A processing method for improving the storage time and collection effect of collector
By adding sodium lauryl sulfate, CO2 gas, aluminum sulfate and Tween 80 to the lithium ore flotation collector, and adjusting the composition and proportion, the problem of short storage time of the collector was solved, the storage time was extended and the The mineral processing effect is improved, especially the desulfurization rate is improved during lithium slag treatment, and the problem of poor stability of the collector in the existing technology is solved.
Patent Information
- Application Number
- CN202211383903.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-11-07
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2042-11-07
AI Technical Summary
The storage time of existing lithium ore flotation collectors is short, resulting in unstable collection effects and inability to meet industrial needs. It is difficult to effectively improve the storage time and collection effects of various collectors with existing technology.
Add sodium lauryl sulfate and CO2 gas to the water, add aluminum sulfate and Tween 80, mix evenly, adjust the composition and proportion of the collector, pressurize the CO2 gas to extend the storage time of the collector, and Improve its mineral processing effect.
It significantly extends the storage time of the collector from days to months, and on this basis improves the mineral processing effect, increases the desulfurization rate of lithium slag, enhances the operating efficiency of mineral processing work and the comprehensive utilization value of lithium slag .
Smart Images

Figure BDA0003929010350000101 
Figure BDA0003929010350000111
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of mineral processing, relates to mineral processing flotation reagent technology, and specifically relates to a processing method for improving the storage time of a collector and the collection effect. Background Art
[0002] Lithium is known as the "energy metal that drives the world's progress". Lithium and its compounds have important strategic significance in the national economy and national defense construction, and are widely used in industries such as pharmaceuticals, ceramics, batteries, aerospace and nuclear energy. Li Chengxiu and others from the Institute of Comprehensive Utilization of Mineral Resources, Chinese Academy of Geological Sciences [1] A detailed introduction to the spodumene ore dressing process was given, including an introduction to the current status of research on flotation collectors. Li Shaoping from Xinjiang Engineering College [2] et al. systematically introduced the research status of lithium mica flotation collectors.
[0003] Generally speaking, most lithium ores with industrial value can be separated by flotation, so the corresponding flotation collectors have always been the focus of research. However, existing research usually only focuses on the problems of fine-grained mud, poor selectivity and foaming, and large dosage of lithium ore in flotation practice, thus focusing on the research and development of efficient, highly selective, low-temperature resistant and environmentally friendly reagents as the main research direction of lithium ore flotation reagents. [3] .
[0004] In actual research and production, the inventors found that the storage time has a great influence on the collection effect of the collector, and can even lead to the instability of the physical and chemical properties of the collector (such as stratification), thus resulting in the loss of practical use value, such as Liu Zhifang et al. in their patent application [4] It is mentioned that after saponified oleic acid is left for more than 2 months, the product properties will change, sodium oleate will precipitate and cause stratification. After sulfonated oleic acid is left for about 10 days, oleic acid and oleic acid sulfate will be severely stratified.
[0005] At present, there are few reports on the impact of storage factors on lithium ore collectors, and even for other flotation objects, there are only sporadic reports. For example, Qin Hu of Sichuan Jiangxi Copper Rare Earth Co., Ltd. reported on the effect of rare earth collector storage time on flotation. [5] In addition, although there is no large-scale research direction for increasing the storage time of flotation agents, some existing studies have already taken obtaining flotation agents with long storage time as a research goal. For example, the Chinese patent application number 201811429935.6, "A flotation inhibitor, its preparation method and application", obtained a flotation inhibitor with high solubility, stable performance and long storage time. [6]; The Chinese patent application number 202110752069.X "A combined collector for desiliconization and carbon removal of phosphogypsum and its solution preparation method and application" has obtained a combined collector that can be stably stored at low temperatures [7] However, these technologies can usually only solve the storage problem of a certain type of medicine, and cannot solve the shortcomings of other existing medicines that are not resistant to storage, resulting in limited actual value.
[0006] Therefore, there is an urgent need in the art for a technology that can increase the storage time of collectors.
[0007] References:
[0008] [1] Li Chengxiu, Cheng Renju, Liu Xing. Research status and prospects of spodumene ore dressing technology in my country[J]. Comprehensive Utilization of Mineral Resources, 2021(05):1-8.
[0009] [3] Li Shaoping, Zhang Junmin, Dilinur Abdukade, Wang Yali. Research status and prospects of lepidolite flotation collectors[J]. Mineral Conservation and Utilization, 2020, 40(06): 77-82.
[0010] [3] Zhu Yimin, Xie Ruiqi, Zhang Meng. Review of research on collectors and regulators for spodumene flotation[J]. Metal Mines, 2019(02):15-21.
[0011] [4] Liu Zhifang, Cao Waifang, Ma Xingwei, Liu Zhenjun, Xiao Yanhua. Fluorite flotation collector [P]. Hunan: CN103341412A, 2013-10-09.
[0012] [5] Qin Hu. Study on the influence of storage time of rare earth collector on flotation[J]. Management and Technology of Small and Medium Enterprises (Second Half Monthly), 2017(08):174-175.
[0013] [6] Zhang Chunlei, Zhang Cheng, He Wen, Yang Guochun, Fu Yuhua. A flotation depressant and its preparation method and application [P]. Jiangxi Province: CN109395886A, 2019-03-01.
[0014] [7] Chai Wencui, Cao Yijun, Zhang Han, Peng Weijun, Fan Guixia. A combined collector for desiliconization and carbon removal of phosphogypsum and its solution preparation method and application [P]. Henan Province: CN113695085A, 2021-11-26. Summary of the invention
[0015] In view of the shortcomings of the prior art, the object of the present invention is to provide a method for flotation collectors for various lithium ores, thereby increasing their storage time and collection effect and at the same time increasing the desulfurization rate when treating lithium slag.
[0016] In order to achieve the above object, the present invention provides the following technical solutions:
[0017] A processing method for improving the storage time and collection effect of a collector, the method comprising:
[0018] (1) adding sodium dodecyl sulfate to water so that the concentration of sodium dodecyl sulfate in water is 0.5 to 1.5 g / L, and stirring at 60 to 95° C.;
[0019] (2) adding a collector to the product obtained in step (1), injecting CO2 gas under pressure, and then adding aluminum sulfate and Tween 80, and mixing them evenly; the weight ratio of aluminum sulfate to collector is 1:150-200, and the weight ratio of Tween 80 to collector is 1:300-400;
[0020] The collector is a combined collector used for lithium ore flotation, and the combined collector is selected from at least two of cyclohexane acid soap, oxidized paraffin soap, dodecylamine, tall oil, sodium oleate, oleic acid, hydroxamic acid, salicylic hydroxamic acid, hydroxylamine hydrochloride, sulfonated soap, and sodium fatty acid methyl ester sulfonate.
[0021] The lithium ore includes spodumene, lepidolite or eucryptite.
[0022] Preferably, the weight ratio of the aluminum sulfate to Tween 80 is 1:1.8.
[0023] Preferably, the weight ratio of the aluminum sulfate to the collector is 1:200.
[0024] Preferably, the combined collector consists of cyclohexane acid soap and oxidized paraffin soap, or consists of oxidized paraffin soap and tall oil, or consists of dodecylamine and sodium oleate, or consists of hydroxamic acid and oxidized paraffin soap, or consists of oxidized paraffin soap, oleic acid and sulfonated soap.
[0025] Preferably, the combined collector consists of oxidized paraffin soap, oleic acid and sulfonated soap.
[0026] Preferably, in the combined collector, the weight ratio of oxidized paraffin soap, oleic acid and sulfonated soap is 6:4:3.
[0027] Preferably, the method further comprises step (3): adding water until the collector reaches a desired concentration, and stirring for 30 to 60 minutes.
[0028] Preferably, the volume ratio of the CO2 gas added in step (2) to the product obtained in step (1) is 1:2 to 3.
[0029] Preferably, in step (1), the concentration of sodium dodecyl sulfate in water is 1 g / L.
[0030] During the research process of the present invention, the inventors found that the collector's collection effect would be greatly weakened after being stored for a period of time. This phenomenon is similar to the situation reported by Qin Hu in his article "Study on the Effect of Storage Time of Rare Earth Collectors on Flotation" (Qin Hu. Study on the Effect of Storage Time of Rare Earth Collectors on Flotation [J]. Management and Technology of Small and Medium Enterprises (Second Half Monthly), 2017(08):174-175).
[0031] At present, there are relatively few studies on adding corresponding additives to collectors to increase their storage time (i.e., the collection effect remains unchanged after a certain period of storage). Existing studies generally adjust the composition and ratio of collectors to obtain better stability, such as Liu Tengfei. [7] The effects of different emulsifiers, emulsifiers and stabilizers and their ratios on the stability of the obtained collector were investigated. The inventor initially added different additives to the collector, but none of them could achieve the effect of increasing the storage time of the collector. In subsequent scientific research, the inventor accidentally passed CO2 gas under pressure into the collector added with relevant reagents when performing related pressurized flotation work, and unexpectedly found that the storage time of the collector was extended.
[0032] Generally speaking, during the flotation process, CO2 is introduced mainly to increase the number of micro-nano gas nuclei in the water, and to change the surface properties of minerals through the nano gas nuclei, thereby improving the flotation efficiency. For example, Ou Leming et al. from Central South University [8] This method is used. In the present invention, the role of CO2 is obviously not to provide micro-nano gas cores. The inventors speculate that the introduction of CO2 may change the solubility and interaction of each component, so that the treated system is in a long-term stable state to maintain long-term stability. The mechanism in this regard needs further research and analysis by researchers in this field.
[0033] Aluminum sulfate in the present invention can be used as a regulator in the flotation of other minerals in a few reports, such as Chen Hui et al. of Yidu Xingfa Chemical Co., Ltd. [9] In the patent, aluminum sulfate is used as one of the components of the regulator. However, in the present invention, the aluminum sulfate in maintaining the collection efficiency cannot be explained by using it as a regulator. Polyaluminum sulfate is usually used as an emulsifier.
[10] , providing a stable emulsion system. Polyaluminium sulfate is an inorganic high molecular polymer between aluminium sulfate and aluminium hydroxide, and aluminium sulfate is usually not used as an emulsifier. Therefore, the aluminium sulfate in the present invention may not be explained by providing a stable emulsion.
[0034] Sodium dodecyl sulfate is a common surfactant and can be used as a foam stabilizer in the field of mineral flotation. For example, Zhao Yuqing et al. from the Qinghai Provincial Geological and Mineral Testing and Application Center
[11] In the patent, sodium lauryl sulfate is used as a bubble stabilizer. However, the present invention obviously cannot be explained by the theory of bubble stabilizer.
[0035] In order to investigate the influence of aluminum sulfate and sodium dodecyl sulfate on the present invention, the present invention conducted control experiments in the corresponding steps and found that aluminum sulfate and sodium dodecyl sulfate are indispensable. Although the absence of Tween can slightly increase the storage period, the increase is of no substantial help to industrial production.
[0036] As shown in one embodiment of the present invention, for a collector composed of oxidized paraffin soap, oleic acid and sulfonated soap, the present invention can extend the storage time of the collector from 3 to 7 days to 6 months. At the same time, after being treated by the present invention, the mineral processing effect of the collector is also slightly improved.
[0037] As shown in a test example of the present invention, the present invention can not only prolong the storage time of the collector, but also improve the desulfurization rate in the treatment of lithium slag.
[0038] It can be seen that the beneficial effects of the present invention and its contribution to the art are:
[0039] A treatment method for significantly increasing the storage time of a collector is provided, and on this basis, the mineral processing effect of the collector is slightly improved, so that workers in this field do not need to prepare the collector on the spot during mineral processing, and thus the collector can be prepared on a large scale and stored for later use, which greatly improves the operating efficiency of the mineral processing work; the present invention can also increase the desulfurization rate during lithium slag processing, which is beneficial to the comprehensive utilization of lithium slag.
[0040] References:
[0041] [7] Liu Tengfei, Feng Li. Effect of additives on the stability of emulsified diesel collectors[J]. Laboratory Research and Exploration, 2012, 31(12): 19-23.
[0042] [8] Ou Leming, Chen Hao, Feng Qiming, Lu Yiping, Zhou Weiguang. A flotation method for bauxite
[0043] [P]. Hunan Province: CN108452941A, 2020-03-10.
[0044] [9] Chen Hui, Zheng Guangming, Liu Xin, Li Fang, Wang Xudong, Sun Hualin, Liu Bingbing. A mixed reverse flotation process for phosphate ore[P]. Hubei Province: CN113182078A, 2021-07-30.
[0045]
[10] Li Haidong. ASA emulsion stabilized by polyaluminium sulfate and inorganic nanoparticles[D]. Qilu University of Technology, 2013.
[0046]
[11] Zhao Yuqing, Ying Yongpeng, Zhang Peiqing, Du Zuopeng, Xiong Xin, Wei Zhenhong, Liu De, Zhu Lin, Xie Haidong. A method for improving the grade of low-grade spodumene rougher concentrate [P]. Hubei Province: CN113058748A, 2021-07-02. DETAILED DESCRIPTION
[0047] The present invention is described in detail below through examples. It is necessary to point out that the following examples are only used to further illustrate the present invention and cannot be understood as limiting the scope of protection of the present invention. Some non-essential improvements and adjustments made by technical personnel in this field based on the above invention content still fall within the scope of protection of the present invention.
[0048] Embodiment 1:
[0049] (1) adding sodium dodecyl sulfate to water so that the concentration of sodium dodecyl sulfate in water is 1 g / L, and stirring at 70 to 80° C.;
[0050] (2) adding a collector to the product obtained in step (1), injecting CO2 gas under pressure, and then adding aluminum sulfate and Tween 80, and mixing them evenly; the weight ratio of aluminum sulfate to collector is 1:200, and the weight ratio of Tween 80 to collector is 1:360;
[0051] The collector is composed of oxidized paraffin soap, oleic acid and sulfonated soap in a weight ratio of 6:4:3.
[0052] Example 2
[0053] (1) adding sodium dodecyl sulfate to water so that the concentration of sodium dodecyl sulfate in water is 1.5 g / L, and stirring at 80 to 95° C.;
[0054] (2) adding a collector to the product obtained in step (1), injecting CO2 gas under pressure, and then adding aluminum sulfate and Tween 80, and mixing them evenly; the weight ratio of aluminum sulfate to collector is 1:150, and the weight ratio of Tween 80 to collector is 1:400;
[0055] The collector is composed of oxidized paraffin soap, oleic acid and sulfonated soap in a weight ratio of 6:4:3.
[0056] Example 3
[0057] (1) adding sodium dodecyl sulfate to water so that the concentration of sodium dodecyl sulfate in water is 0.5 g / L, and stirring at 60 to 70° C.;
[0058] (2) adding a collector to the product obtained in step (1), injecting CO2 gas under pressure, and then adding aluminum sulfate and Tween 80, and mixing them evenly; the weight ratio of aluminum sulfate to collector is 1:300, and the weight ratio of Tween 80 to collector is 1:300;
[0059] The collector is composed of oxidized paraffin soap, oleic acid and sulfonated soap in a weight ratio of 6:4:3.
[0060] Example 4
[0061] Except that the collector is composed of oxidized paraffin soap and cyclohexane acid soap in a weight ratio of 11:1, the rest is the same as Example 1.
[0062] Example 5
[0063] Except that the collector is composed of oxidized paraffin soap and tall oil in a weight ratio of 9:1, the rest is the same as Example 1.
[0064] Example 6
[0065] Except that the collector is composed of dodecylamine and sodium oleate in a molar ratio of 1:6, the rest is the same as Example 1.
[0066] Example 7
[0067] Except that the collector is composed of hydroxamic acid and oxidized paraffin soap in a weight ratio of 1:8, the rest is the same as Example 1.
[0068] Test Example 1
[0069] Example 1 was used as the experimental group, and multiple schemes were set as the control group. The spodumene beneficiation test was carried out with reference to the process of Figure 1 in Reference 1 (He Guichun, Xiang Huamei, Jiang Wei, Qi Meichao. Experimental study on the beneficiation process of a low-grade spodumene mine in Sichuan [J]. Non-metallic Minerals, 2014, 37(01): 48-50.), and the collector feeding was adjusted to one-time feeding (the experimental groups of the following other test examples were all fed once based on reference to their respective references).
[0070] Control group 1: The collector was treated by adding the collector to 80°C water, injecting CO2 gas under pressure, and then adding aluminum sulfate and Tween 80 and mixing them evenly; the weight ratio of aluminum sulfate to collector was 1:200, and the weight ratio of Tween 80 to collector was 1:360. The collector was composed of oxidized paraffin soap, oleic acid and sulfonated soap in a weight ratio of 6:4:3.
[0071] Control group 2: The treatment of the collector is as follows: sodium dodecyl sulfate is added to water so that the concentration of sodium dodecyl sulfate in water is 1g / L, and stirred evenly at 70-80°C; the collector is added, CO2 gas is pressurized, and then Tween 80 is added and mixed evenly; the weight ratio of Tween 80 to the collector is 1:360; the collector is composed of oxidized paraffin soap, oleic acid and sulfonated soap in a weight ratio of 6:4:3.
[0072] Control group 3: The treatment of the collector is as follows: sodium dodecyl sulfate is added to water so that the concentration of sodium dodecyl sulfate in water is 1g / L, and stirred evenly at 70-80°C; the collector is added, CO2 gas is pressurized, and then aluminum sulfate is added and mixed evenly; the weight ratio of aluminum sulfate to collector is 1:200; the collector is composed of oxidized paraffin soap, oleic acid and sulfonated soap in a weight ratio of 6:4:3.
[0073] Blank control group: The collector of reference 1 was used, that is, the collector was composed of oxidized paraffin soap, oleic acid and sulfonated soap in a weight ratio of 6:4:3, without any treatment, and was stored after preparation.
[0074] The collectors of the experimental group, the blank control group and the control groups 1-3 were stored at room temperature (15-20°C) for 0 days, 3 days, 7 days, 14 days, 30 days, 2 months, 4 months and 6 months, and then the ore dressing test was carried out. The spodumene used was a spodumene mine in Sichuan, and the ore grade was 1.43%. The experimental results are shown in Table 1:
[0075] Table 1
[0076]
[0077]
[0078] Note 1: The data in the table are obtained by taking the average value after each group of experiments were carried out 3 times. After 2 and 4 months of storage, the grade of the experimental group increased slightly with the storage time, which does not mean that the longer the storage time, the higher the mineral processing effect. It should be understood that the mineral processing effect is not affected.
[0079] Note 2: In the table, “-” means that the corresponding test was not conducted because it is no longer necessary.
[0080] Test Example 2
[0081] For the collector treated in Example 2-3, after being stored for 0 and 6 months with reference to Test Example 1, a mineral processing test was carried out. It was found that after the collector was stored for 6 months, relative to the storage for 0 day, after the mineral processing test, the Li2O grade decreased by no more than 2%, and the recovery rate decreased by no more than 5% (the relevant data is not shown anymore).
[0082] Test Example 3
[0083] For the collector treated in Example 4, a beneficiation test was carried out according to the process in Figure 1 of Reference 2 (He Yangyang, Xie Zhiyuan. Study on the beneficiation test of a spodumene mine in western Sichuan [J]. Chemical Minerals and Processing, 2017, 46(5): 13-14).
[0084] After 0 and 6 months of storage in reference example 1, a mineral processing test was carried out. It was found that after the collector was stored for 6 months, relative to the storage for 0 day, after the mineral processing test, the concentrate grade decreased by no more than 3%, and the recovery rate decreased by no more than 8% (the relevant data is not shown anymore).
[0085] The collector of reference 2 (not treated in any way, stored immediately after preparation) was used as a blank control for the test, and the storage time of the collector did not exceed 3 days (i.e., after 3 days of storage, the concentrate grade dropped by more than 20%).
[0086] Test Example 4
[0087] The collector treated in Example 5 was subjected to a mineral processing test with reference to the mineral processing flow of Reference 3 (Zhao Yun. Exploration of the flotation recovery rate of high-grade spodumene [J]. Xinjiang Nonferrous Metals, 2005 (S): 37-39).
[0088] Referring to Example 1, after storage for 0 and 6 months, a mineral processing test was carried out. It was found that after the collector was stored for 6 months, relative to storage for 0 days, after the mineral processing test, the concentrate grade decreased by no more than 2%, and the recovery rate decreased by no more than 6% (the relevant data is not shown anymore).
[0089] The collector of reference 3 (without any treatment, stored immediately after preparation) was used as a blank control for the test, and the storage time of the collector did not exceed 3 days (i.e., after 3 days of storage, the concentrate grade dropped by more than 20%).
[0090] Test Example 5
[0091] The collector treated in Example 7 was subjected to a mineral processing test with reference to the mineral processing flow of Reference 4 (Fan Xinbin. Improvement of spodumene flotation reagent for recycling spodumene from Koktokay tailings [J]. Xinjiang Nonferrous Metals, 2012, 35(06): 46-48.).
[0092] Referring to Example 1, after storage for 0 and 6 months, a mineral processing test was carried out. It was found that after the collector was stored for 6 months, relative to storage for 0 day, after the mineral processing test, the concentrate grade decreased by no more than 1%, and the recovery rate decreased by no more than 5% (the relevant data is not shown anymore).
[0093] The collector of reference 4 (without any treatment, stored immediately after preparation) was used as a blank control for the test, and the storage time of the collector did not exceed 7 days (i.e., after 7 days of storage, the concentrate grade dropped by more than 20%).
[0094] Test Example 6
[0095] Except that the target mineral is lithium mica from a certain place in Jiangxi Province, and the collector is composed of dodecylamine and sodium oleate in a weight ratio of 3:1, the collector treated in Example 1 is subjected to a mineral processing test with reference to the mineral processing process of Reference 5 (Wang Linlin, Zhu Lingyan, Liu Yuelong, Liu Gousheng. Research on the flotation of medium and low grade lithium mica using anionic and cationic mixed collectors [J]. Nonferrous Metals (Mineral Processing Part), 2019(03):86-92.).
[0096] Referring to Example 1, after storage for 0 and 6 months, a mineral processing test was carried out. It was found that after the collector was stored for 6 months, relative to storage for 0 day, after the mineral processing test, the concentrate grade decreased by no more than 3%, and the recovery rate decreased by no more than 5% (the relevant data is not shown anymore).
[0097] The collector of reference 5 (without any treatment, stored immediately after preparation) was used as a blank control for the test, and the storage time of the collector did not exceed 7 days (i.e., after 7 days of storage, the concentrate grade decreased by more than 15%).
[0098] Test Example 7
[0099] This experiment investigated the effect of Example 6 on the desulfurization rate when treating lithium slag. Dodecylamine and sodium oleate were used as collectors (the molar ratio was 1:6), and the collectors were treated according to the steps of Example 1. The desulfurization process in Example 1 of ZL201810044973.3 was referred to for desulfurization treatment, and the collector not treated by Example 1 was used as a blank control. After comparison, on the 3rd day and the 7th day, the desulfurization rate was 11.7% and 26.4% higher than that of the blank control group, respectively.
Claims
1. A treatment method for increasing the storage time and collection effect of collectors, It is characterized in that The method comprises: (1) adding sodium dodecyl sulfate to water so that the concentration of sodium dodecyl sulfate in water is 0.5 to 1.5 g / L, and stirring at 60 to 95° C.; (2) Add the collector to the product obtained in step (1), and pressurize and inject CO 2 gas, then add aluminum sulfate and Tween 80 and mix well; the weight ratio of aluminum sulfate to collector is 1:150-200, and the weight ratio of Tween 80 to collector is 1:300-400; The collector is a combined collector used for lithium ore flotation, and the combined collector is selected from at least two of cyclohexane acid soap, oxidized paraffin soap, dodecylamine, tall oil, sodium oleate, oleic acid, hydroxamic acid, salicylic hydroxamic acid, hydroxylamine hydrochloride, sulfonated soap, and sodium fatty acid methyl ester sulfonate.
2. The processing method according to claim 1, It is characterized in that The lithium ore includes spodumene, lepidolite or eucryptite.
3. The processing method according to claim 1, It is characterized in that The weight ratio of the aluminum sulfate to Tween 80 is 1:1.
8.
4. The processing method according to claim 3, It is characterized in that The weight ratio of the aluminum sulfate to the collector is 1:
200.
5. The processing method according to claim 1, It is characterized in that The combined collector consists of naphthenic acid soap and oxidized paraffin soap, or consists of oxidized paraffin soap and tall oil, or consists of dodecylamine and sodium oleate, or consists of hydroxamic acid and oxidized paraffin soap, or consists of oxidized paraffin soap, oleic acid and sulfonated soap.
6. The processing method according to claim 5, It is characterized in that In the combined collector, the weight ratio of oxidized paraffin soap, oleic acid and sulfonated soap is 6:4:
3.
7. The processing method according to claim 1, It is characterized in that The method further comprises step (3): adding water until the collector reaches a desired concentration, and stirring for 30 to 60 minutes.
8. The processing method according to claim 3, It is characterized in that The CO added in step (2) 2 The volume ratio of the gas to the product obtained in step (1) is 1:2-3.
9. The processing method according to claim 6, It is characterized in that In step (1), the concentration of sodium dodecyl sulfate in water is 1 g / L.