A TiAl alloy blade and a manufacturing method thereof

Through additive design and electron beam 3D printing combined with electromagnetic field-assisted processing and post-processing technology, the forming difficulty and brittleness problems of TiAl alloy blades have been solved, rapid and efficient manufacturing and performance improvement have been achieved, and the disadvantages of coarse structure and component segregation of traditional casting have been overcome. .

CN115740494BActive Publication Date: 2024-10-11CHENGDU ADVANCED METAL MATERIALS IND TECH RES INST CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211360099.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-11-02
Publication Date
2024-10-11
Estimated Expiration
2042-11-02

AI Technical Summary

Technical Problem

The traditional processing method of TiAl alloy blades has problems such as difficult forming, high brittleness, long mold manufacturing cycle, and difficult machining. Moreover, laser 3D printing technology cannot perform high-temperature preheating and cannot effectively solve the crack problem of TiAl alloy materials.

Method used

Using additive design and electron beam 3D printing methods combined with electromagnetic field in-situ auxiliary processing and post-processing technology, through additive processing design, anti-deformation compensation design, electron beam 3D printing and heat treatment, a TiAl alloy with dimensional accuracy and surface finish is prepared. blade.

Benefits of technology

The rapid and efficient manufacturing of TiAl alloy blades is achieved, and parts with fine grains, uniform structures, and excellent performance are obtained. The problems of coarse crystal structures and component segregation in traditional casting are solved, and the material utilization rate and production efficiency are improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115740494B_ABST
    Figure CN115740494B_ABST
Patent Text Reader

Abstract

The present invention belongs to the technical field of metal additive manufacturing, and discloses a TiAl alloy blade and a manufacturing method thereof, including performing additive processing design and additive processing simulation analysis on a blade model; performing anti-deformation compensation design on the blade model to obtain a compensation optimization model of the blade; processing the attitude optimization data, support generation data and slice data of the printed part according to the compensation optimization model and exporting the processed data; setting 3D printing process parameters according to the processed data; wrapping an electromagnetic field environment on the forming surface of the 3D printed part; performing 3D printing processing of the TiAl alloy blade under the 3D printing process parameters and electromagnetic field environment to obtain a blank; and post-processing the blank to obtain a finished TiAl alloy blade. The present invention adopts additive design and electron beam 3D printing method, cooperates with electromagnetic field in-situ auxiliary processing and post-processing process, to quickly prepare TiAl alloy blade parts with dimensional accuracy and surface finish within the permitted range.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of metal additive manufacturing, and in particular relates to a TiAl alloy blade and a manufacturing method thereof. Background Art

[0002] TiAl-based alloys have become one of the most promising high-temperature structural materials due to their high melting point, high specific strength, high-temperature creep resistance and good oxidation resistance. In the range of 700-850℃, the specific strength of TiAl alloys is significantly higher than that of ordinary titanium alloys and nickel-based high-temperature alloys. TiAl alloys are mainly used to manufacture parts such as compressor blades and low-pressure turbine blades for aircraft engines. At present, domestic Changjiang series commercial aircraft engines such as CJ1000A and CJ2000 have an urgent need for TiAl alloy low-pressure turbine blades. The weight of TiAl blades is 50% lower than that of the original nickel-based high-temperature alloy blades, and the fuel consumption is reduced by 15%, which significantly improves the performance of the engine. There are currently two main production methods for TiAl alloy blades, one is precision casting, and the other is additive manufacturing. The GEnx engine of GE in the United States and the LEAP engine of the Franco-American joint venture CFM International both use precision casting combined with precision machining or precision forging casting of TiAl alloy blades. The disadvantages are coarse casting structure, long mold manufacturing cycle, and difficult machining. This is because TiAl alloys have intrinsic brittleness, poor room temperature plasticity, and difficulty in forming.

[0003] In order to solve the many problems existing in the traditional processing methods of TiAl alloy blades, additive design and additive manufacturing technology are introduced. Additive manufacturing is an emerging manufacturing technology. It prepares parts by stacking materials "from bottom to top". It has the characteristics of high material utilization, high processing efficiency, and the ability to process complex parts. 3D printed parts have the advantages of fine grains, uniform organization, and excellent mechanical properties. They have obvious advantages in manufacturing small batches, complex structures, special-shaped parts, refractory parts, gradient or lattice structure parts, especially in the field of engine manufacturing. It has been increasingly used. Due to the intrinsic brittleness of TiAl alloy materials, laser 3D printing technology cannot preheat the printed layer at high temperature, so it is not suitable for the processing of TiAl alloy materials. Electron beam melting (EBM) technology can achieve high-temperature preheating treatment in the processing chamber, which can inhibit the generation of cracks in TiAl alloys. The prepared TiAl alloy parts have the characteristics of fine grains and uniform organizational composition. It can effectively solve the disadvantages of coarse crystal structure, easy internal looseness and component segregation of traditional cast TiAl materials. It has the advantages of short production process and high production efficiency. Therefore, it is necessary to provide a method for manufacturing TiAl alloy blades using electron beam selective melting technology. Summary of the invention

[0004] In order to overcome the defects of the above-mentioned prior art, the purpose of the present invention is to provide a TiAl alloy blade and an additive manufacturing method thereof, by adopting additive design and electron beam 3D printing method to quickly and efficiently prepare TiAl alloy blades, and through electromagnetic field in-situ assisted processing and post-processing process, obtain TiAl alloy blade parts with dimensional accuracy and surface finish within the permitted range.

[0005] To achieve the above object, the present invention provides the following technical solutions:

[0006] A method for manufacturing a TiAl alloy blade comprises the following steps:

[0007] Conduct additive manufacturing design and additive manufacturing process simulation analysis on the blade model;

[0008] The blade compensation model is obtained by performing anti-deformation compensation design on the blade model, and the additive manufacturing process simulation is continued on the blade compensation model to obtain the compensation optimization model of the blade;

[0009] Processing the posture optimization data, support generation data and slice data of the printed part according to the compensation optimization model and exporting the processed data;

[0010] Set 3D printing process parameters according to the processed data;

[0011] Wrap an electromagnetic field environment around the forming surface of the 3D printed part;

[0012] Performing 3D printing processing on the TiAl alloy blade under the 3D printing process parameters and electromagnetic field environment to obtain a blank;

[0013] The blank is post-processed to obtain a finished TiAl alloy blade.

[0014] Furthermore, the additive manufacturing design and additive manufacturing process simulation analysis of the blade model include:

[0015] By designing the blade processing allowance, selecting the 3D printer, setting the printing parameters, creating the substrate, optimizing the print part posture, support generation, slicing and printing processing and manufacturing, and designing the heat treatment process, the 3D printing process, the heat treatment process, the TiAl alloy blade separation process, and the overall and local deformation and stress cloud map of the TiAl alloy blade after the support of the TiAl alloy blade is removed are calculated and analyzed.

[0016] Furthermore, the blade model is designed for anti-deformation compensation and the additive manufacturing process is simulated to obtain a compensation optimization model of the blade, including:

[0017] Perform anti-deformation compensation design on the blade model to obtain a compensation model;

[0018] The additive manufacturing process is further simulated on the compensation model to calculate and verify that the overall and local deformation and stress distribution of the blade are within the preset range. After more than two iterative calculations, the compensation optimization model of the blade is obtained.

[0019] Further, a 3D printing process of a TiAl alloy blade is performed under the 3D printing process parameters and electromagnetic field environment to obtain a blank, comprising:

[0020] Control the vacuum degree of the processing chamber to ≤0.3Pa, set the slice thickness to 30-300μm, and set the scanning size of the substrate to 81-400cm 2 , set the preheating temperature to 1000-1300°C, set the number of preheating cycles to 3-9 times, and set the electron beam focusing current to 15-48 mA.

[0021] Further, the TiAl alloy blade is 3D printed under the 3D printing process parameters and electromagnetic field environment to obtain a blank, and further includes:

[0022] Whenever a layer of material is printed and the powder-laying phase begins, the electron beam is temporarily turned off and current is intermittently applied to the electromagnetic induction coil.

[0023] The parameters of loading current and voltage are: voltage 0.1~60kV, current 0.1~10 3 A, the current action time is 0.01~1s, the current pause time is 0~1s, when the current pause time is 0s, the current is a steady current, when the pause time is not 0s, the current is a pulse current.

[0024] Further, the TiAl alloy blade is 3D printed under the 3D printing process parameters and electromagnetic field environment to obtain a blank, and further includes:

[0025] The forming substrate material for 3D printing processing is martensitic stainless steel, titanium alloy or nickel-based high-temperature alloy.

[0026] Furthermore, the blank is post-processed to obtain a finished TiAl alloy blade, including:

[0027] Separating the blank from the substrate and recovering TiAl alloy powder on the surface of the blank and the substrate;

[0028] The part support of the blank is removed, and the blank is subjected to heat treatment, machining, and surface finishing to obtain a finished TiAl alloy blade.

[0029] Further, the heat treatment includes:

[0030] Use a vacuum heat treatment furnace or a hot isostatic pressing furnace to heat treat the blank, then cool it to room temperature in the furnace and take it out;

[0031] The process parameters of the heat treatment include: vacuum degree 5~20×10 -3 Pa, heating rate 15 ~ 25 ℃ / min, holding temperature 1150 ~ 1350 ℃, holding time 0.5 ~ 5h, cycle heat treatment times 0 ~ 5 times.

[0032] Furthermore, the surface finishing treatment includes:

[0033] The heat-treated blanks are polished by machining, manual grinding and polishing, magnetic polishing machine and vibration finishing equipment to reduce the roughness of the blanks to ≤Ra1.6μm;

[0034] The polished blank is finely polished using plasma polishing or abrasive flow process to reduce the roughness of the blank to ≤Ra0.1μm.

[0035] On the other hand, the present invention also discloses a TiAl alloy blade, which is prepared by the above method.

[0036] Technical effects and advantages of the present invention:

[0037] The present invention can activate the forming surface of the printed part by implementing electromagnetic field assisted treatment on the forming area during the electron beam 3D printing process, which helps the TiAl alloy molten pool to obtain electromagnetic field assisted effect, promotes the liquid phase flow in the molten pool to fill the pores, and forms a dense structure, which is beneficial to crushing grains, reducing anisotropy, and improving the comprehensive performance of the material; the present invention adopts additive design, blade model anti-deformation compensation design and electron beam 3D printing method to quickly and efficiently prepare TiAl alloy blades, and through post-processing technology, obtains TiAl alloy blade parts with dimensional accuracy and surface finish within the permitted range; the TiAl alloy blade prepared by this method has the advantages of high part dimensional accuracy, good surface roughness, excellent performance, short production cycle and high material utilization rate.

[0038] Other features and advantages of the present invention will be described in the following description, and partly become apparent from the description, or understood by practicing the present invention. The purpose and other advantages of the present invention can be realized and obtained by the structures pointed out in the description, claims and drawings. BRIEF DESCRIPTION OF THE DRAWINGS

[0039] Figure 1 The present invention is a flow chart of a method for manufacturing a TiAl alloy blade. DETAILED DESCRIPTION

[0040] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0041] Figure 1 FIG. 1 is a flow chart of a method for manufacturing a TiAl alloy blade according to the present invention, as shown in FIG. Figure 1 As shown, the present invention provides an additive manufacturing method for a TiAl alloy blade, comprising:

[0042] Conduct additive manufacturing design and additive manufacturing process simulation analysis on the blade model;

[0043] Perform anti-deformation compensation design on the blade model to obtain a blade compensation model, and then perform additive manufacturing process simulation on the blade compensation model to obtain a blade compensation optimization model;

[0044] Using the compensation optimization model to process data before printing;

[0045] Set 3D printing process parameters according to the processed data;

[0046] Wrap an electromagnetic field environment around the forming surface of the 3D printed part;

[0047] Performing 3D printing processing on the TiAl alloy blade under the 3D printing process parameters and electromagnetic field environment to obtain a blank;

[0048] The blank is post-processed to obtain a finished TiAl alloy blade.

[0049] Furthermore, the additive manufacturing design and additive manufacturing process simulation analysis of the blade model include:

[0050] By designing the blade processing allowance, selecting the 3D printer, setting the printing parameters, creating the substrate, optimizing the print posture, support generation, slicing and printing processing and manufacturing, and designing the heat treatment process, the 3D printing process, the heat treatment process, the TiAl alloy blade detaching from the substrate, and the TiAl alloy blade after the support is removed, the overall and local deformation and stress cloud diagram of the TiAl alloy blade are calculated and analyzed.

[0051] Further, an anti-deformation compensation design is performed on the blade model to obtain a compensation model;

[0052] The additive manufacturing process simulation is continued for the compensation model to calculate and verify that the overall and local deformation and stress distribution of the blade are within a preset range. After more than two iterative calculations, the compensation optimization model of the blade is obtained.

[0053] Furthermore, the posture optimization data, support generation data and slicing data of the printed part are processed according to the compensation optimization model and the processed data are exported.

[0054] Furthermore, when the TiAl alloy blade is 3D printed, the vacuum degree of the processing chamber is controlled to be ≤0.3Pa, the slice thickness is set to 30-300μm, and the scanning size of the substrate is set to 81-400cm 2 , set the preheating temperature to 1000-1300°C, set the number of preheating cycles to 3-9 times, and set the electron beam focusing current to 15-48 mA.

[0055] Furthermore, every time a layer of material is printed and the powder spreading stage begins, the electron beam is temporarily turned off and current is intermittently applied to the induction coil; the parameters of the applied current and voltage are: voltage 0.1~60kV, current 0.1~10 3 A, the current action time is 0.01~1s, and the current pause time is 0~1s. When the current pause time is 0s, the current is a steady current. When the pause is not 0s, the current is a pulse current. According to the principle of electromagnetic induction, the conductive coil will generate a magnetic field at the same time. The magnetic field has a stirring effect on the liquid metal in the molten pool. In the process of electron beam 3D printing, electromagnetic field-assisted treatment is implemented in the forming area, which can activate the forming surface of the printed part, help the TiAl alloy molten pool to obtain electromagnetic field-assisted effect, and promote the liquid phase in the molten pool in the printing area to flow at a faster speed to fill the pores and form a dense material structure, which is beneficial to break the grains, reduce anisotropy, and improve the comprehensive performance of the material.

[0056] Furthermore, the forming substrate processed by 3D printing is made of martensitic stainless steel, titanium alloy or nickel-based high-temperature alloy.

[0057] Furthermore, when the blank is post-processed, the blank is separated from the substrate and the TiAl alloy powder on the surface of the blank and the substrate is recovered; the part support of the blank is removed, and the blank is heat treated, machined and surface finished to obtain a finished TiAl alloy blade.

[0058] Furthermore, when the blank is heat treated, a vacuum heat treatment furnace or a hot isostatic pressing furnace is used to heat treat the blank, and then the blank is cooled to room temperature with the furnace and taken out; the process parameters of the heat treatment include: vacuum degree 5 to 20×10 - 3 Pa, heating rate 15-25°C / min, holding temperature 1150-1350°C, holding time 0.5-5h, number of cyclic heat treatment 0-5 times; the microstructure of the TiAl alloy is adjusted by heat treating the billet.

[0059] Furthermore, when the surface of the heat-treated blank is polished, machining, manual grinding and polishing, magnetic polishing machine, and vibration finishing equipment are used to polish the blank, which can reduce the roughness of the blank to ≤Ra1.6μm; plasma polishing or abrasive flow process is used to fine-polish the polished blank, which can reduce the roughness of the blank to ≤Ra0.1μm. The processing and polishing accuracy are selected according to the dimensional accuracy and surface finish requirements of the product.

[0060] On the other hand, the present invention further discloses a TiAl alloy blade, which is manufactured by the above method, and the materials of the TiAl alloy blade include Ti45Al8Nb, Ti48Al2Nb2Cr and Ti48Al4Nb2Cr.

[0061] Example

[0062] S1: The blade model was designed using UG NX12 3D model design software, with a size of 19.5×30×55mm. The additive manufacturing simulation software 3D EXPERIENCE was used to perform additive manufacturing design and process simulation analysis on the blade model. By designing the blade machining allowance of 0.5-2.5mm, selecting the 3D printer, setting the printing parameters, creating a substrate of 150×150×10mm, optimizing the print part posture, support generation, slicing and printing manufacturing, and designing the heat treatment process, the 3D printing process, the heat treatment process, the TiAl alloy blade separated from the substrate, and the TiAl alloy blade after the support was removed, the overall and local deformation and stress cloud of the TiAl alloy blade were calculated and analyzed.

[0063] S2: Design the blade model for anti-deformation compensation, obtain the compensation model, and import the compensation model into the simulation software, continue to simulate the additive manufacturing process, and calculate and verify that the overall and local deformation and stress distribution of the compensation model are within the permitted range. After no less than two iterative calculations, the compensation optimization model is finally obtained, and the parameters required for additive manufacturing are determined, including setting the placement of the three-dimensional model to the vertical placement of the blade, adding a contour support structure, and determining the electron beam 3D printing process parameters: the powder uses Ti45Al8Nb alloy spherical powder, the preheating temperature is 1000-1300℃, the beam spot current is 10-48mA, the beam spot diameter is 10-150mA, and the beam spot scanning speed is 1000-7000m / s, and the compensation optimization model file in stl format is exported.

[0064] S3. Input the blade compensation optimization model stl file into the 3D printer control software Build Assembler, process the print part posture optimization data, support generation data and slice data, and export the processed data. The format of the exported data is abf.

[0065] S4. Input the exported abf data into the 3D printer control software EBM Control to implement 3D printing process parameter settings.

[0066] S5. Load 30-100 kg of Ti45Al8Nb alloy powder into the powder storage bin of the 3D printer. The particle size distribution of the Ti45Al8Nb alloy powder is 45-150 μm, and the fluidity is 30 s / 50 g, completing the preparation state of the electron beam 3D printer.

[0067] S6. Start the 3D printing process of the TiAl alloy blade. At the same time, turn on the electromagnetic induction coil current around the forming plane. The parameters are: voltage 300V, current 100A, current action time 0.5s, current pause time 0.25s, to create an electromagnetic field environment that wraps the printed forming surface. When the printer completes printing a layer of material, it enters the powder spreading stage. At this time, the electron beam is temporarily turned off. At this time, current can be intermittently loaded to the induction coil. Powder spreading and electron beam printing are performed alternately until the entire printing task is completed, and the current loading to the induction coil is stopped.

[0068] S7. After the blank is formed by 3D printing, the substrate, powder and blank assembly are taken out from the printer and placed together in a powder-specific recovery system to blow and recover the Ti45Al8Nb alloy powder so that the blank is separated from the substrate and powder.

[0069] S8, remove the support, put the blank into the hot isostatic pressing furnace and high vacuum heat treatment furnace for treatment, the vacuum degree of the heat treatment process is 5×10 -3 Pa, heating rate is 15℃ / min, holding temperature is 1150℃, holding time is 1h, cycle heat treatment times are 2 times, then cool to room temperature with the furnace, take out the blank. The blank after heat treatment is milled by machining method, and the surface roughness of the blade after machining can reach Ra1.6μm, and TiAl alloy blade parts with dimensional accuracy and surface finish within the permitted range are obtained.

[0070] After testing, the test rod prepared by the same process as the TiAl alloy blade, according to the GB / T228.1-2010 testing standard, the room temperature fracture strength of the test rod reached 670-770MPa, and the elongation reached 2.5-3.5%; the fracture strength of the test rod at 750°C reached 740-840MPa, and the elongation reached 16-18%; the fracture strength of the test rod at 800°C reached 810-910MPa, and the elongation reached 44-46%; therefore, the performance of the TiAl alloy blade prepared by this method is greatly improved.

[0071] Finally, it should be noted that the above is only a preferred embodiment of the present invention and is not intended to limit the present invention. Although the present invention has been described in detail with reference to the aforementioned embodiments, it is still possible for those skilled in the art to modify the technical solutions described in the aforementioned embodiments or to make equivalent substitutions for some of the technical features therein. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. A method for manufacturing a TiAl alloy blade, characterized in that: The method comprises the following steps: Conduct additive manufacturing design and additive manufacturing process simulation analysis on the blade model; Performing anti-deformation compensation design on the blade model to obtain a blade compensation model, and further performing additive manufacturing process simulation on the blade compensation model to obtain a compensation optimization model of the blade; Processing the posture optimization data, support generation data and slice data of the printed part according to the compensation optimization model and exporting the processed data; Set 3D printing process parameters according to the processed data; Wrap an electromagnetic field environment around the forming surface of the 3D printed part; Performing 3D printing processing on a TiAl alloy blade under the 3D printing process parameters and electromagnetic field environment to obtain a blank; Post-processing the blank to obtain a finished TiAl alloy blade; The additive manufacturing design and additive manufacturing process simulation analysis of the blade model include: By designing the blade processing allowance, selecting the 3D printer, setting the printing parameters, creating the substrate, optimizing the print part posture, support generation, slicing and printing processing and manufacturing, and designing the heat treatment process, the 3D printing process, the heat treatment process, the process of TiAl alloy blades separating from the substrate, and the overall and local deformation and stress cloud diagram of the TiAl alloy blade after the support is removed; The method of performing anti-deformation compensation design on the blade model and continuing to simulate the additive manufacturing process to obtain a compensation optimization model of the blade includes: Performing anti-deformation compensation design on the blade model to obtain a compensation model; The additive manufacturing process simulation is continued for the compensation model, and the overall and local deformation and stress distribution of the blade are calculated and verified to be within a preset range. After more than two iterative calculations, a compensation optimization model of the blade is obtained; The 3D printing process of the TiAl alloy blade is performed under the 3D printing process parameters and electromagnetic field environment to obtain a blank, and further includes: Whenever a layer of material is printed and the powder-laying phase begins, the electron beam is temporarily turned off and current is intermittently applied to the electromagnetic induction coil. The parameters of loading current and voltage are: voltage 0.1~60kV, current 0.1~10 3 A, the current action time is 0.01~1s, the current pause time is 0~1s, when the current pause time is 0s, the current is a steady current, when the pause time is not 0s, the current is a pulse current; The process of post-processing the blank to obtain a finished TiAl alloy blade comprises: Separating the blank from the substrate and recovering TiAl alloy powder on the surface of the blank and the substrate; Removing the part support of the blank, and subjecting the blank to heat treatment, machining, and surface finishing to obtain a finished TiAl alloy blade; The heat treatment comprises: Use a vacuum heat treatment furnace or a hot isostatic pressing furnace to heat treat the blank, then cool it to room temperature in the furnace and take it out; The process parameters of the heat treatment include: vacuum degree 5~20×10 -3 Pa, heating rate 15 ~ 25 ℃ / min, holding temperature 1150 ~ 1350 ℃, holding time 0.5 ~ 5h, cycle heat treatment times 0 ~ 5 times.

2. The method for manufacturing a TiAl alloy blade according to claim 1, characterized in that: The 3D printing process of the TiAl alloy blade is performed under the 3D printing process parameters and electromagnetic field environment to obtain a blank, comprising: Control the vacuum degree of the processing chamber to ≤0.3Pa, set the slice thickness to 30-300μm, and set the scanning size of the substrate to 81-400cm 2 , set the preheating temperature to 1000-1300°C, set the number of preheating cycles to 3-9 times, and set the electron beam focusing current to 15-48 mA.

3. The method for manufacturing a TiAl alloy blade according to claim 1, characterized in that: The 3D printing process of the TiAl alloy blade is performed under the 3D printing process parameters and electromagnetic field environment to obtain a blank, and further includes: The material of the forming substrate processed by 3D printing is martensitic stainless steel, titanium alloy or nickel-based high-temperature alloy.

4. The method for manufacturing a TiAl alloy blade according to claim 1, characterized in that: The surface finishing treatment comprises: The heat-treated blanks are polished by machining, manual grinding and polishing, magnetic polishing machine and vibration finishing equipment to reduce the roughness of the blanks to ≤Ra1.6μm; The polished blank is finely polished using plasma polishing or abrasive flow process to reduce the roughness of the blank to ≤Ra0.1μm.