Split-type conductive crystallizer and electroslag remelting device and method for improving molten pool distribution
Through the annular current of the split-type conductive crystallizer and the rotating flow of the liquid slag pool, the problems of increased molten pool depth and segregation in the production of large steel ingots are solved, the uniformity of molten pool temperature and composition is achieved, and the surface quality and quality of the ingots are improved. Production efficiency.
Patent Information
- Application Number
- CN202211579174.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-12-08
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2042-12-08
AI Technical Summary
In the production process of large steel ingots, traditional conductive crystallizers lead to an increase in the depth of the molten pool and aggravation of segregation, resulting in poor surface quality. In addition, the existing technology increases the complexity and cost of the conductive section, and the non-coaxial magnetic field distribution is uneven, which affects the ingot casting. quality.
A split-type conductive crystallizer is used, and two conductive rings with cooling water chambers are used to form an annular crystallizer wall. Insulating pads and conductive columns are set up to form a reverse or forward annular current, generate an axial magnetic field, and promote the melt pool composition and Temperature uniformity and reduction of droplet size and pool depth through the rotational flow of the liquid slag pool.
It improves the uniformity of molten pool temperature and composition, refines the ingot structure, reduces slag skin thickness, improves surface quality, and saves costs and equipment complexity.
Smart Images

Figure CN115710640B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of metallurgy, and in particular relates to a petal-type conductive crystallizer and an electroslag remelting device and method for improving molten pool distribution. Background Art
[0002] At present, the demand for heavy equipment is increasing, and key parts often need to be forged from large steel ingots. Therefore, how to quickly produce large steel ingots that meet quality requirements has become a common concern for metallurgical workers.
[0003] Traditional large steel ingots are generally produced by die casting. As the thickness and size of the ingot increase, the cooling and solidification speed is slower, the solidification time is longer, and the solute redistribution coefficient of the elements, the solidification speed of different parts, the flow state and the temperature distribution are very different. During the solidification process, problems such as changes in organizational morphology, component segregation, shrinkage, cracks and inclusions usually occur, which is very unfavorable for the production of high-quality large forgings. After the emergence of electroslag remelting, it has been used to prepare large steel ingots due to its advantages such as small inclusions and dense organization. However, as the size of the ingot increases, the depth of the ingot metal molten pool increases and the segregation becomes more severe. The preparation of large steel ingots by electroslag remelting in a conductive crystallizer is generally achieved by adding a conductive segment to change the electroslag remelting power supply circuit, changing the temperature field distribution of the slag pool and reducing the depth of the metal molten pool. However, because the increase in the conductive segment reduces the temperature of the lower slag pool, the slag skin is too thick, and the shallow metal molten pool is not enough to melt the slag skin, resulting in poor surface quality. The coaxial conductive ESR furnace has a complex structure and high cost; the non-coaxial ESR furnace has a simple structure, but its magnetic field distribution is uneven, which disrupts the circumferential uniformity of the ingot quality. Zhong Yunbo et al. found in their study "Study on Solidification Structure of ESR Ingots under Steady Magnetic Field" that setting a magnetic field outside the ESR furnace can make the metal molten pool move back and forth, improve segregation, and refine the structure, but setting a magnetic field outside the ESR furnace also increases the complexity of equipment and control. Summary of the invention
[0004] In order to improve the problems of uneven heat and composition generated during the production of large-size steel ingots, the present invention provides a split-type conductive crystallizer and an electroslag remelting device and method for improving the distribution of the molten pool. The provided split-type conductive crystallizer is a fixed crystallizer formed by two conductive rings with cooling water chambers to form an annular crystallizer wall, and a bottom water tank is used as the crystallizer base. An insulating pad is provided at the connection between the two conductive rings, and each conductive ring is also connected to a conductive column, and a conductive brush is sleeved on the conductive column. The current is transmitted along the annular crystallizer wall / conductive brush to the conductive brush / annular crystallizer wall, so that a reverse or forward circular current is formed in the split-type conductive crystallizer. The circular current generates an axial magnetic field in the liquid slag pool and the metal molten pool, increases the momentum source term of the molten pool and the liquid slag pool, promotes the uniformity of the molten pool composition and temperature, improves the heat distribution of the molten pool, uniformizes the chemical composition and refines the ingot structure. In the liquid slag pool, the radial current and the axial magnetic field work together to generate a rotating electromagnetic force, which promotes the rotational flow of the liquid slag pool, promotes the rapid dripping of molten droplets and reduces the size of molten droplets; the molten droplets rotate to the molten pool near the wall of the split-type conductive crystallizer rather than the core of the metal molten pool, reducing the heat brought into the core of the metal molten pool by the molten droplets. In addition, the rotational flow of the liquid slag pool will cause the high-temperature area of the liquid slag pool to be transferred from the lower slag pool of the consumable electrode to the liquid slag pool area near the wall of the split-type crystallizer, which helps to reduce the heat transferred from the liquid slag pool to the core of the metal molten pool and reduce the depth of the metal molten pool; and increase the heat transfer between the liquid slag pool and the molten pool near the split-type crystallizer, increase the temperature of the side wall of the metal molten pool, and reduce the slag skin thickness of the liquid slag pool.
[0005] The split-petal conductive crystallizer of the present invention comprises a first conductive ring and a second conductive ring, the first conductive ring and the second conductive ring form an annular crystallizer wall, and are insulated and connected to a bottom water tank to form a fixed crystallizer, an insulating pad is arranged between the first conductive ring and the second conductive ring, and a cooling water cavity is arranged inside the first conductive ring and the second conductive ring;
[0006] One end of the first conductive ring or the second conductive ring on both sides of the insulating pad is extended and connected with a corresponding conductive column, and the position where the first conductive column is set on the first conductive ring and the position where the second conductive column is set on the second conductive ring are connected end to end.
[0007] Furthermore, a line connecting the first conductive column and the second conductive column passes through the center of the petal-type conductive crystallizer.
[0008] Furthermore, the structure of the split-petal conductive crystallizer is centrally symmetrical.
[0009] Furthermore, the insulating pads are all made of high temperature resistant materials and have a thickness of 3 to 20 mm.
[0010] Furthermore, the insulating pad isolates the current on one of the conductive rings from the other conductive column and the conductive brush, thereby ensuring that the current flows in a single direction on the conductive ring.
[0011] Furthermore, the height of the conductive column is flush with the height of the annular crystallizer wall formed by the first conductive ring and the second conductive ring.
[0012] Furthermore, the bottom water tank is a conductive bottom water tank, which is insulated from the annular crystallizer wall formed by the first conductive ring and the second conductive ring, and an insulating sheet is provided between the bottom water tank and the annular crystallizer wall.
[0013] Furthermore, a cooling water chamber is provided in the bottom water tank.
[0014] The electroslag remelting device for improving the distribution of the molten pool of the present invention comprises a power supply, a petal-type conductive crystallizer, a consumable electrode, a conductive brush and a switch;
[0015] A first conductive brush is sleeved on the first conductive column of the split-type conductive crystallizer, and a second conductive brush is sleeved on the second conductive column;
[0016] One pole of the power supply is connected to the consumable electrode, and is also connected to the first conductive brush and the second conductive brush through a circuit with an S1 switch, and is also connected to the bottom water tank of the split-type conductive crystallizer through a circuit with an S4 switch;
[0017] The other pole of the power supply is connected to the first conductive brush and the second conductive brush through a circuit with an S2 switch; and is also connected to the bottom water tank through a circuit with an S3 switch.
[0018] Furthermore, the electroslag remelting device for improving the molten pool distribution is also provided with a weighing system, a conductive brush posture adjustment mechanism and a control system; the conductive brush posture adjustment mechanism is synchronously connected to the first conductive brush and the second conductive brush.
[0019] The weighing system is used to weigh the mass of the split-type conductive crystallizer. The weighing system transmits the weighed mass to the control system. The control system controls the conductive brush posture adjustment mechanism according to the weighed mass, so that the first conductive brush and the second conductive brush slide on the conductive column as the liquid slag pool level moves.
[0020] In the above device, the power source is alternating current.
[0021] In the above device, the above-mentioned S1 switch, S2 switch, S3 switch and S4 switch are large current control switches.
[0022] The electroslag remelting method for improving the distribution of the molten pool of the present invention is an electroslag remelting method for improving the temperature distribution of the molten pool, uniform chemical composition and refined solidification structure by using a petal-type conductive crystallizer. The above-mentioned device is used and the following steps are performed:
[0023] Step 1, placing a consumable electrode above the split-type conductive crystallizer, and controlling the axis of the consumable electrode to coincide with the axis of the split-type conductive crystallizer;
[0024] Step 2, pouring the molten slag that has reached the preset temperature into the split-type conductive crystallizer to form a liquid slag pool; at this time, the S1 switch, the S2 switch, the S3 switch, and the S4 switch are in the disconnected state;
[0025] In the step 2, the liquid slag pool is the molten slag that has been heated to a preset temperature after being slag-melted by a slag-melting device, and the molten slag is poured into the pool from the slag-melting device.
[0026] Step 3: Connect the power supply circuit and provide the following four power supply circuits for electroslag remelting according to different steel grades, different slag systems and different smelting requirements:
[0027] First power supply circuit: When the pouring of slag stops, the S3 switch is closed, so that the power supply, consumable electrode, liquid slag pool, metal molten pool, electroslag ingot, and bottom water tank form the first power supply circuit, which is the traditional electroslag remelting circuit;
[0028] Second power supply circuit: when the pouring of slag stops, the S1 switch and the S3 switch are closed, so that the power supply, the consumable electrode, the liquid slag pool, the conductive column, the conductive brush, the metal molten pool, the electroslag ingot, and the bottom water tank form the second power supply circuit, wherein the conductive column, the conductive brush, the liquid slag pool are connected in parallel with the consumable electrode and the liquid slag pool;
[0029] The third power supply circuit: when the pouring of slag stops, the S2 switch and the S3 switch are closed, so that the power supply, the consumable electrode, the liquid slag pool, the conductive column, the conductive brush, the molten metal pool, the electroslag ingot, and the bottom water tank form the third power supply circuit, wherein the conductive column, the conductive brush, the liquid slag pool are connected in parallel with the liquid slag pool, the molten metal pool, the electroslag ingot, and the bottom water tank;
[0030] Fourth power supply circuit: when the pouring of slag stops, the S2 switch and the S4 switch are closed, so that the power supply, the consumable electrode, the liquid slag pool, the conductive column, the conductive brush, the bottom water tank, the electroslag ingot, and the metal molten pool form the fourth power supply circuit, wherein the consumable electrode and the liquid slag pool are connected in parallel with the bottom water tank, the electroslag ingot, the metal molten pool, and the liquid slag pool;
[0031] A series or parallel circuit is provided by one of the above power supply circuits, so that the Joule heat generated by the liquid slag pool under the action of the current heats the consumable electrode to cause it to start to melt and drip;
[0032] Step 4. In the above four power supply circuits, the current passing through the conductive brush and the conductive column forms a directional current on the conductive ring. The directional current generates an axial magnetic field in the liquid slag pool, and the current transmitted through the liquid slag pool forms a radial current. The axial magnetic field interacts with the radial current of the liquid slag pool to generate a rotational electromagnetic force, which promotes the rotational motion of the liquid slag pool.
[0033] Step 5: Under the action of the electric current, the Joule heat generated by the liquid slag pool heats the consumable electrode to make it begin to melt, and the metal droplets formed by the melting of the consumable electrode pass through the liquid slag pool and sink to the bottom of the liquid slag pool, gradually accumulating to form a molten metal pool;
[0034] Step 6. As the electroslag remelting proceeds, the consumable electrode gradually descends. When the height of the consumable electrode drops to the target position, the power supply is stopped, and the consumable electrode is separated from the liquid slag pool, and the first power supply circuit, the second power supply circuit, the third power supply circuit or the fourth power supply circuit are disconnected. The solidified casting is cooled to room temperature to obtain an electroslag ingot.
[0035] In the above method, the pre-melted slag is first dried in a resistance furnace to remove moisture, then cooled to room temperature with the furnace, and then placed in a graphite crucible of a slag-melting device, at which time the bottom end of the graphite electrode is located inside the pre-melted slag; the pre-melted slag is heated by a slag-melting power supply to form molten slag, and the molten slag is heated to a preset temperature; then the molten slag is poured into a petal-type conductive crystallizer through a slag outlet.
[0036] In the above method, cooling water is circulated into the cooling water chambers of the first conductive ring and the second conductive ring in the split-type conductive crystallizer, and cooling water is circulated into the cooling water chamber of the bottom water tank.
[0037] In the above method, for the second power supply circuit, the third power supply circuit, and the fourth power supply circuit, the power distribution of the two circuits is adjusted by adjusting the up and down movement of the conductive brush, thereby adjusting the flow rate of the liquid slag pool, and the speed of the material in the liquid slag pool rotating in the circumferential direction is controlled at 0.5~120r / min.
[0038] The diameter of the electroslag ingot of the present invention is ≥60mm and the length is ≥1500mm.
[0039] In the above method, the current on the conductive brush is divided into two parts, one is the directional current formed by the crystallizer wall, which generates an axial magnetic field, and the other is the radial current formed by the liquid slag pool.
[0040] In the above method, different power supply circuits have different functions. Different steel grades and different slag systems have different smelting requirements. The present invention provides four power supply circuits corresponding to different smelting requirements. For example, some steel grades have relatively low cleanliness requirements and only need electroslag remelting to improve their structure. In this case, a traditional electroslag remelting furnace can be used, that is, the first power supply circuit is used for electroslag remelting, thereby reducing the accelerated corrosion of the conductive brush and the petal-type conductive crystallizer, saving costs; if the second power supply circuit is used, the stirring of the slag-metal interface is increased, and the reaction of the slag-metal interface is promoted; if the third power supply circuit is used, the heat distribution and composition uniformity of the slag pool are improved; if the fourth power supply circuit is used, the advantages of the second and third power supply circuits are combined, which not only improves the temperature distribution and composition uniformity of the slag pool, reduces gas and inclusions in the steel, but also accelerates the slag-metal reaction, greatly improving the dynamic environment of electroslag remelting.
[0041] Compared with the prior art, the petal-type conductive crystallizer and the electroslag remelting device and method for improving the distribution of the molten pool of the present invention have the following beneficial effects:
[0042] The liquid slag start-up method is adopted to increase the convenience of its operation. During the remelting process, the power supply circuit and the position of the conductive brush are changed to promote the flow of the liquid slag pool, promote the rapid dripping of the molten droplets and reduce the size of the molten droplets; at the same time, the temperature field of the metal molten pool is reasonably optimized to reduce the heat brought into the core of the metal molten pool by the molten droplets. In addition, the rotational flow of the liquid slag pool transfers the high-temperature area of the liquid slag pool from the lower liquid slag pool of the electrode to the liquid slag pool area near the crystallizer wall, which helps to reduce the heat transferred from the liquid slag pool to the core of the molten pool and reduce the depth of the metal molten pool, but increases the heat transfer between the liquid slag pool and the molten pool near the crystallizer, increases the temperature of the side wall of the molten pool, and then promotes the uniformity of the temperature field, improves the surface quality of the ingot, and increases the effective thermal conductivity through the rotational flow of the liquid slag pool, increases the cooling rate, reduces segregation, breaks up dendrites to provide nucleation particles, and refines the structure. BRIEF DESCRIPTION OF THE DRAWINGS
[0043] Figure 1 A schematic diagram of the main structure of an electroslag remelting device with a split-type conductive crystallizer to improve the distribution of the molten pool according to an embodiment of the present invention;
[0044] Figure 2 It is a schematic diagram of the top view of the structure of an electroslag remelting device with a split-type conductive crystallizer to improve the molten pool distribution according to an embodiment of the present invention.
[0045] Figure 3 In the electroslag remelting device and method for improving the molten pool distribution with a split-type conductive crystallizer according to the embodiment of the present invention, the forward magnetic field distribution and magnetic field conditions.
[0046] Figure 4In the electroslag remelting device and method for improving the molten pool distribution with a split-type conductive crystallizer according to the embodiment of the present invention, the reverse magnetic field distribution and magnetic field conditions.
[0047] In the above figure: 1-consumable electrode; 2-liquid slag pool; 3-conductive brush; 4-metal molten pool; 5-split conductive crystallizer; 6-electroslag ingot; 7-power supply; 8-S1 switch; 9-S2 switch; 10-S3 switch; 11-S4 switch;
[0048] 501-first conductive ring; 502-second conductive ring; 503-first conductive column; 504-second conductive column; 505-bottom water tank; 506-insulating pad; 507-cooling water chamber;
[0049] a-first short net; b-second short net; c-third short net; d-fourth short net; e-fifth short net; f-sixth short net. DETAILED DESCRIPTION
[0050] The present invention is further described in detail below in conjunction with embodiments.
[0051] In the embodiment of the present invention, the axis of the consumable electrode coincides with the axis of the split-type conductive crystallizer.
[0052] In the embodiment of the present invention, the height of the liquid slag pool in the split-type conductive crystallizer is 60-80 mm.
[0053] The consumable electrode used in the embodiment of the present invention is made of G 20 Cr2Ni4A.
[0054] The high temperature resistant material of the insulating pad in the embodiment of the present invention is asbestos.
[0055] In the embodiment of the present invention, the high temperature resistant material of the insulating sheet is asbestos.
[0056] In the embodiment of the present invention, the inner diameter of the split-petal conductive crystallizer is 300 mm.
[0057] The diameter of the consumable electrode in the embodiment of the present invention is 200 mm.
[0058] In the embodiment of the present invention, the speed of the material in the liquid slag pool rotating along the circumferential direction is controlled at 0.5-120 r / min.
[0059] In the embodiment of the present invention, the length of the consumable electrode is 2200 mm.
[0060] The slag in the embodiment of the present invention contains components in mass percentage of CaF2 55-70%, CaO 0-25%, Al2O3 25-30%, and MgO 0-5%, and the sum of the total components is equal to 100%.
[0061] In the embodiment of the present invention, the melting rate of the consumable electrode is 220-400 kg / h.
[0062] Example 1
[0063] The main structure of the electroslag remelting device with a split-type conductive crystallizer to improve the distribution of the molten pool is as follows Figure 1 As shown, it includes: a power supply 7, a petal-type conductive crystallizer 5, and a conductive brush 3; wherein the petal-type conductive crystallizer 5 includes a first conductive ring 501, a second conductive ring 502, a bottom water tank 505, an insulating pad 506, a first conductive column 503 and a second conductive column 504, the first conductive ring 501 and the second conductive ring 502 form an annular crystallizer wall, a cooling water cavity 507 is provided inside the first conductive ring 501 and the second conductive ring 502, the first conductive ring 501 and the second conductive ring 502 are separated by an insulating pad 506, and a first conductive column 503 and a second conductive column 504 are respectively provided on the same side of the first conductive ring 501 and the second conductive ring 502 to form an end-to-end connection, and its top view is shown in FIG. Figure 2 .
[0064] The electroslag remelting device for improving the distribution of the molten pool includes two conductive brushes 3 which are respectively sleeved on the first conductive column 503 and the second conductive column 504;
[0065] The conductive brush 3 is connected to the first short net a, and the first short net a is connected to the second short net b and the third short net c through the S1 switch 8 and the S2 switch 9 respectively. One end of the second short net b is connected to one pole of the power supply 7, and one end of the third short net c is connected to the other pole of the power supply 7. The third short net c is connected to the fifth short net e through the S3 switch 10, and the other end of the fifth short net e is connected to the conductor of the bottom water tank 505. One end of the sixth short net f is connected to the consumable electrode 1, and the other end is short-circuited with the second short net and the fourth short net d. The fourth short net is connected to the fifth short net e through the S4 switch 11. The second short net b, the third short net c and the fourth short net d are all provided with a large current switch; the first short net a is provided with an S1 switch 8, the second short net b is provided with an S2 switch 9, the third short net c is provided with an S3 switch 10, and the fourth short net d is provided with an S4 switch 11. A cooling water cavity is provided inside the conductive ring.
[0066] The electroslag remelting method of the split-type conductive crystallizer to improve the temperature distribution of the molten pool, uniform chemical composition and refine the solidification structure is:
[0067] (1) The consumable electrode 1 is mounted on the top of the split-type conductive crystal mold 5, and the axis of the consumable electrode 1 coincides with the axis of the split-type conductive crystal mold 5;
[0068] (2) Cooling water is introduced into the cooling water chambers inside the first conductive ring 501 and the second conductive ring 502, and circulated for heat exchange; cooling water is introduced into the cooling water chamber inside the bottom water tank 505, and circulated for heat exchange;
[0069] The molten slag having reached a preset temperature is poured into the split-type conductive crystallizer 5 to form a liquid slag pool 2; the molten slag is slag heated to a preset temperature after being slag-melted by a slag-melting device, and the molten slag is poured from the slag-melting device; at this time, the S1 switch 8, the S2 switch 9, the S3 switch 10, and the S4 switch 11 are in the disconnected state;
[0070] (3) Switch S3 is closed, so that the power supply, consumable electrode, liquid slag pool, metal molten pool, electroslag ingot, and bottom water tank form a first power supply circuit. The Joule heat generated by the liquid slag pool under the action of the current heats the consumable electrode to cause it to begin to melt;
[0071] (4) The metal droplets formed by the melting of the consumable electrode 1 sink to the bottom of the liquid slag pool 2 and gradually accumulate to form a molten metal pool 4; the molten metal pool 4 is solidified by the cooling effect of the bottom water tank 505, the first conductive ring 501, and the second conductive ring 502 to form an electroslag ingot 6;
[0072] When the consumable electrode 1 melts to the target position, the consumable electrode 1 is lifted up by the lifting device to separate from the liquid slag pool 2, the power supply circuit is disconnected, and the electroslag ingot 6 is cooled to room temperature to obtain a steel ingot.
[0073] The wiring method of this embodiment can reduce the accelerated corrosion of the conductive brush and the conductive crystallizer, thereby saving costs.
[0074] Example 2
[0075] The device structure is the same as that of Example 1;
[0076] The method is the same as in Example 1, except that:
[0077] (1) When the liquid level of the liquid slag pool 2 reaches a preset position, the pouring of molten slag is stopped, and the S1 switch 8 and the S3 switch 10 are closed, so that the power supply, the consumable electrode, the liquid slag pool, the conductive column, the conductive brush, the metal molten pool, the electroslag ingot, and the bottom water tank form a second power supply circuit, wherein the conductive column, the conductive brush, the liquid slag pool, the consumable electrode, and the liquid slag pool are connected in parallel; the Joule heat generated by the liquid slag pool 2 under the action of the current heats the consumable electrode 1 to cause it to begin to melt;
[0078] The metal droplets formed by the melting of the consumable electrode 1 sink to the bottom of the liquid slag pool 2 and gradually accumulate to form a molten metal pool 4; the molten metal pool 4 is solidified by the cooling effect of the bottom water tank 505, the first conductive ring 501, and the second conductive ring 502 to form an electroslag ingot 6;
[0079] The weighing system is used to weigh the mass of the split-type conductive crystallizer. The weighing system transmits the weighed mass to the control system. The control system controls the conductive brush posture adjustment mechanism according to the weighed mass, so that the first conductive brush and the second conductive brush slide on the conductive column as the liquid slag pool moves. The melting speed of the consumable electrode 1 and the liquid level of the metal molten pool 4 are controlled by controlling the movement of the conductive brush 3;
[0080] When the consumable electrode 1 melts to the target position, the consumable electrode 1 is lifted up by the lifting device to separate from the liquid slag pool 2, the power supply circuit is disconnected, and the electroslag ingot 6 is cooled to room temperature to obtain a steel ingot;
[0081] In the above process, the ratio of the current passing through the consumable electrode 1 and the conductive brush 3 is 4 times; the current flowing into the consumable electrode is 4000A, the current passing through each conductive brush is 1000A, and the total current passing through the bottom water tank 505 is 6000A;
[0082] The melting rate of the consumable electrode is 220kg / h. The prepared ingot has good internal solidification quality without defects such as looseness and shrinkage. The degree of element segregation is greatly reduced compared with Example 1. There is no slag inclusion and wrinkles on the surface of the ingot, and the surface quality is very excellent. In the subsequent processing, the cutting amount is greatly reduced, which greatly improves the yield rate. The wiring method of this embodiment increases the stirring of the slag-metal interface and promotes the reaction of the slag-metal interface.
[0083] Example 3
[0084] The device structure is the same as that of Example 1;
[0085] The method is the same as in Example 1, except that:
[0086] (1) When the pouring of slag is stopped, the S2 switch and the S3 switch are closed, so that the power supply, the consumable electrode, the liquid slag pool, the conductive column, the conductive brush, the molten metal pool, the electroslag ingot, and the bottom water tank form a third power supply circuit, wherein the conductive column, the conductive brush, the liquid slag pool are connected in parallel with the liquid slag pool, the molten metal pool, the electroslag ingot, and the bottom water tank;
[0087] (2) When the consumable electrode stops descending, disconnect the third power supply circuit;
[0088] (3) Adjust the conductive brush to the appropriate position, the current ratio of the conductive brush to the bottom water tank is 2.5 times; the total current flowing into the consumable electrode is 6000A, the current passing through the bottom water tank is 1000A, and the current passing through the conductive brush is 2500A; the melting rate of the consumable electrode is 350kg / h;
[0089] And because of the alternating current supply of the power supply, the current passes through the conductive brushes and conductive columns from the crystallizer wall to form a reverse circular current ( Figure 4), and the longitudinal current formed by the current passing through the bottom water tank, the electroslag ingot and the molten metal pool and the liquid slag pool interacts with each other to generate a rotating electromagnetic force, which promotes the rotation of the liquid slag pool.
[0090] Similarly, when the positive circular current ( Figure 3 ), and the longitudinal current formed by the current passing through the consumable electrode liquid slag pool interacts with each other, generating a rotating electromagnetic force in the slag pool, which promotes the rotation of the liquid slag pool.
[0091] The prepared ingot has good internal solidification quality without defects such as looseness and shrinkage. Although the melting speed of the consumable electrode is increased, the degree of element segregation is still greatly reduced compared with Example 1, and there is no slag inclusion or wrinkles on the surface of the ingot, and the surface quality is very excellent. In the subsequent processing, the cutting amount is greatly reduced, which greatly improves the yield rate. The wiring of this embodiment improves the heat distribution and composition uniformity of the liquid slag pool.
[0092] Example 4
[0093] The device structure is the same as that of Example 1;
[0094] The method is the same as in Example 1, except that:
[0095] (1) When the pouring of slag is stopped, the S2 switch and the S4 switch are closed, so that the power supply, the consumable electrode, the liquid slag, the conductive column, the conductive brush, the bottom water tank, the electroslag ingot, and the molten metal pool form a fourth power supply circuit, wherein the consumable electrode, the liquid slag pool, the bottom water tank, the electroslag ingot, the molten metal pool, and the liquid slag pool are connected in parallel;
[0096] (2) When the consumable electrode stops descending, disconnect the fourth power supply circuit;
[0097] (3) Adjust the conductive brush to the appropriate position, the current ratio of the consumable electrode to the bottom water tank is 2 times; the current flowing into the conductive brush is 3000A, the current passing through the bottom water tank is 2000A, and the current passing through the consumable electrode is 4000A; the melting rate of the consumable electrode is 220kg / h;
[0098] The prepared ingot has good internal solidification quality without defects such as looseness and shrinkage. Although the melting rate of the consumable electrode is slowed down, the degree of element segregation is still greatly reduced compared with Example 1, and there is no slag inclusion or wrinkle on the surface of the ingot, and the surface quality is very excellent. In the subsequent processing process, the cutting amount is greatly reduced, which greatly improves the yield rate.
[0099] This embodiment combines the advantages of Embodiments 2 and 3, improves the temperature distribution and composition uniformity of the liquid slag pool, reduces gas and inclusions in the steel, accelerates the slag-metal reaction, and greatly improves the dynamic environment of electroslag remelting.
Claims
1. An electroslag remelting device for improving molten pool distribution, characterized in that: It includes a power supply, a split-type conductive crystallizer, a consumable electrode, a conductive brush and a switch; The split-type crystallizer comprises a first conductive ring and a second conductive ring, the first conductive ring and the second conductive ring form a crystallizer wall, and are insulated and connected to the bottom water tank to form a fixed crystallizer, an insulating pad is arranged between the first conductive ring and the second conductive ring, and cooling water chambers are arranged inside the first conductive ring and the second conductive ring; One end of the first conductive ring or the second conductive ring on both sides of the insulating pad is extended and connected with a corresponding conductive column; A first conductive brush is sleeved on the first conductive column of the split-type conductive crystallizer, and a second conductive brush is sleeved on the second conductive column; One pole of the power supply is connected to the consumable electrode, and is also connected to the first conductive brush and the second conductive brush through a circuit with an S1 switch, and is also connected to the bottom water tank of the split-type conductive crystallizer through a circuit with an S4 switch; The other pole of the power supply is connected to the first conductive brush and the second conductive brush through a circuit with an S2 switch; and is also connected to the bottom water tank through a circuit with an S3 switch; The insulation pads are all made of high temperature resistant materials, with a thickness of 3 to 20 mm; The insulating pad isolates the current on one of the conductive rings from the other conductive column and the conductive brush, thereby ensuring that the current flows in a single direction on the conductive ring.
2. The electroslag remelting device for improving molten pool distribution according to claim 1, characterized in that: The structure of the split-petal conductive crystallizer is centrally symmetrical; the position where the first conductive column is arranged in the first conductive ring and the position where the second conductive column is arranged in the second conductive ring are connected end to end.
3. The electroslag remelting device for improving molten pool distribution according to claim 1, characterized in that: The height of the conductive column is flush with the height of the annular crystallizer wall formed by the first conductive ring and the second conductive ring.
4. The electroslag remelting device for improving molten pool distribution according to claim 1, characterized in that: The bottom water tank is a conductive bottom water tank, which is insulated from the annular crystallizer wall formed by the first conductive ring and the second conductive ring, and an insulating sheet is arranged between the bottom water tank and the annular crystallizer wall; a cooling water cavity is arranged in the bottom water tank.
5. An electroslag remelting method for improving molten pool distribution, characterized in that: Using the device described in claim 1, the following steps are performed: Step 1, placing a consumable electrode above the split-type conductive crystallizer, and controlling the axis of the consumable electrode to coincide with the axis of the split-type conductive crystallizer; Step 2, pouring the molten slag that has reached the preset temperature into the split-type conductive crystallizer to form a liquid slag pool; at this time, the S1 switch, the S2 switch, the S3 switch, and the S4 switch are in the disconnected state; Step 3: Connect the power supply circuit and provide the following four power supply circuits for electroslag remelting according to different steel grades, different slag systems and different smelting requirements: First power supply circuit: When the pouring of slag stops, the S3 switch is closed, so that the power supply, consumable electrode, liquid slag pool, metal molten pool, electroslag ingot, and bottom water tank form the first power supply circuit, which is the traditional electroslag remelting circuit; Second power supply circuit: when the pouring of slag stops, the S1 switch and the S3 switch are closed, so that the power supply, the consumable electrode, the liquid slag pool, the conductive column, the conductive brush, the metal molten pool, the electroslag ingot, and the bottom water tank form the second power supply circuit, wherein the conductive column, the conductive brush, the liquid slag pool are connected in parallel with the consumable electrode and the liquid slag pool; The third power supply circuit: when the pouring of slag stops, the S2 switch and the S3 switch are closed, so that the power supply, the consumable electrode, the liquid slag pool, the conductive column, the conductive brush, the molten metal pool, the electroslag ingot, and the bottom water tank form the third power supply circuit, wherein the conductive column, the conductive brush, the liquid slag pool are connected in parallel with the liquid slag pool, the molten metal pool, the electroslag ingot, and the bottom water tank; Fourth power supply circuit: when the pouring of slag stops, the S2 switch and the S4 switch are closed, so that the power supply, the consumable electrode, the liquid slag pool, the conductive column, the conductive brush, the bottom water tank, the electroslag ingot, and the metal molten pool form the fourth power supply circuit, wherein the consumable electrode and the liquid slag pool are connected in parallel with the bottom water tank, the electroslag ingot, the metal molten pool, and the liquid slag pool; Step 4: In the above four power supply circuits, the current passing through the conductive brush and the conductive column forms a directional current on the conductive ring, and the directional current generates an axial magnetic field in the liquid slag pool, while the current transmitted through the liquid slag pool forms a radial current. The axial magnetic field interacts with the radial current of the liquid slag pool to generate a rotating electromagnetic force, which promotes the rotation of the liquid slag pool; Step 5: Under the action of the electric current, the Joule heat generated by the liquid slag pool heats the consumable electrode to make it begin to melt, and the metal droplets formed by the melting of the consumable electrode pass through the liquid slag pool and sink to the bottom of the liquid slag pool, gradually accumulating to form a molten metal pool; Step 6. As the electroslag remelting proceeds, the consumable electrode gradually descends. When the height of the consumable electrode drops to the target position, the power supply is stopped, and the consumable electrode is separated from the liquid slag pool, and the first power supply circuit, the second power supply circuit, the third power supply circuit or the fourth power supply circuit are disconnected. The solidified casting is cooled to room temperature to obtain an electroslag ingot.
6. The electroslag remelting method for improving molten pool distribution according to claim 5, characterized in that: In the step 2, the pre-melted slag is first dried in a resistance furnace to remove moisture, then cooled to room temperature with the furnace, and then placed in a graphite crucible of a slag-melting device, at which time the bottom end of the graphite electrode is located inside the pre-melted slag; the pre-melted slag is heated by a slag-melting power supply to form molten slag, and the molten slag is heated to a preset temperature; then the molten slag is poured into a petal-type conductive crystallizer through a slag outlet.
7. The electroslag remelting method for improving molten pool distribution according to claim 5, characterized in that: For the second power supply circuit, the third power supply circuit and the fourth power supply circuit, the power distribution of the two circuits is adjusted by adjusting the up and down movement of the conductive brush, thereby adjusting the flow rate of the liquid slag pool. The speed of the material in the liquid slag pool rotating in the circumferential direction is controlled at 0.5~120r / min.
Citation Information
Patent Citations
Electroslag remelting furnace current control device and using method thereof
CN112650341A
Device for preparing composite steel ingot plate blank by electroslag remelting method
CN114606391A
Device and method for preparing composite steel ingot based on conductive crystallizer
CN114854994A
Conduct electricity, continuous casting type electroslag refining furnace of new type crystallizer
CN201296773Y
Electroslag remelting method, and device for its implementation
RU2497959C1