Preparation method of sepiolite-carbon nitride composite photocatalyst, its product and application

By compounding sepiolite with carbon nitride and adding TiO2, a sepiolite-carbon nitride-TiO2 composite photocatalyst is formed, which solves the problem of insufficient catalytic activity of graphite phase carbon nitride and significantly improves its photocatalysis under visible light. performance, achieving the effect of efficient degradation of organic dyes.

CN115739159BActive Publication Date: 2024-10-22ZHEJIANG KELEI NEW MATERIAL CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211563924.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-12-07
Publication Date
2024-10-22
Estimated Expiration
2042-12-07

AI Technical Summary

Technical Problem

The catalytic activity of graphite phase carbon nitride photocatalyst is not high, resulting in insufficient photocatalytic performance under visible light. Moreover, the adsorption capacity and surface area of ​​ordinary carbon nitride are small, making it difficult to effectively degrade organic pollutants.

Method used

Sepiolite is combined with carbon nitride, and a sepiolite-carbon nitride-TiO2 composite photocatalyst is synthesized through a specific preparation method to improve its adsorption performance and defect degree, thereby enhancing the photocatalytic activity under visible light. The method includes stirring and ultrasonic treatment of sepiolite in deionized water, adding melamine and benzoic acid to form a precursor and then calcining it, and finally compounding with TiO2 to prepare a composite material with improved photocatalytic activity.

Benefits of technology

The catalytic activity and adsorption performance of the composite material are significantly improved, and organic dyes, especially methylene blue, can be efficiently degraded under visible light, with a removal rate of 98%. At the same time, the preparation process is simple and the conditions are mild, making it suitable for large-scale production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115739159B_ABST
    Figure CN115739159B_ABST
Patent Text Reader

Abstract

The present invention relates to a preparation of a catalyst, and in particular to a preparation method of a sepiolite-carbon nitride-TiO2 composite photocatalyst, its products and applications. It comprises the following steps: adding sepiolite to deionized water, stirring, ultrasonicating, making it fully dispersed in water, and heating and stirring under oil bath conditions; adding melamine to deionized water and ultrasonically dispersing it uniformly, adding it to the sepiolite slurry, and continuing to stir and mix for a certain time; adding benzoic acid solution, the molar ratio of melamine to benzoic acid is (90-110): 1; continuing to stir; drying the mixed solution, grinding it into powder, and obtaining a precursor; calcining the precursor; adding the obtained sepiolite-carbon nitride composite material and TiO2 powder to nitric acid, mixing and standing, washing and drying, grinding, and obtaining the target product, sepiolite-carbon nitride-TiO2 composite photocatalyst. The present invention improves the catalytic activity of graphite phase carbon nitride by compounding, modifying, and loading through the above specific methods.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the preparation of a catalyst, and in particular to a preparation method of a sepiolite-carbon nitride-TiO2 composite photocatalyst, a product thereof and an application thereof. Background Art

[0002] Industrial wastewater has a complex composition and contains a variety of organic matter. Although the commonly used physical treatment methods (adsorption, flocculation, membrane separation, etc.) are simple to operate and have a high removal rate, this method only transfers organic pollutants from one phase to another. If a certain desorbent or desorption means is not used, it will easily cause secondary pollution. In addition, the amount of adsorbent used is large and difficult to recycle, resulting in increased costs and is not suitable for large-scale use. Photocatalytic oxidation is a method that can use semiconductor materials as catalysts. When exposed to light, the electrons on the valence band of the catalyst are excited and migrate to the conduction band to form electrons and holes. Among them, electrons are reducing and holes are oxidizing, which then excite the surrounding water and oxygen to form more active free radicals, thereby destroying organic molecules and decomposing them or even mineralizing them into CO2 and H2O. The photocatalytic method can use clean energy to degrade organic matter, which is environmentally friendly and economical, and can quickly convert organic matter into non-toxic small molecules.

[0003] As the research field of photocatalysts gradually shifts from the ultraviolet region to the visible light region, modified TiO2 photocatalysts, Bi-based photocatalysts, Zn-based photocatalysts and carbon-based photocatalysts have gradually become the key research areas of photocatalysts. Among them, carbon-based materials have unique advantages in electron transport and spatial confinement, and carbon-based materials do not contain transition metals and will not cause secondary pollution.

[0004] Graphitic carbon nitride (g-C3N4) is a typical carbon material with a graphite-like lamellar structure. It has low preparation cost, high chemical stability, and can undergo electron transition under visible light irradiation to catalyze and oxidize organic pollutants. However, ordinary carbon nitride has a small specific surface area, small adsorption capacity, and low photocatalytic performance. Summary of the invention

[0005] The first technical purpose of the present invention is to solve the problem of low photocatalytic activity of the above-mentioned carbon nitride by compounding it with natural clay sepiolite to synthesize a sepiolite-carbon nitride composite photocatalyst, improve its adsorption performance, increase its defect degree, and improve the photocatalytic activity of the composite material under visible light.

[0006] The second technical purpose of the present invention is to provide the application of the sepiolite-carbon nitride composite photocatalyst prepared by the above method.

[0007] The technical solution adopted for the first technical purpose of the present invention is:

[0008] A method for preparing a sepiolite-carbon nitride composite photocatalyst comprises the following steps:

[0009] (1) Add sepiolite to deionized water, stir and ultrasonicate to fully disperse it in the water, and heat and stir under oil bath conditions; wherein the mass concentration of sepiolite in deionized water is 0.5-3%, and the oil bath temperature is 60-95°C;

[0010] (2) After melamine is evenly dispersed in deionized water by ultrasonication, it is added to the sepiolite slurry and stirred for a certain period of time; the mass ratio of sepiolite to melamine is 1: (6-10);

[0011] (3) adding a certain amount of benzoic acid solution dropwise, wherein the molar ratio of melamine to benzoic acid is (90-110):1; and continuing stirring;

[0012] (4) Drying the mixed liquid and grinding it into powder to obtain a precursor;

[0013] (5) calcining the precursor at a temperature of 500-600° C. for 2-6 hours to obtain a sepiolite-carbon nitride composite material;

[0014] (6) The sepiolite-carbon nitride composite material and TiO2 powder are added to nitric acid with a mass concentration of 4-7 mol / L in a mass ratio of (4-6):1, ultrasonicated, stirred and allowed to stand, washed, dried and ground to obtain the target product, sepiolite-carbon nitride-TiO2 composite photocatalyst.

[0015] The present invention improves the catalytic activity by compounding, modifying and loading the above specific methods; at the same time, a small amount of TiO2 is added to further improve the photocatalytic activity of the composite material under visible light, and the preparation method of the composite photocatalyst is simple, convenient, and mild in conditions, which is conducive to large-scale preparation.

[0016] Preferably, the mass concentration of the sepiolite in step (1) is 1.5%, and the mixture is stirred in an oil bath at 70-90°C to obtain a sepiolite slurry.

[0017] Preferably, the amount of melamine added in step (2) is such that the mass ratio of sepiolite to melamine is 1:8.

[0018] Preferably, the amount of benzoic acid added in step (3) is such that the molar ratio of melamine to benzoic acid is 100:1.

[0019] Preferably, the precursor in step (5) is calcined in a muffle furnace at a calcination temperature of 550° C. for a calcination time of 3-5 h.

[0020] Preferably, the concentration of nitric acid in step (6) is 5 M, and the mass ratio of the sepiolite-carbon nitride composite material to TiO2 is 5:1.

[0021] The technical solution adopted by the second technical purpose of the present invention is:

[0022] A sepiolite-carbon nitride-TiO2 composite photocatalyst is prepared by adopting the above preparation method.

[0023] The third technical objective of the present invention is achieved through the following technical solutions:

[0024] The invention discloses an application of a sepiolite-carbon nitride-TiO2 composite photocatalyst for degrading an organic dye methylene blue under visible light.

[0025] In summary, the present invention has the following beneficial effects: the present invention improves the catalytic activity of graphite phase carbon nitride by compounding, modifying and loading through the above specific method; at the same time, adding a small amount of TiO2 further improves the photocatalytic activity of the composite material under visible light, and the preparation method of this composite photocatalyst is simple, convenient, and mild in conditions, which is conducive to large-scale preparation. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] Figure 1 XRD patterns of g-C3N4 synthesized from three different raw materials;

[0027] Figure 2 is the XRD pattern of benzoic acid modified carbon nitride (g-C3N4-B);

[0028] Figure 3 This is the SEM image of benzoic acid modified carbon nitride (g-C3N4-B);

[0029] Figure 4 XRD patterns of sepiolite and sepiolite-carbon nitride composite material (Hg-C3N4);

[0030] Figure 5 This is the SEM image of sepiolite-carbon nitride composite material (Hg-C3N4);

[0031] Figure 6 This is the SEM image of the sepiolite-carbon nitride-TiO2 composite photocatalyst (Hg-C3N4-TiO2);

[0032] Figure 7 The photocatalytic effects of the catalysts of Examples 1-4 on methylene blue under darkness and light are shown. DETAILED DESCRIPTION

[0033] Example 1: Pure carbon nitride (g-C3N4) photocatalyst

[0034] 1. Preparation method

[0035] (1) Weigh 30g urea, 30g thiourea, and 60g melamine respectively into a ceramic crucible, compact it, cover it with a lid, wrap it with tin foil, place it in a muffle furnace, heat it to 550℃, keep it for 4h, and the heating rate is 10℃ / min. After cooling to room temperature, grind it into powder to obtain carbon nitride prepared from different raw materials;

[0036] (2) The yield of each product was obtained by weighing the obtained carbon nitride, among which the g-C3N4 prepared from urea was 1.5g, with a yield of 5%; the g-C3N4 prepared from thiourea was 4g, with a yield of 13.3%; the g-C3N4 prepared from melamine was 30g, with a yield of 50%;

[0037] 2. Testing

[0038] Figure 1 The XRD diagram of g-C3N4 synthesized from three different raw materials shows that the three samples have two diffraction peaks at 2θ=13° and 27°, which are consistent with the g-C3N4 standard card and correspond to the (100) and (002) crystal planes, respectively. This shows that g-C3N4 can be prepared by calcining the three raw materials. Among them, the g-C3N4 crystal form obtained by calcining melamine and thiourea is better than that of urea, and among the three raw materials, melamine has the highest yield, so melamine is selected as the raw material for preparing g-C3N4.

[0039] Example 2: Benzoic acid modified carbon nitride (Bg-C3N4)

[0040] 1. Preparation method

[0041] (1) Weigh 60 g of melamine and add it into deionized water (solid-to-liquid ratio 1:12), ultrasonicate for 15 min, stir and disperse for 30 min, and stir in an oil bath at 90 °C for 30 min;

[0042] (2) Add 20 mL of 0.0048 mol benzoic acid (n tris:n benzene = 100:1) dropwise;

[0043] (3) Continue stirring for 2 h, remove the supernatant, dry at 80 °C, and grind into powder;

[0044] (4) Place the mixture into a crucible, compact it, cover it, and wrap it with tin foil. Heat the muffle furnace to 550°C and maintain for 4 hours at a heating rate of 10°C / min.

[0045] (5) After cooling, grinding is performed to obtain benzoic acid-modified carbon nitride (g-C3N4-B);

[0046] 2. Testing

[0047] Figure 2This is the XRD pattern of carbon nitride modified with benzoic acid (g-C3N4-B). After g-C3N4 modified with benzoic acid, the characteristic peaks of the (100) and (002) crystal planes still exist, and the peak of the (002) crystal plane is enhanced.

[0048] Figure 3 This is the SEM image of benzoic acid-modified carbon nitride (g-C3N4-B). It can be clearly observed that g-C3N4 has larger flakes, ranging from a few microns to tens of microns, and is stacked layer by layer.

[0049] Example 3: Sepiolite-Carbon Nitride Composite Material (Hg-C3N4)

[0050] 1. Preparation method

[0051] (1) 7.5 g of sepiolite was added to deionized water, sheared and dispersed at 1500 rpm for 10 min, and then ultrasonicated for 5 min to form a 1.5% uniform slurry, which was then stirred in an oil bath at 90 °C for 30 min;

[0052] (2) 60 g of melamine was added to deionized water and ultrasonically stirred for 30 min, then the sepiolite slurry was added and stirring was continued for 1 h;

[0053] (3) Add 20 mL of 0.0048 mol benzoic acid dropwise (n tris:n benzene = 100:1);

[0054] (4) Continue stirring for 2 h and ultrasonicate for 30 min;

[0055] (5) The mixed solution was dried at 80°C, ground into powder, and then heated to 550°C in a muffle furnace for calcination for 4 h at a heating rate of 10°C / min;

[0056] (6) After cooling, grinding to obtain a sepiolite-carbon nitride composite material (Hg-C3N4);

[0057] 2. Testing

[0058] Figure 4 The XRD patterns of sepiolite and sepiolite-carbon nitride composite material (Hg-C3N4) show that the XRD pattern of Hg-C3N4 has characteristic peaks of both sepiolite and g-C3N4. The introduction of sepiolite does not destroy the structure of g-C3N4, and its crystal form is also good.

[0059] Figure 5 This is the SEM image of the sepiolite-carbon nitride composite material (Hg-C3N4). Needle-shaped sepiolite structures can be observed on the carbon nitride flakes, which makes the surface of the carbon nitride rough, which is beneficial to increase its surface area and roughness.

[0060] Example 4: Sepiolite-Carbon Nitride-TiO2 Composite Photocatalyst (Hg-C3N4-TiO2)

[0061] 1. Preparation method

[0062] (1) Weigh 10 g of the sepiolite-carbon nitride composite material prepared in Example 3 and 2 g of P25 TiO2 powder, add them to 5 M nitric acid, ultrasonicate for 30 min, stir at room temperature for 3 h, and let stand overnight;

[0063] (2) removing the supernatant, washing, drying, and grinding to obtain a sepiolite-carbon nitride-TiO2 composite photocatalyst (Hg-C3N4-TiO2);

[0064] 2. Testing

[0065] Figure 6 This is a SEM image of the sepiolite-carbon nitride-TiO2 composite photocatalyst (Hg-C3N4-TiO2). It can be seen that nano-sized granular TiO2 is loaded on the sheet, further increasing the surface area of ​​the composite material and increasing its photocatalytic active sites.

[0066] Example 5: Photocatalytic application of various materials

[0067] The photocatalytic performance of each photocatalyst prepared in Examples 1-4 was tested under visible light.

[0068] Test method:

[0069] A 50W LED lamp is used as the light source, and its wavelength range is 380~780nm. Add the samples prepared in Examples 1-4 to a beaker containing 20mg / L methylene blue solution (MB) in an amount of 1g / L, perform magnetic stirring, and point the light source directly above the beaker. First stir for 60 minutes in the dark (lights off) to allow it to reach adsorption equilibrium, and then carry out photocatalytic reaction under light (lights on). Sampling is performed at certain time intervals, and after passing through a 0.22 μm water-based needle filter membrane, the absorbance of methylene blue is measured at 669nm in a spectrophotometer, and the removal rate of methylene blue is calculated to test the photocatalytic performance of each photocatalyst. The results are shown in Figure 7 .

[0070] Figure 7The photocatalytic effect of each catalyst on methylene blue in the dark and under light is shown in the figure. It can be seen from the figure that graphite carbon nitride has a certain photocatalytic activity under visible light, and g-C3N4 can remove about 40% of MB after 2.5 hours of light exposure. After modification with benzoic acid, its MB photolysis removal rate increased to 56%. The introduction of sepiolite improved its adsorption and photocatalytic properties, and the MB removal rate reached 69%. The further introduction of TiO2 further improved its adsorption and photocatalytic properties, and the final photocatalytic MB removal rate reached 98%.

[0071] This specific embodiment is merely an explanation of the present invention and is not a limitation of the present invention. After reading this specification, those skilled in the art may make non-creative modifications to the present embodiment as needed. However, as long as they are within the scope of the claims of the present invention, they are protected by the patent law.

Claims

1. A sepiolite-carbon nitride-TiO 2 Composite photocatalyst preparation method, Features The following steps are involved: (1) adding sepiolite to deionized water, stirring and ultrasonicating the mixture to fully disperse the mixture in the water, and heating and stirring the mixture in an oil bath; wherein the mass concentration of the sepiolite in step (1) is 1.5%, and stirring the mixture in an oil bath at 70 to 90° C. is performed to obtain a sepiolite slurry; (2) adding melamine to deionized water and uniformly dispersing it by ultrasonication, then adding it to the sepiolite slurry and continuing to stir and mix for a certain period of time; the amount of melamine added is such that the mass ratio of sepiolite to melamine is 1:8; (3) adding benzoic acid solution in an amount such that the molar ratio of melamine to benzoic acid is 100:1, and continuing stirring; (4) Drying the mixed liquid and grinding it into powder to obtain a precursor; (5) calcining the precursor in a muffle furnace at a temperature of 550° C. for a time of 4-5 h to obtain a sepiolite-carbon nitride composite material; (6) Sepiolite-carbon nitride composite material and TiO 2 The powder was added to nitric acid with a mass concentration of 5 mol / L at a mass ratio of 5:1, mixed and allowed to stand, washed, dried, and ground to obtain the target product, sepiolite-carbon nitride-TiO 2 Composite photocatalyst.

2. A sepiolite-carbon nitride-TiO 2 The composite photocatalyst is prepared by the preparation method described in claim 1.

3. A sepiolite-carbon nitride-TiO according to claim 2 2 Application of composite photocatalyst in degradation of organic dye methylene blue under visible light.