1000-1030° C.
[0053] (2) introducing a carbon source, a titanium source and an auxiliary gas into the reaction system, and using a chemical vapor deposition method to deposit TiC on the surface of the substrate in step (1), thereby obtaining conical nano-TiC on the surface of the substrate;
[0054] (3) introducing a nitrogen source, a titanium source and an auxiliary gas into the reaction system, and using a chemical vapor deposition method, depositing TiN on the surface of the conical nano-TiC inner layer obtained in step (2) to form a blocky micron TiN outer layer, thereby obtaining a hydrogen barrier composite coating.
[0055] (4) The hydrogen barrier composite coating is cooled in two stages. The first stage of cooling is as follows: the titanium source is stopped, the nitrogen source flow rate is reduced to 500-1000sccm, the cooling rate is 5-8°C / min, and the temperature is reduced to 700-750°C; the second stage of cooling is as follows: when the temperature is reduced to 700-750°C, the nitrogen source flow rate is reduced to 200-500sccm; when the temperature is reduced to 100-200°C, the nitrogen source is stopped, and then cooled to room temperature.
[0056] In step 1, preferably, the substrate includes at least one of carbon steel, cemented carbide, and corrosion-resistant alloy.
[0057] Preferably, the steel material is ordinary stainless steel.
[0058] More preferably, the steel material is 316L stainless steel.
[0059] Preferably, the sandblasting uses at least one of white corundum sand, brown corundum sand and quartz sand.
[0060] Preferably, the sandblasting is performed using brown corundum sand with a particle size of 300-500 meshes.
[0061] Preferably, the cleaning is carried out using at least one of a metal surface cleaning agent, alcohol, acetone, and water.
[0062] Preferably, the cleaning agent is alcohol.
[0063] Preferably, ultrasonic cleaning is used for cleaning for 20-30 minutes.
[0064] In step 2, preferably, the carbon source is at least one of methane, ethane, acetylene and propylene. Preferably, the carbon source is propylene, and the carbon source flow rate is 600-1000 sccm.
[0065] Preferably, the blocky micron TiC outer layer is heated to 1000-1030° C. at a heating rate of 5-8° C. / min for deposition, and the deposition time is 120-540 min; preferably, the deposition time is 150-450 min; more preferably, the deposition time is 180-200 min.
[0066] In step 3, preferably, the nitrogen source is at least one of nitric oxide, nitrogen dioxide, nitrogen and ammonia, and the flow rate of the nitrogen source is 1500-2000sccm; preferably, the nitrogen source is nitrogen.
[0067] Preferably, the bulk micron TiN outer layer is heated to 1010-1050°C at a heating rate of 5-8°C / min for deposition, and the deposition time is 120-540min; preferably, the deposition time is 150-450min; more preferably, the deposition time is 180-200min.
[0068] In step 2 and step 3, preferably, the titanium source is introduced into the reaction system through an auxiliary gas carrier, the flow rate of the auxiliary gas is 1000-1500sccm, and the titanium source is at least one of butyl titanate, titanium tetrachloride, titanium trichloride, titanium dichloride, titanium chloride, and titanium powder; preferably, the titanium source is titanium tetrachloride.
[0069] The auxiliary gas is at least one of argon, nitrogen, helium and hydrogen. Preferably, the auxiliary gas is hydrogen.
[0070] Example 1
[0071] Preparation of Micron TiN / Nano TiC Hydrogen Barrier Composite Coating on 316L Stainless Steel Surface
[0072] 1. Grind and remove impurities from the surface of a 316L stainless steel substrate with a size of 50mm*10mm*3mm, use white corundum sand for surface sandblasting, then polish the surface, and then use alcohol to ultrasonically clean the substrate. Then put the cleaned substrate into an oven, dry it at 75°C for 3 hours, and then place it in a CVD device.
[0073] 2. Use a two-stage vacuum pump set to evacuate the CVD device to 10 -1Pa, then hydrogen and argon are introduced simultaneously, with a hydrogen flow rate of 600 sccm and an argon flow rate of 200 sccm. The furnace heating program is started, the heating rate is set to 8°C / min, and the deposition temperature is set to 1020°C.
[0074] 3. Prepare the nano-TiC inner layer by chemical vapor deposition, including the steps of: heating the CVD device to 1020°C to enter the coating deposition program, introducing titanium tetrachloride, propylene and auxiliary gas. The propylene flow rate is 800 sccm, and the deposition time is 180 minutes, wherein titanium tetrachloride is carried into the CVD device with hydrogen as the auxiliary gas, and the hydrogen flow rate is 1200 sccm.
[0075] 4. After the deposition of the nano-TiC inner layer is completed, the micron TiN outer layer preparation stage is entered, including the steps of: heating the CVD device to 1035°C to enter the coating deposition program, and introducing titanium tetrachloride, nitrogen and auxiliary gas. The nitrogen flow rate is 1800sccm, and the deposition time is 200min. Titanium tetrachloride is carried into the CVD device with hydrogen as the auxiliary gas, and the hydrogen flow rate is 1000sccm.
[0076] 5. After the deposition is completed, the CVD device enters a controllable cooling mode, the introduction of titanium tetrachloride and titanium source is stopped, the nitrogen source flow rate is reduced to 500 sccm, the cooling rate is 5°C / min, and after cooling to 700°C, the nitrogen source flow rate is reduced to 200 sccm; when the temperature drops to 100°C, the introduction of the nitrogen source is stopped, and then cooled to room temperature to obtain a micron TiN / nano TiC hydrogen barrier composite coating composited on the surface of 316L stainless steel.
[0077] Determination
[0078] The micron TiN / nano TiC hydrogen barrier composite coating obtained in Example 1 and composited on the surface of 316L stainless steel was subjected to XRD and SEM tests. The results are as follows: Figure 2-5 shown.
[0079] Figure 1 It is a schematic diagram of the structure of the micron TiN / nano TiC hydrogen barrier composite coating on the surface of stainless steel according to the present invention. Figure 1 It shows that the micron TiN / nano TiC hydrogen barrier composite coating on the surface of stainless steel of the present invention is composed of an outer TiN hydrogen barrier layer and an inner TiC hydrogen storage layer.
[0080] Figure 2 This is the XRD test diagram of the micron TiN / nano TiC hydrogen barrier composite coating obtained in Example 1 and composited on the surface of 316L stainless steel. Figure 2It shows that the micron TiN / nano TiC hydrogen barrier composite coating obtained in Example 1 on the surface of 316L stainless steel is composed of TiN, TiC and a small amount of Fe phase, and the crystal structure is a face-centered cubic structure. The preferred orientation of grain growth of the micron TiN and nano TiC coatings is the (111) plane.
[0081] Figure 3 This is a SEM test image of the morphology of the micron TiN outer layer of the micron TiN / nano-TiC hydrogen barrier composite coating composited on the surface of 316L stainless steel obtained in Example 1. Figure 3 It shows that the micron TiN / nano TiC hydrogen barrier composite coating obtained in Example 1 on the surface of 316L stainless steel has a dense and uniform outer surface of the micron TiN layer, and the coating is composed of TiN grains with block-shaped shapes, and the block-shaped grains overlap each other. The grain size is 1-1.5μm.
[0082] Figure 4 This is a SEM test image of the nano-TiC inner layer morphology of the micron-TiN / nano-TiC hydrogen barrier composite coating composited on the surface of 316L stainless steel obtained in Example 1. Figure 4 It shows that the nano-TiC inner layer of the micron TiN / nano-TiC hydrogen barrier composite coating on the surface of 316L stainless steel obtained in Example 1 is dense and uniform on the surface, and the coating is composed of TiC grains with a conical shape, and the size of the conical grains is 60-150nm.
[0083] Figure 5 This is a cross-sectional SEM test image of the micron TiN / nano-TiC hydrogen barrier composite coating obtained in Example 1 and composited on the surface of 316L stainless steel. Figure 5 It is shown that the micron TiN / nano TiC hydrogen barrier composite coating obtained in Example 1 and composited on the surface of 316L stainless steel is tightly bonded to the substrate, and the coating thickness is 5-6 μm.
[0084] Performance Testing
[0085] Hydrogen barrier performance test
[0086] Method: A high temperature hydrogen permeation test was conducted on the micron TiN / nano TiC hydrogen barrier composite coating prepared in Example 1 and composited on the surface of 316L stainless steel.
[0087] Hydrogen permeation test method: Before the test, a leak detector is used to detect leaks on the welded samples to ensure the accuracy of the test results; a secondary vacuum pump group is used to evacuate the test pipeline, high-pressure chamber, and low-pressure chamber to ensure that the vacuum degree of the low-pressure chamber is 10 -6Pa, and the sample was degassed for 12 hours; the sample was heated to 300℃ and kept constant by resistance heating, and then filled with high-purity deuterium gas at a pressure of 100KPa. The change of deuterium ion flow permeating through the coating over time was detected by a quadrupole mass spectrometer, so that the deuterium permeability at different times could be obtained; combined with the deuterium permeability permeating through the test sample at the same temperature, the PRF value of the composite hydrogen barrier coating at different temperatures could be obtained.
[0088] result:
[0089] The PRF value of the micron TiN / nano TiC hydrogen barrier composite coating composited on the surface of 316L stainless steel prepared in Example 1 is 645.
[0090] Example 2
[0091] The method is the same as that of Example 1, except that in step 2, the deposition temperature of the outer layer TiN is 1020°C.
[0092] The results show that the surface of the outer TiN layer is dense and uniform, and the grains of the outer TiN layer show a micron-crystalline block structure; the size of the block grains is 0.8-1.2μm; the PRF value of the composite coating is 632.
[0093] Example 3
[0094] The method is the same as that of Example 1, except that in step 3, the inner layer TiC deposition temperature is 1010°C.
[0095] The results show that the inner TiC layer has a dense and uniform surface and a nanoscale cone-shaped structure, in which the size of the cone-shaped grains is 120-200nm; the PRF value of the composite coating is 630.
[0096] Example 4
[0097] The method is the same as that of Example 1, except that in step 3, the carbon source is ethane.
[0098] The results show that the inner TiC surface is dense and uniform, and the inner TiC layer shows a nanoscale cone structure, in which the size of the cone grains is 150-200nm; the PRF value of the composite coating is 625.
[0099] Example 5
[0100] The method is the same as that of Example 1, except that in step 3, the titanium source is titanium trichloride.
[0101] The results show that the composite coating is dense and uniform, the outer TiN layer has a micron-crystalline block structure, the size of the block grains is 1-1.2μm, the inner TiC coating has a nanoscale cone structure, the size of the cone grains is 200-250nm, and the PRF value of the composite coating is 622.
[0102] Comparative Examples 1-4
[0103] Preparation of TiN / TiC composite crystal coating on 316L stainless steel surface
[0104] The TiN / TiC composite crystal coatings described in Comparative Examples 1-4 were prepared in a similar manner to Example 1, except that the parameters in the coating preparation process were changed as shown in Table 2, and the grain morphology and grain size of the coatings were characterized. At the same time, the hydrogen barrier properties of the coatings were determined according to the same high-temperature hydrogen permeability performance test method as in Example 1.
[0105] Table 2 Characterization and performance test of TiN / TiC composite crystal coatings prepared in Comparative Examples 1-4 on the surface of 316L stainless steel
[0106]
[0107] Comparison of Examples 1-5 and Comparative Examples 1-4
[0108] The coatings prepared in Example 5 and Comparative Examples 1-4 were compared in terms of grain morphology, grain size and hydrogen barrier performance. It can be seen from Table 2 that the PRF value of the micron TiN / nano-TiC hydrogen barrier composite coating composited on the surface of 316L stainless steel prepared in Example 1 (such as in Example 5, the PRF value is 622) is significantly larger than the TiN / TiC composite crystal coating prepared in Comparative Examples 1-4 (such as in Comparative Example 4, the PRF value is 541); the grain size of the micron TiN layer of the micron TiN / nano-TiC hydrogen barrier composite coating composited on the surface of 316L stainless steel prepared in Example 1 (the outer layer TiN grain size in Example 2 is 0.8-1.2 μm) is significantly larger than the TiN / TiC composite crystal coating prepared in Comparative Examples 1-4 (such as in Comparative Example 2, the outer layer TiN grain size is 0.3-0.8 μm). The grain size of the nano TiC layer of the micron TiN / nano TiC hydrogen barrier composite coating composited on the surface of 316L stainless steel prepared in Example 1 (the inner TiC grain size in Example 5 is 200-250nm) is significantly smaller than the TiN / TiC composite crystal coating prepared in Comparative Examples 1-4 (such as the inner TiC grain size in Comparative Example 2 is 450-800nm). Therefore, compared with Comparative Examples 1-4, the micron TiN / nano TiC hydrogen barrier composite coating composited on the surface of 316L stainless steel prepared in Example 1 of the present invention has excellent hydrogen barrier performance.
[0109] Example 6
[0110] The method is the same as Example 1, except that: in step 1, the substrate is carbon steel with a surface roughness of 0.05, is dried at 70°C for 5 hours, the vacuum degree is 0.02MPa, the flow rate of hydrogen + argon mixed gas is 500sccm, the heating rate is 5°C / min, and the deposition temperature is 1000°C.
[0111] The results show that the composite coating is dense and uniform, the outer TiN layer has a micron-crystalline block structure, the size of the block grains is 0.9-1.2μm, the inner TiC coating has a nanoscale cone structure, the size of the cone grains is 150-220nm, and the PRF value of the composite coating is 625.
[0112] Example 7
[0113] The method is the same as Example 1, except that: in step 1, the substrate is cemented carbide with a surface roughness of 0.2, is dried at 90°C for 3 hours, the vacuum degree is 0.015MPa, the flow rate of hydrogen + argon mixed gas is 600sccm, the heating rate is 7°C / min, and the deposition temperature is 1030°C.
[0114] The results show that the composite coating is dense and uniform, the outer TiN layer has a micron-crystalline block structure, the size of the block grains is 0.9-1.1μm; the inner TiC coating has a nanoscale cone structure, the size of the cone grains is 160-230nm; the PRF value of the composite coating is 627.
[0115] Example 8
[0116] The method is the same as Example 1, except that: in step 1, the substrate is a corrosion-resistant alloy with a surface roughness of 0.1, is dried at 85°C for 4 hours, has a hydrogen + argon mixed gas flow rate of 700sccm, a heating rate of 7°C / min, and a deposition temperature of 1020°C.
[0117] The results show that the composite coating is dense and uniform, the outer TiN layer has a micron-crystalline block structure, the size of the block grains is 0.9-1.2μm, the inner TiC coating has a nanoscale cone structure, the size of the cone grains is 170-230nm, and the PRF value of the composite coating is 630.
[0118] Example 9
[0119] The method is the same as Example 1, except that: in step 2, the carbon source is a mixture of methane and ethane with a flow rate of 600 sccm, the titanium source is a mixture of butyl titanate and titanium tetrachloride, the titanium source is introduced into the reaction system through a helium belt, and the helium flow rate is 1500 sccm; the deposition time is 120 min.
[0120] The results show that the composite coating is dense and uniform, the outer TiN layer has a micron-crystalline block structure, the size of the block grains is 1.0-1.2μm, the inner TiC coating has a nanoscale cone structure, the size of the cone grains is 160-230nm, and the PRF value of the composite coating is 630.
[0121] Example 10
[0122] The method is the same as Example 1, except that in step 2, acetylene is used as the carbon source with a flow rate of 1000 sccm, titanium trichloride and titanium dichloride are used as the titanium source, the titanium source is introduced into the reaction system through a nitrogen belt, the flow rate of nitrogen is 1300 sccm, and the deposition time is 540 min.
[0123] The results show that the composite coating is dense and uniform, the outer TiN layer has a micron-crystalline block structure, the size of the block grains is 0.9-1.2μm; the inner TiC coating has a nanoscale cone structure, the size of the cone grains is 150-220nm; the PRF value of the composite coating is 629.
[0124] Embodiment 11
[0125] The method is the same as Example 1, except that: in step 2, the carbon source is a mixture of acetylene, ethane, and propylene with a flow rate of 900 sccm; the titanium source is titanium chloride, and the titanium source is introduced into the reaction system through a nitrogen belt with a nitrogen flow rate of 1300 sccm; the deposition time is 150 min.
[0126] The results show that the composite coating is dense and uniform, the outer TiN layer has a micron-crystalline block structure, the size of the block grains is 1.0-1.2μm; the inner TiC coating has a nanoscale cone structure, the size of the cone grains is 180-230nm; the PRF value of the composite coating is 628.
[0127] Example 12
[0128] The remaining values are the same as those in Example 9, except that the deposition time is 450 min.
[0129] The results show that the composite coating is dense and uniform, the outer TiN layer has a micron-crystalline block structure, the size of the block grains is 1.0-1.2μm; the inner TiC coating has a nanoscale cone structure, the size of the cone grains is 160-220nm; the PRF value of the composite coating is 627.
[0130] Embodiment 13
[0131] The remaining values are the same as those in Example 9, except that the deposition time is 200 min.
[0132] The results show that the composite coating is dense and uniform, the outer TiN layer has a micron-crystalline block structure, the size of the block grains is 1.0-1.2μm; the inner TiC coating has a nanoscale cone structure, the size of the cone grains is 160-230nm; the PRF value of the composite coating is 628.
[0133] Embodiment 14
[0134] The method is the same as Example 1, except that: in step 3, the nitrogen source is a mixed gas of nitric oxide and nitrogen dioxide, with a flow rate of 1500sccm; the titanium source is a mixture of titanium tetrachloride, titanium trichloride and titanium dichloride, and the titanium source is introduced into the reaction system through an argon belt, and the argon flow rate is 1000sccm.
[0135] The results show that the composite coating is dense and uniform, the outer TiN layer has a micron-crystalline block structure, the size of the block grains is 1.0-1.3μm; the inner TiC coating has a nanoscale cone structure, the size of the cone grains is 160-240nm; the PRF value of the composite coating is 626.
[0136] Embodiment 15
[0137] The method is the same as Example 1, except that: in step 3, the nitrogen source is ammonia with a flow rate of 2000 sccm; the titanium source is titanium powder, and the titanium source is introduced into the reaction system through helium and hydrogen belts, and the flow rate of helium and hydrogen is 1500 sccm.
[0138] The results show that the composite coating is dense and uniform, the outer TiN layer has a micron-crystalline block structure, the size of the block grains is 1.0-1.2μm; the inner TiC coating has a nanoscale cone structure, the size of the cone grains is 150-230nm; the PRF value of the composite coating is 627.
[0139] Example 16
[0140] The method is the same as Example 1, except that: in step 3, the nitrogen source is a mixture of ammonia, nitrogen and nitric oxide, with a flow rate of 1700sccm; the titanium source is a mixture of butyl titanate, titanium chloride and titanium powder, and the titanium source is introduced into the reaction system through argon and hydrogen, and the flow rate of argon and hydrogen is 1300sccm.
[0141] The results show that the composite coating is dense and uniform, the outer TiN layer has a micron-crystalline block structure, the size of the block grains is 0.9-1.2μm; the inner TiC coating has a nanoscale cone structure, the size of the cone grains is 170-240nm; the PRF value of the composite coating is 629.
[0142] Embodiment 17
[0143] The rest of the values are the same as those in Example 14, except that the deposition temperature is 1010°C and the deposition time is 120 min.
[0144] The results show that the composite coating is dense and uniform, the outer TiN layer has a micron-crystalline block structure, the size of the block grains is 0.9-1.1μm; the inner TiC coating has a nanoscale cone structure, the size of the cone grains is 160-220nm; the PRF value of the composite coating is 625.
[0145] Embodiment 18
[0146] The rest of the values are the same as those in Example 14, except that the deposition temperature is 1050°C and the deposition time is 540 min.
[0147] The results show that the composite coating is dense and uniform, the outer TiN layer has a micron-crystalline block structure, the size of the block grains is 0.9-1.2μm; the inner TiC coating has a nanoscale cone structure, the size of the cone grains is 160-230nm; the PRF value of the composite coating is 626.
[0148] Embodiment 19
[0149] The rest of the values are the same as those in Example 14, except that the deposition temperature is 1030°C and the deposition time is 150 min.
[0150] The results show that the composite coating is dense and uniform, the outer TiN layer has a micron-crystalline block structure, the size of the block grains is 0.9-1.2μm; the inner TiC coating has a nanoscale cone structure, the size of the cone grains is 150-220nm; the PRF value of the composite coating is 627.
[0151] Embodiment 20
[0152] The remaining values are the same as those in Example 14, except that the deposition temperature is 1020°C and the deposition time is 450 min.
[0153] The results show that the composite coating is dense and uniform, the outer TiN layer has a micron-crystalline block structure, the size of the block grains is 0.9-1.2μm; the inner TiC coating has a nanoscale cone structure, the size of the cone grains is 150-230nm; the PRF value of the composite coating is 628.
[0154] Embodiment 21
[0155] The rest of the values are the same as those in Example 14, except that the deposition temperature is 1040°C and the deposition time is 180 min.
[0156] The results show that the composite coating is dense and uniform, the outer TiN layer has a micron-crystalline block structure, the size of the block grains is 0.9-1.1μm; the inner TiC coating has a nanoscale cone structure, the size of the cone grains is 160-230nm; the PRF value of the composite coating is 629.
[0157] Embodiment 22
[0158] The method is the same as Example 1, except that: in step 4, the nitrogen source flow rate is reduced to 1000 sccm, the cooling rate is 8°C / min, and the temperature is reduced to 750°C; the second stage cooling is: the nitrogen source flow rate is reduced to 500 sccm, and when the temperature drops to 200°C, the nitrogen source is stopped, and then cooled to room temperature.
[0159] The results show that the composite coating is dense and uniform, the outer TiN layer has a micron-crystalline block structure, the size of the block grains is 0.9-1.3μm; the inner TiC coating has a nanoscale cone structure, the size of the cone grains is 150-230nm; the PRF value of the composite coating is 627.
[0160] Embodiment 22
[0161] The method is the same as Example 1, except that: in step 4, the nitrogen source flow rate is reduced to 1000 sccm, the cooling rate is 8°C / min, and the temperature is reduced to 750°C; the second stage cooling is: the nitrogen source flow rate is reduced to 500 sccm, and when the temperature drops to 200°C, the nitrogen source is stopped, and then cooled to room temperature.
[0162] The results show that the composite coating is dense and uniform, the outer TiN layer has a micron-crystalline block structure, the size of the block grains is 1.0-1.3μm; the inner TiC coating has a nanoscale cone structure, the size of the cone grains is 170-220nm; the PRF value of the composite coating is 628.
[0163] Embodiment 23
[0164] The method is the same as Example 1, except that: in step 4, the nitrogen source flow rate is reduced to 800 sccm, the cooling rate is 6°C / min, and the temperature is reduced to 725°C; the second stage cooling is: the nitrogen source flow rate is reduced to 300 sccm, and when the temperature drops to 150°C, the nitrogen source is stopped, and then cooled to room temperature.
[0165] The results show that the composite coating is dense and uniform, the outer TiN layer has a micron-crystalline block structure, the size of the block grains is 1.0-1.2μm; the inner TiC coating has a nanoscale cone structure, the size of the cone grains is 150-220nm; the PRF value of the composite coating is 627.
Claims
1. A hydrogen barrier composite coating, characterized in that: The composite coating comprises a micron TiN outer layer and a nano TiC inner layer, wherein the micron TiN outer layer is composed of micron-sized blocky TiN grains, and the nano TiC inner layer is composed of nano-sized conical TiC grains; The particle size of the micron-sized block TiN grains is 1µm-3µm; the particle size of the conical TiC grains is 40nm-300nm, and the thickness of the composite coating is 3µm-8µm.
2. The method for preparing a hydrogen barrier composite coating according to claim 1, characterized in that: S1 provides a substrate; S2 deposits TiC on the surface of the substrate by chemical vapor deposition in the presence of a carbon source and a titanium source under an auxiliary gas to obtain a nano-TiC inner layer; S3 deposits TiN on the TiC inner layer by chemical vapor deposition in the presence of a nitrogen source and a titanium source under an auxiliary gas to obtain a micron TiN outer layer, thereby forming a hydrogen barrier composite coating.
3. The method for preparing a hydrogen barrier composite coating according to claim 2, characterized in that: In step S1, the substrate is preheated to 1000°C-1030°C, with a heating rate of 5°C / min-8°C / min.
4. The method for preparing a hydrogen barrier composite coating according to claim 2, characterized in that: In step S2, the flow rate of the carbon source is 600 sccm-1000 sccm, and the carbon source is at least one of methane, ethane, acetylene and propylene.
5. The method for preparing a hydrogen barrier composite coating according to claim 2, characterized in that: In step S2, the temperature is raised to 1000°C-1030°C at a heating rate of 5°C / min-8°C / min for deposition, and the deposition time is 120min-540min.
6. The method for preparing a hydrogen barrier composite coating according to claim 2, characterized in that: In steps S2 and S3, the titanium source is introduced into the reaction system with an auxiliary gas as a carrier, the flow rate of the auxiliary gas is 800sccm-1500sccm, and the titanium source is at least one of butyl titanate, titanium tetrachloride, titanium trichloride, titanium dichloride, titanium chloride, and titanium powder.
7. The method for preparing a hydrogen barrier composite coating according to claim 2, characterized in that: In step S3, the nitrogen source flow rate is 1500sccm-2000sccm, and the nitrogen source is at least one of nitric oxide, nitrogen dioxide, nitrogen and ammonia.
8. The method for preparing a hydrogen barrier composite coating according to claim 2, characterized in that: In step S3, the temperature is raised to 1010°C-1050°C at a heating rate of 5°C / min-8°C / min for deposition, and the deposition time is 120min-540min.
9. The method for preparing a hydrogen barrier composite coating according to claim 2, characterized in that: The obtained hydrogen barrier composite coating is cooled in two stages. In the first stage, the titanium source is stopped, the nitrogen source flow rate is reduced to 500 sccm-1000 sccm, the cooling rate is 5°C / min-8°C / min, and the temperature is reduced to 700°C-750°C; In the second stage, the nitrogen source flow rate is reduced to 200 sccm-500 sccm, and the cooling rate is 5°C / min-8°C / min. When the temperature drops to 100°C-200°C, the nitrogen source is stopped and cooled to room temperature.
Citation Information
Cited By
Self-repairing hydrogen barrier composite coating for hydrogen storage or transportation device as well as preparation method and application of self-repairing hydrogen barrier composite coating
CN121293874A
A self-repairing hydrogen barrier composite coating for hydrogen storage or transport devices and its preparation method and application