A polyamide composition and its preparation method and application

By adding specific layered mica powder and polyamide resin to the polyamide composition, the problem of jet-print defects during injection molding is solved, which significantly improves the melt flow stability and enhances the anti-jet thread ability, especially in The effect is significant under high filler content.

CN115746545BActive Publication Date: 2024-12-03KINGFA SCI & TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211391315.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-11-08
Publication Date
2024-12-03
Estimated Expiration
2042-11-08

AI Technical Summary

Technical Problem

Polyamide is prone to spray mark defects during injection molding, especially in places where the wall thickness suddenly becomes thinner, resulting in the melt solidification to form snake-shaped traces. The problem is more obvious, especially when the content of inorganic fillers is high, and existing solutions exist. limitation.

Method used

By adding a specific amount of layered mica powder to the polyamide composition, the diameter-thickness ratio is between 50:1 and 90:1, the number of mesh is ≥200 mesh, combining a specific type of polyamide resin and other fillers, using a twin screw Extruder extrusion and granulation are prepared to produce a polyamide composition with improved melt flow stability.

Benefits of technology

It significantly improves the flow stability of the melt during injection molding and suppresses the appearance defects of the spray marks. Especially in the case of high filler content, the test results show that the L value is ≥110mm, preferably the L value ≥160mm, which enhances the material's anti-jet marks. ability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115746545B_ABST
    Figure CN115746545B_ABST
Patent Text Reader

Abstract

A polyamide composition comprises the following components by weight: 60 parts of polyamide resin; 0-60 parts of inorganic filler; 5-40 parts of layered mica powder; the mica powder is a layered structure, with a diameter-to-thickness ratio of 50:1-90:1, and a mesh size of ≥200 meshes. The present invention can significantly improve the defects of the appearance of spray marks generated during the injection molding process, especially when a large amount of fillers are contained, by adding a specific amount of layered mica powder with a specific structure to the polyamide composition.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] A polyamide composition and its preparation method and application Background Art

[0002] Polyamide has excellent mechanical properties and molding processability, and is widely used in the automotive, construction, electronic and electrical appliances, and home appliances industries. However, due to the generally low molecular weight of polycondensates such as polyamide, the result is good processing fluidity but easy to appear jetting marks in the place where the wall thickness of the injection mold becomes thinner. The so-called jetting mark refers to the trace of the polymer melt flowing in the direction of the injection molded part, which is like a snake bending. Under normal circumstances, the polymer melt fills the mold in a "fountain flow" manner along the inner wall of the mold to stably fill the mold, but when the melt passes through the gate at high speed, or the melt suddenly turns from a thick wall to a thin wall, the melt will be sprayed into the cavity in a "jet" manner, forming a folded material strip, and the subsequent melt will stably fill the entire cavity. Because the previously sprayed folded material strip first hits the cooled cavity wall and solidifies, it cannot be integrated with the subsequent stable filling melt, and a serpentine mark appears. Especially when the content of inorganic fillers is high, the jetting mark defect is more obvious.

[0003] At present, there are two ways to solve the spray mark: 1) In product design, use a gradual transition wall thickness instead of a sudden wall thickness change; 2) In mold design, try to avoid opening the gate at one end of the wall thickness, or design a baffle structure to block the spray; 3) In terms of process, adopt a slow injection molding process; 4) In terms of materials, choose polymers with high molecular weight and high melt viscosity. However, the above methods are both practical and have certain limitations. For example, 1) due to the actual use requirements, product design cannot avoid the structural design of sudden changes in wall thickness; method 2) due to the mold structure, sometimes the gate cannot be moved to the appropriate position; method 3) sometimes the process loses one thing while focusing on another and cannot be improved; method 4) sometimes due to the existing synthesis process level, the molecular weight or viscosity of the polymer cannot be further increased. Summary of the invention

[0004] The above technical defects are overcome, and a polyamide composition having significantly improved appearance defects of spray marks and a preparation method and application thereof are provided.

[0005] The present invention is achieved through the following technical solutions:

[0006] A polyamide composition, comprising the following components in parts by weight:

[0007] 60 parts of polyamide resin;

[0008] Inorganic filler 0-60 parts;

[0009] 5-40 parts of layered mica powder;

[0010] The layered mica powder has a layered structure, a diameter-to-thickness ratio of 50:1-90:1, and a mesh size of ≥200 meshes.

[0011] Preferably, the diameter-to-thickness ratio of the layered mica powder is between 60:1 and 80:1.

[0012] Preferably, the content of the layered mica powder is 12-20 parts.

[0013] Layered mica powder is the refined product of mica powder. Through refined processing, each layer of mica powder is peeled off to achieve the corresponding diameter-to-thickness ratio and mesh number.

[0014] The polyamide resin suitable for the technical solution of the present invention is selected from at least one of aliphatic polyamide resins and semi-aromatic polyamide resins; the aliphatic polyamide resin is selected from at least one of PA66, PA610, PA612, PA1010, PA106, PA1212, PA46, MXD6, PA92, PA102, PA6, PA7, PA11, PA12, and PA13; the semi-aromatic polyamide resin is selected from at least one of PA9T, PA10T, PA11T, PA12T, PA13T, PA6T / MT, PA6T / 6I, PA6T / 66, and PA66 / 6T; preferably PA66, PA610, and PA6T / 66.

[0015] The relative viscosity of the polyamide resin is 2-3, and the testing standard is GB / T 12006.1-2009.

[0016] The other fillers are selected from at least one of glass fiber, talc, calcium carbonate, titanium dioxide, glass microbeads, carbon fiber, graphene, and wollastonite.

[0017] Whether to add 0-2 parts of at least one of an antioxidant and a lubricant can be selected according to actual needs.

[0018] The antioxidant may be: 1,3,5-trimethyl-2,4,6-tris(3,5-di-tert-butyl-4-hydroxybenzyl)benzene; 2,5-di-tert-butyl-4-hydroxybenzyl dimethylamine; diethyl-3,5-di-tert-butyl-4-hydroxybenzyl phosphate; stearyl-3,5-di-tert-butyl-4-hydroxybenzyl phosphate; 3,5-di-tert-butyl-4-hydroxyphenyl-3,5-distearyl-thiotriazolylamine; 2,6-di-tert-butyl-4-hydroxymethylphenol; 2,4-di-(n-octylthio)-6-(4-hydroxy-3,5-di-tert-butylglycerol allyl ether)-1,3,5-triazine; N,N'-hexamethylenebis( 3,5-di-tert-butyl-4-hydroxy-hydrocinnamic acid); N,N'-bis-(3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionyl)hexanediamine; octadecyl-3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate; pentaerythritol-tetrakis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate]; triethylene glycol-bis[3-(3,5-dimethyl-4-hydroxyphenyl)propionate]; triethylene glycol bis[β-(3-tert-butyl-4-hydroxy-5-methylphenyl)propionate]; 2,2'-thiodiethyl-bis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate, etc.

[0019] The lubricant may be: at least one of stearate lubricants, fatty acid lubricants, and stearate ester lubricants; the stearate lubricant is selected from at least one of calcium stearate, magnesium stearate, and zinc stearate; the fatty acid lubricant is selected from at least one of fatty acids, fatty acid derivatives, and fatty acid esters; the stearate ester lubricant is selected from at least one of pentaerythritol stearate.

[0020] The preparation method of the polyamide composition of the present invention comprises the following steps: uniformly mixing the components, extruding and granulating through a twin-screw extruder, setting the temperature range of the 1-8 zones of the screw extruder to 180-230° C. and the rotation speed range to 300-500 rpm to obtain the polyamide composition.

[0021] The polyamide composition of the present invention is used for preparing parts requiring good appearance, such as housings of electronic appliances.

[0022] The present invention has the following beneficial effects:

[0023] Jet marks are caused by unstable flow of the melt during the injection molding process. The present invention can significantly improve the melt flow stability during the injection molding process by adding a specific amount of layered mica powder with a specific geometric structure (within a specific diameter-to-thickness ratio and mesh number range) to the polyamide composition, thereby suppressing the appearance defects of the jet marks generated during the injection molding process, especially when a large amount of fillers are contained (through the test and evaluation of the jet marks of the present invention, the polyamide composition of the present invention has an L value ≥110mm, preferably an L value ≥160mm). BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1 : Spray pattern evaluation mold. DETAILED DESCRIPTION

[0025] The present invention is described in detail below in conjunction with specific embodiments. The following embodiments will help those skilled in the art to further understand the present invention, but are not intended to limit the present invention in any form. It should be noted that, for those of ordinary skill in the art, several variations and improvements may be made without departing from the concept of the present invention. These all belong to the protection scope of the present invention.

[0026] The sources of experimental raw materials used in the present invention are as follows:

[0027] PA6-1: HY-2800A, relative viscosity 2.7, Haiyang Chemical Fiber Group;

[0028] PA6-2: HY-2000A, relative viscosity 2.0, Haiyang Chemical Fiber Group;

[0029] PA6-3: PA6 VOLGAMID F34, relative viscosity 3.4, Kuibyshev nitrogen;

[0030] PA 66: EP-158, relative viscosity 2.7, Huafeng Group;

[0031] PA 610:3 RILSAN SMNO F, relative viscosity 2.7, ARKEMA;

[0032] PA 6T / 66: Selar PA3426, relative viscosity 2.7, DUPONT;

[0033] Mica powder Mesh Diameter-thickness ratio Brand factory A 400 60:1 Suzorite 200-S IMERYS B 200 80:1 Suzorite 325-S IMERYS C 600 65:1 Suzorite150-NY IMERYS D 400 50:1 4-K IMERYS E 300 90:1 WG-160 IMERYS F 150 50:1 C-3000 IMERYS G 500 40:1 1-K IMERYS H 400 100:1 Suzorite 60-S IMERYS

[0034] Ordinary non-laminated mica powder: PHM-20S0, IMERYS;

[0035] Chopped glass fiber: ECS-03-568H, Jushi Group;

[0036] Lubricant: stearate lubricant, lithium stearate, brand SAK-LIS-PE, SUN ACE KAKOH (PTE.) LTD., parallel tests using the same lubricant.

[0037] Preparation method of the polyamide composition of the embodiment and comparative example: the components are mixed uniformly, extruded and granulated by a twin-screw extruder, and the temperature range of the screw extruder 1-8 zones is set to 180-230° C. and the rotation speed range is 300-500 rpm to obtain a polyamide composition.

[0038] Test method for spray marks: To quantitatively evaluate the spray marks of material injection molding, the following is designed: Figure 1 The mold, (a) is the front view of the mold cavity, with scale lines inside, and the minimum scale is 10mm, (b) is the top view of the mold cavity. Spray mark evaluation method: Each time a group of samples are compared and evaluated, the same injection molding machine is used, and the same injection molding process parameters are used (it is recommended to use a high injection speed, which is 90% of the maximum injection speed of the machine. Spray marks are prone to occur at high speeds). The mold temperature is fixed at 80°C and cooled by circulating water. After the mold temperature stabilizes, the spray mark evaluation test begins. According to the internal scale value of the mold, the scale L where the spray phenomenon begins to occur is recorded (if it exceeds half of the minimum scale, it is counted as one scale, and if it is less than half of the minimum scale, it is omitted). Each sample is injected 10 times and the average value L is taken. The larger the L value, the stronger the material's ability to resist the occurrence of spray marks.

[0039] Table 1: Contents of components (parts by weight) and test results of polyamide compositions of Examples 1-7

[0040] Example 1 Example 2 Example 3 Example 4 Example 5 Example 6 Example 7 PA6-1 60 60 60 60 PA66 60 PA610 60 PA6T / 66 60 Mica powder types A A A A A A A Mica powder content 5 5 5 5 15 15 15 Chopped Glass Fiber 5 20 40 Lubricants 0.3 0.3 0.3 0.3 0.3 0.3 0.3 L value 11 15 17 14 18 17 16

[0041] It can be seen from Examples 1-7 that PA66, PA610, and PA6T66 are preferred to have stronger anti-jet mark capability; the content of inorganic filler also significantly affects the anti-jet mark capability.

[0042] Table 2: Content of each component (parts by weight) and test results of polyamide compositions of Examples 8-15

[0043] Example 8 Example 9 Example 10 Embodiment 11 Example 12 Embodiment 13 Embodiment 14 Embodiment 15 PA6-1 60 60 60 60 60 60 60 60 Mica powder types A A A A B C D E Mica powder content 12 15 20 40 15 15 15 15 Lubricants 0.3 0.3 0.3 0.3 0.3 0.3 0.3 0.3 L value 16 20 18 12 17 18 14 15

[0044] It can be seen from Examples 1 / 8-11 that the preferred content of the layered mica powder is 12-20 parts.

[0045] It can be seen from Examples 9 / 12-15 that the preferred diameter-to-thickness ratio of the layered mica powder is between 60:1 and 80:1.

[0046] Table 3: Content of each component (parts by weight) and test results of the polyamide composition of Examples 16-17

[0047] Example 16 Embodiment 17 PA6-2 60 PA6-3 60 Mica powder types A A Mica powder content 15 15 Lubricants 0.3 0.3 L value 19 20

[0048] Table 4: Content of each component (parts by weight) and test results of the polyamide compositions of Comparative Examples 1-7

[0049] Comparative Example 1 Comparative Example 2 Comparative Example 3 Comparative Example 4 Comparative Example 5 Comparative Example 6 Comparative Example 7 PA6 60 60 60 60 PA66 60 PA610 60 PA 6T / 66 60 Mica powder types A A Normal non-laminated Mica powder content 2 50 15 Chopped Glass Fiber 20 20 20 20 Lubricants 0.3 0.3 0.3 0.3 0.3 0.3 0.3 L value 6 5 4 6 8 5 3

[0050] It can be seen from Comparative Example 1 that the addition of specific mica powder can significantly inhibit the formation of jetting marks.

[0051] It can be further seen from Comparative Examples 2-4 that jetting patterns are more likely to occur when a large amount of chopped glass fibers are contained.

[0052] It can be seen from Comparative Examples 5 / 6 that when the mica powder content is too low, the effect of inhibiting jetting lines is not significant, while when the content is too high, the effect of inhibiting jetting lines is reduced.

[0053] It can be seen from Comparative Example 7 that the use of unrefined ordinary mica powder cannot achieve the effect of suppressing jetting marks.

[0054] Table 5: Content of each component (parts by weight) and test results of polyamide compositions of comparative examples 8-10

[0055] Comparative Example 8 Comparative Example 9 Comparative Example 10 PA6 60 60 60 Mica powder types F G H Mica powder content 15 15 15 Chopped Glass Fiber 20 20 20 Lubricants 0.3 0.3 0.3 L value 5 6 5

[0056] It can be seen from Comparative Examples 8-10 that when the aspect ratio and mesh number of the layered mica powder are not within the range of the present invention, the L value is also low.

Claims

1. A polyamide composition, characterized in that By weight, it includes the following components: 60 parts of polyamide resin; 5-40 parts of layered mica powder; Glass fiber 5-60 parts; The layered mica powder has a layered structure, a diameter-to-thickness ratio of 60:1-65:1, and a mesh size of 400-600 meshes; The polyamide resin is selected from at least one of PA66, PA610 and PA6T / 66.

2. The polyamide composition according to claim 1, characterized in that The content of the layered mica powder is 12-20 parts.

3. The polyamide composition according to claim 1, characterized in that The relative viscosity of the polyamide resin is 2-3.

4. The polyamide composition according to claim 1, characterized in that By weight, it also includes 0-2 parts of at least one of an antioxidant and a lubricant.

5. The method for preparing the polyamide composition according to any one of claims 1 to 4, characterized in that: The method comprises the following steps: uniformly mixing the components, extruding and granulating through a twin-screw extruder, setting the temperature range of the 1-8 zones of the screw extruder to be 180-230° C. and the rotation speed range to be 300-500 rpm, and obtaining a polyamide composition.