A method for characterizing metal composites in solar cells using PL

Through the PL characterization method, the graphical screen samples and brightness measurements with different metallization ratios are used to solve the problems of large deviations and complex operations in the metal composite test of solar cells, and the precise characterization and rapid testing of the metal composite size are achieved, which significantly improves the Test accuracy and efficiency.

CN115728273BActive Publication Date: 2024-11-15DONGFANG HUANSHENG PHOTOVOLTAIC (JIANGSU) CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202111012952.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-08-31
Publication Date
2024-11-15
Estimated Expiration
2041-08-31

AI Technical Summary

Technical Problem

The existing solar cell metal composite testing methods have large deviation values, complex operation and long testing time, resulting in a slow slurry research and development process.

Method used

By using the PL characterization method, by making graphic screen samples with different metallization ratios, performing sintering processing and brightness measurement, virtual voltage and dark saturation current density are calculated, and dark saturation current in metallized and non-metalized areas are derived. Density, achieves accurate characterization of metal composite size.

Benefits of technology

It improves the test accuracy and can accurately characterize metal composites below 100fA/cm2, simplifies the operation process and significantly shortens the test time.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_3
    Figure SMS_3
  • Figure SMS_6
    Figure SMS_6
Patent Text Reader

Abstract

The present invention provides a method for characterizing solar cell metal composites using PL, including: making a sample substrate and installing a graphic screen with different metallization ratios; printing a corresponding target slurry on a target test surface of the substrate according to different graphic screens to obtain a test sample; testing the ivoc of the unmetallized test sample to obtain a C value; obtaining the ivoc of the test sample with different metallization ratios according to the C value and the measured brightness value of the test sample with different metallization ratios, and then calculating the J0_total of the different metallization ratios according to the obtained ivoc; performing linear fitting according to different metallization ratios and the corresponding J0_total to obtain the dark saturation current density of the metallized region and the dark saturation current density of the non-metallized region. The beneficial effect of the present invention is to accurately test the composite size of the metallized portion of the solar cell surface, and can accurately characterize 100fA / cm 2 The following metal composites also have the advantage of being easier and more convenient to operate.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of solar cells, and in particular relates to a method for characterizing metal composites of solar cells by using PL. Background Art

[0002] With the development of solar cell technology and testing equipment, more and more precise requirements are put forward for the characterization methods of basic parameters of solar cells. Metal recombination is a parameter that characterizes the size of the metallization conductive paste on the surface of the cell during the production process of solar cells. The size of the metal recombination has a great influence on the cell opening voltage. With the development of technology, the current p+ recombination has been reduced to 400fA / cm 2 Below, especially n+ has been reduced to 100fA / cm 2 Below, in the original test method using sunsvoc, the opposite sides of different metallization patterns are mesh metal structures. For example, to test the n+ J0_metal, a p+ metallization mesh structure is required, which results in 600fA / cm on the p+ side. 2 The grids on the left and right are much higher than the n+ test target value to be tested, resulting in a large deviation. The fitting value is generally below 10%, and the general operation is more complicated and the test time is long, which leads to a slow process of related research and development of the slurry. Summary of the invention

[0003] The problem to be solved by the present invention is to provide a method for characterizing solar cell metal composites using PL, which effectively solves the problems in the prior art test methods, such as large deviation values, generally complex operations, and long test times, which lead to slow research and development processes related to slurries.

[0004] In order to solve the above technical problems, the technical solution adopted by the present invention is: a method for characterizing metal composites of solar cells using PL, comprising:

[0005] Make sample substrates and install graphic screens with different metallization ratios;

[0006] Screen printing a corresponding target slurry on the target test surface of the substrate according to different patterns to obtain different metallization patterns, and then sintering the patterns to obtain test samples;

[0007] Test the ivoc of the unmetallized test sample, and then calculate the value of C according to the measured brightness value; calculate the ivoc of the test sample with different metallization ratios according to the value of C and the measured brightness value of the test sample with different metallization ratios, and then calculate the J0_total of different metallization ratios according to the obtained ivoc;

[0008] Linear fitting is performed according to different metallization ratios and the corresponding J0_total to obtain the dark saturation current density of the metallization area and the dark saturation current density of the non-metallization area.

[0009] Preferably, in the step of obtaining the value of C according to the brightness values ​​of different metallization ratios, according to the formula

[0010]

[0011] Where C is the relationship constant; is the brightness; ivoc is the virtual voltage; V t is the voltage constant.

[0012] Preferably, in the step of calculating J0_total of different metallization ratios according to the obtained ivoc of different metallization ratios, according to the formula

[0013] j gen =q(1-R)j γ

[0014] j rec =J0_total×exp(ivoc / V t )

[0015] j gen =j tec

[0016] Among them, j gen Generates current for the battery; rec is the recombination current of the battery; q is a constant; R is the reflectivity; j γ is the luminous flux; J0_total is the dark saturation current density; ivoc is the virtual voltage; V t is the voltage constant.

[0017] Preferably, in the step of performing linear fitting according to different metallization ratios and the corresponding J0_total, the metallization ratio is used as the abscissa and the corresponding J0_total is used as the ordinate to perform linear fitting, according to the formula

[0018] J0_metal=a+1\2*b

[0019] J0_pass=1\2*b

[0020] Where a is the slope of the fitted straight line; b is the intercept of the straight line; J0_metal is the dark saturation current density of the metallized area; J0_pass is the dark saturation current density of the non-metallized area.

[0021] Preferably, the metallization pattern is a metallization grid line pattern.

[0022] Preferably, the width of the basic gate line is 20-50 μm.

[0023] Preferably, the mesh number of the graphic screen is 380-520 meshes.

[0024] Preferably, a PL testing device is used to measure the brightness of the test sample, and during the test, the metallization pattern faces the opposite direction to the PL testing device.

[0025] Preferably, the sintering temperature for the sintering process is determined according to the target test surface of the substrate and the target slurry.

[0026] Using the above technical solution, in order to accurately test the composite size of the metallized part of the solar cell surface, a method was developed to calculate the corresponding ivoc using the different brightness of photoluminescence under different metallization ratios, and then derive the total surface composite J0_total and the J0_metal of the metallized part. Compared with the Sunsvoc method for testing the metal composite of solar cells, the PL test method has high accuracy and can accurately characterize 100fA / cm 2 The following metal composites also have the advantage of being easier and more convenient to operate. DETAILED DESCRIPTION

[0027] The present invention will be further described below in conjunction with embodiments:

[0028] In the description of the embodiments of the present invention, it should be understood that the terms "top", "bottom", etc., indicating orientations or positional relationships, are only for the convenience of describing the present invention and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore should not be understood as a limitation on the present invention.

[0029] A method for characterizing solar cell metal composites using PL, comprising:

[0030] S1: Make a substrate with a PN junction, which can be a PNP, NNN, NPN, PPP symmetrical structure, or a PNN, PN, NPP and other battery structures; and install a graphic screen with different metallization ratios, the metallization ratio can be set to 0, 3%, 6%, 10%, 13%, 16%, 20% and other proportions, so as to obtain J0_total with different metal ratios of the same slurry or different slurries; a graphic screen can have only one graphic with a metallization ratio, or it can have several graphics with different metallization ratios, and it is designed according to the needs and the size of the graphic screen. The graphic screen is generally set to 9-grid, 4-grid or 16-grid designs, in which the basic graphic is a square area with several metallized grid lines inside the square, and the mesh number of the graphic screen is generally 380-520 meshes; the width of the metallized grid lines is generally 20-50μm,

[0031] S2: Printing the corresponding target slurry on the target test surface of the substrate according to different patterns to obtain different metallization patterns, and then sintering to obtain test samples; wherein the metallization pattern is a number of metallization grid line patterns printed on the substrate by the corresponding target slurry through the pattern screen, and the number of metallization grid lines can be linearly increased according to different metallization ratios, or designed according to specific parameters, generally between 0-20%.

[0032] The sintering temperature for performing the sintering process is determined according to the target test surface of the substrate and the target slurry.

[0033] S3: Test the ivoc of the unmetallized test sample, and then calculate the C value based on the measured brightness value; the unmetallized test sample means that there is no metallized pattern on the target test surface of the substrate, that is, there is no metallized grid line. The ivoc value measured by the sintion module in the PL test equipment or WCT120 is the accurate value, and the formula is used to calculate the C value.

[0034]

[0035] C is the relationship constant; is the brightness; ivoc is the virtual voltage; V t is the voltage constant;

[0036] Substitute the IVOC value of the unmetallized test sample obtained from the test into the above formula: is the brightness measured by the PL test equipment. Substituting it into the above formula, V t is a known voltage constant, which is also substituted into the above formula to finally obtain the relationship constant C.

[0037] During the testing process of the PL test equipment, the metallized graphic part, namely the metallized gate line, is oriented in the opposite direction to the PL test equipment. The exposure time selected by the PL test equipment is 0.01S, and the condition is 1sun.

[0038] S4: The ivoc of the test samples with different metallization ratios is obtained by the value of C and the measured brightness of the test samples with different metallization ratios, and then the J0_total of the different metallization ratios is calculated according to the obtained ivoc of the different metallization ratios and the measured brightness of the test samples with different metallization ratios; wherein, the ivoc value of the test samples with different metallization ratios is measured by the sintion module in the PL test equipment or WCT120. The ivoc value obtained by the metallized test sample is inaccurate and needs to be calculated by the formula

[0039]

[0040] After S3 obtains the relationship constant C, substitute the relationship constant C into the formula, and then use the brightness of different metallization ratios obtained by the PL test equipment to calculate the brightness of different metallization ratios. Substituting into the formula, V t is a known voltage constant, which is also substituted into the above formula to finally obtain the calculated ivoc value. This ivoc value is an accurate value. Substitute this accurate value into the formula for calculating J0_total to calculate the dark saturation current density.

[0041] By formula

[0042] j geg =q(1-R)j γ

[0043] j rec =J0_total×exp(ivoc / V t )

[0044] j gen =j rec

[0045] j gen Generates current for the battery; rec is the recombination current of the battery; q is a constant; R is the reflectivity; j γ is the luminous flux; J0_total is the dark saturation current density; ivoc is the virtual voltage; V t is the voltage constant;

[0046] Calculate the value of J0_total. In equilibrium, j gen With j rec equal, that is, the current generated by the battery is the same as the composite current, and the equation q(1-R)j can be obtained γ =J0_total×exp(ivoc / V t ), q is a constant, substituted into the equation, R is the reflectivity, which can be obtained through PL testing equipment and is also substituted into the formula, j γ is the luminous flux, which is a known quantity. Substitute it into the equation, and the part on the left is the known quantity. ivoc uses the exact value calculated in the above steps and substitutes it into the equation. V t is the voltage constant, which is also a known quantity. Substituting it into the above equation, the only unknown quantity in the equation is J0_total. The J0_total value of different metallization ratios can be calculated through the equation.

[0047] S5: Linear fitting is performed based on different metallization ratios and corresponding J0_total to obtain the dark saturation current density of the metallized area and the dark saturation current density of the non-metallized area, where:

[0048] With the metallization ratio as the horizontal axis and the corresponding J0_total as the vertical axis, a linear fit is performed according to the formula:

[0049] J0_metal=a+1\2*b

[0050] J0_pass=1\2*b

[0051] a is the slope of the fitted straight line; b is the intercept of the straight line; J0_metal is the dark saturation current density of the metallized area; J0_pass is the dark saturation current density of the non-metallized area;

[0052] Finally, the dark saturation current density of the metallized area is obtained.

[0053] To accurately test the composite size of the metallized part of the solar cell surface, we developed a method to calculate the corresponding ivoc using the different brightness of photoluminescence under different metallization ratios, and then deduce the total surface composite J0_total and the J0_metal of the metallized part. By calculating the J0_metal solution by testing the brightness value after metallizing the test sample with a special pattern, the minimum effective test value of J0_metal is reduced from 200fA / cm2 of the traditional SUNSVOC method to 20fA / cm2 or even lower, which can accurately characterize 100fA / cm 2 For the following metal composites, the correlation coefficient of the fitting curve can reach more than 90%; in addition, this solution omits the metallization process of back gridding, simplifying the test complexity.

[0054] Here are some specific examples:

[0055] Example 1

[0056] S1: Make a sample substrate, which is an N-type crystalline silicon substrate; and install graphic screens with different metallization ratios, the metallization ratios are set to 0, 3%, 6%, 10%, 13%, 16%, 20% and other proportions; a graphic screen can have only one graphic with a metallization ratio, or it can have several graphics with different metallization ratios, and it is designed according to the needs and the size of the graphic screen. The graphic screen is set to a 4-grid, in which the basic graphic is a square area, and there are several metallized grid lines inside the square, and the mesh count of the graphic screen is 450 meshes; the width of the metallized grid line is 35μm.

[0057] S2: Screen-printing silver-aluminum paste on the target test surface of the substrate according to different patterns to obtain a metallized pattern, and then sintering it at a temperature of 800°C to obtain a test sample; wherein the metallized pattern is a plurality of metallized grid line patterns printed on the substrate by a pattern screen of the corresponding target paste, and the number of metallized grid lines can be linearly increased according to different metallization ratios, or designed according to specific parameters. In this embodiment, the metallization ratios are 0%, 3.75%, 5.62%, 7.47%, and 9.33%.

[0058] S3: Test the ivoc of the unmetallized test sample, and then calculate the C value based on the measured brightness value; the unmetallized test sample means that there is no metallized pattern on the target test surface of the substrate, that is, there is no metallized grid line. The ivoc value measured by the sintion module in the PL test equipment or WCT120 is the accurate value, and the formula is used to calculate the C value.

[0059]

[0060] C is the relationship constant; is the brightness; ivoc is the virtual voltage; V t is the voltage constant;

[0061] Substitute the IVOC value of the unmetallized test sample obtained from the test into the above formula: is the brightness measured by the PL test equipment. Substituting it into the above formula, V t is a known voltage constant, which is also substituted into the above formula to finally obtain the relationship constant C.

[0062] During the PL test, the metallized pattern, i.e. the metallized grid line, faces the opposite direction of the PL test. The exposure time selected by the PL test is 0.01s and the condition is 1sun. The ivoc value is 706mv. is 9688; V t is 25.9mv; substituting into the formula, the final C value is 1.40584E-08.

[0063] S4: deriving the ivoc of the test samples with different metallization ratios through the value of C, and then calculating the J0_total of the test samples with different metallization ratios according to the ivoc of the test samples with different metallization ratios and the measured brightness values; wherein,

[0064] The ivoc values ​​of test samples with different metallization ratios are measured using the sintion module in the PL test equipment or WCT120. The ivoc values ​​obtained for the metallized test samples are inaccurate and need to be calculated using the formula

[0065]

[0066] After S3 obtains the relationship constant C, substitute the relationship constant C into the formula, and then use the brightness of different metallization ratios obtained by the PL test equipment to calculate the brightness of different metallization ratios. Substituting into the formula, V t is a known voltage constant, which is also substituted into the above formula to finally obtain the calculated ivoc value. This ivoc value is an accurate value. Substitute this accurate value into the formula for calculating J0_total to calculate the dark saturation current density.

[0067] For 9688mv, 7893mv, 8183mv, 7589.5mv, 7381.5mv; V t is 25.9mv; C value is 1.40584E-08, which is substituted into the formula to obtain the ivoc values ​​of 706mv, 700.69mv, 701.6mv, 699.6mv, and 698.9mv.

[0068] By formula

[0069] j geg =q(1-R)j γ

[0070] j rec =J0_total×exp(ivoc / V t )

[0071] j gen =j rec

[0072] j nen Generates current for the battery; rec is the recombination current of the battery; q is a constant; R is the reflectivity; j γ is the luminous flux; J0_total is the dark saturation current density; ivoc is the virtual voltage; V t is the voltage constant;

[0073] Calculate the value of J0_total. In equilibrium, j gen With j rec equal, that is, the current generated by the battery is the same as the composite current, and the equation q(1-R)j can be obtained γ =J0_total×exp(ivoc / V t ), q is a charge, i.e. a constant, substituted into the equation, R is the reflectivity, which can be obtained through PL testing equipment and is also substituted into the formula, j γis the luminous flux, which is a known quantity. Substitute it into the equation, and the part on the left is the known quantity. ivoc uses the exact value calculated in the above steps and substitutes it into the equation. V t is the voltage constant, which is also a known quantity. Substituting it into the above equation, the only unknown quantity in the equation is J0_total. The J0_total value of different metallization ratios is calculated by the equation, and the J0_total value is 55.25fA / cm 2 、67.82fA / cm 2 、65.41fA / cm 2 、70.53fA / cm 2 、72.52fA / cm 2 .

[0074] S5: Perform linear fitting based on the metallization ratio and the corresponding J0_total to obtain the dark saturation current density of the metallization area and the dark saturation current density of the non-metallization area, where:

[0075] With the metallization ratio as the horizontal axis and the corresponding J0_total as the vertical axis, a linear fit is performed according to the formula:

[0076] J0_metal=a+1\2*b

[0077] J0_pass=1\2*b

[0078] a is the slope of the fitted straight line; b is the intercept of the straight line; J0_metal is the dark saturation current density of the metallized area; J0_pass is the dark saturation current density of the non-metallized area; and finally the dark saturation current density of the metallized area is obtained.

[0079] In this embodiment, a is 249 fA / cm 2 ; b is 20fA / cm 2 ; Substituting into the formula, we get J0_metal is 254fA / cm 2 ; J0_pass is 10fA / cm 2 .

[0080] Example 2

[0081] S1: Make a substrate with a PN junction, which is an N-type crystalline silicon substrate; and install graphic screens with different metallization ratios, the metallization ratios are set to 0, 3%, 6%, 10%, 13%, 16%, 20% and other proportions; a graphic screen can have only one graphic with a metallization ratio, or it can have several graphics with different metallization ratios, and it is designed according to the needs and the size of the graphic screen. The graphic screen is set to 4 grids, in which the basic graphic is a square area, and there are several metallized grid lines inside the square, and the mesh count of the graphic screen is 500 meshes; the width of the metallized grid line is 50μm.

[0082] S2: Screen-printing silver-aluminum paste on the target test surface of the substrate according to different patterns to obtain a metallized pattern, and then sintering it at a temperature of 750°C to obtain a test sample; wherein the metallized pattern is a plurality of metallized grid line patterns printed on the substrate by a pattern screen of the corresponding target paste, and the number of metallized grid lines can be linearly increased according to different metallization ratios, or designed according to specific parameters. In this embodiment, the metallization ratios are 0%, 5%, 10%, 15%, and 20%.

[0083] S3: Test the ivoc of the unmetallized test sample, and then calculate the value of C based on the measured brightness value; where,

[0084] The unmetallized test sample means that there is no metallized pattern on the target test surface of the substrate, that is, there is no metallized grid line. The ivoc value measured by the sintion module in the PL test equipment or WCT120 is an accurate value.

[0085]

[0086] C is the relationship constant; is the brightness; ivoc is the virtual voltage; V t is the voltage constant;

[0087] Substitute the IVOC value of the unmetallized test sample obtained from the test into the above formula: is the brightness measured by the PL test equipment. Substituting it into the above formula, V t is a known voltage constant, which is also substituted into the above formula to finally obtain the relationship constant C.

[0088] During the PL test, the metallized pattern, i.e. the metallized grid line, faces the opposite direction of the PL test. The exposure time selected by the PL test is 0.01s and the condition is 1sun. The ivoc value is 706mv. 9688mv; V t is 25.9mv; substituting into the formula, the final C value is 1.40584E-08.

[0089] S4: deriving the ivoc of the test samples with different metallization ratios through the value of C, and then calculating the J0_total of the test samples with different metallization ratios according to the ivoc of the test samples with different metallization ratios and the measured brightness values; wherein,

[0090] The ivoc values ​​of test samples with different metallization ratios are measured using the sintion module in the PL test equipment or WCT120. The ivoc values ​​obtained for the metallized test samples are inaccurate and need to be calculated using the formula

[0091]

[0092] After S3 obtains the relationship constant C, substitute the relationship constant C into the formula, and then use the brightness of different metallization ratios obtained by the PL test equipment to calculate the brightness of different metallization ratios. Substituting into the formula, V t is a known voltage constant, which is also substituted into the above formula to finally obtain the calculated ivoc value. This ivoc value is an accurate value. Substitute this accurate value into the formula for calculating J0_total to calculate the dark saturation current density.

[0093] The C value is 1.40584E-08, 8829mv, 8083mv, 7499mv, 7029mv; V t is 25.9 mv; substituting into the formula, the final IVOC values ​​are 703.6mv, 701.3mv, 699.4mv, and 697.7mv.

[0094] By formula

[0095] j gen =q(1-R)j γ

[0096] j rec =J0_total×exp(ivoc / V t )

[0097] j gen =j rec

[0098] j gen Generates current for the battery; rec is the recombination current of the battery; q is a constant; R is the reflectivity; j γ is the luminous flux; J0_total is the dark saturation current density; ivoc is the virtual voltage; V t is the voltage constant;

[0099] Calculate the value of J0_total. In equilibrium, j gen With j rec equal, that is, the current generated by the battery is the same as the composite current, and the equation q(1-R)j can be obtained γ =J0_total×exp(ivoc / V t ), q is a constant, substituted into the equation, R is the reflectivity, which can be obtained through PL testing equipment and is also substituted into the formula, j γ is the luminous flux, which is a known quantity. Substitute it into the equation, and the part on the left is the known quantity. ivoc uses the exact value calculated in the above steps and substitutes it into the equation. V t is the voltage constant, which is also a known quantity. Substituting it into the above equation, the only unknown quantity in the equation is J0_total. The J0_total values ​​of different metallization ratios are calculated by the equation, and J0_total is 55.25 fA / cm 2 、 60.63fA / cm 2 、66.22fA / cm 2 、71.38fA / cm 2 、76.15fA / cm 2 .

[0100] S5: Perform linear fitting based on the metallization ratio and the corresponding J0_total to obtain the dark saturation current density of the metallization area and the dark saturation current density of the non-metallization area, where:

[0101] With the metallization ratio as the horizontal axis and the corresponding J0_total as the vertical axis, a linear fit is performed according to the formula:

[0102] J0_metal=a+1\2*b

[0103] J0_pass=1\2*b

[0104] a is the slope of the fitted straight line; b is the intercept of the straight line; J0_metal is the dark saturation current density of the metallized area; J0_pass is the dark saturation current density of the non-metallized area; and finally the dark saturation current density of the metallized area is obtained.

[0105] In this embodiment, a is 138.9 fA / cm 2 ; b is 4fA / cm 2 ; Substituting into the formula, we get J0_metal is 134.9fA / cm 2 ; J0_pass is 8fA / cm 2 .

[0106] The embodiments of the present invention are described in detail above, but the contents described are only preferred embodiments of the present invention and cannot be considered to limit the scope of implementation of the present invention. All equivalent changes and improvements made within the scope of the present invention should still fall within the scope of the patent coverage of the present invention.

Claims

1. A method for characterizing metal composites in solar cells using PL. include: Make sample substrates and install graphic screens with different metallization ratios; Screen printing a corresponding target slurry on the target test surface of the substrate according to different patterns to obtain different metallization patterns, and then sintering the patterns to obtain test samples; Test the ivoc of the unmetallized test sample, and then calculate the C value based on the measured brightness value. According to the formula The C value is calculated, where: C is the relationship constant; is the brightness obtained by the test; ivoc is the virtual voltage obtained by the test; V t is the voltage constant; The ivoc of the test samples with different metallization ratios is obtained by the value of C and the measured brightness of the test samples with different metallization ratios. Then, the J0_total of the test samples with different metallization ratios is calculated based on the obtained ivoc. According to the formula j gen =q(1-R)j γ j rec =J0_total×exp(ivoc / V t ) I gen =j rec The J0_total value is calculated, where: j gen Generates current for the battery; rec is the recombination current of the battery; q is a constant; R is the reflectivity obtained by the test; j γ is the luminous flux; J0_total is the dark saturation current density; ivoc is the virtual voltage obtained by the test; V t is the voltage constant; According to different metallization ratios and the corresponding J0_total, linear fitting is performed to obtain the dark saturation current density of the metallized area and the dark saturation current density of the non-metallized area. The metallization ratio is used as the abscissa and the corresponding J0_total is used as the ordinate. Linear fitting is performed according to the formula J0_metal=a+1\2*b J0_pass=1\2*b The J0_metal and J0_pass are calculated, where: a is the slope of the fitted straight line; b is the intercept of the straight line; J0_metal is the dark saturation current density of the metallized area; J0_pass is the dark saturation current density of the non-metallized area.

2. A method for characterizing solar cell metal composites using PL according to claim 1, Features: The metallization pattern is a metallization grid line pattern.

3. A method for characterizing solar cell metal composites using PL according to claim 2, Features: The width of the metallized gate line is 20-50 μm.

4. A method for characterizing metal composites of solar cells using PL according to any one of claims 1 to 3, Features: The mesh number of the graphic screen is 380-520 meshes.

5. The method of characterizing metal composites of solar cells using PL according to claim 1, Features: The brightness of the test sample is measured using a PL test device. During the test, the metallization pattern faces the opposite direction to the PL test device.

6. The method of characterizing metal composites of solar cells using PL according to claim 1, Features: The sintering temperature for performing the sintering process is determined according to the target test surface of the substrate and the target slurry.