A method for activating a proton exchange membrane water electrolyzer
By passing deionized water into the anode side of the electrolytic cell and applying a load, operating different current density and voltage modes, the membrane electrode is activated, which solves the problem of increased resistance of the electrolytic cell and achieves the efficient performance of the membrane electrode.
Patent Information
- Application Number
- CN202211414729.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-11-11
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2042-11-11
AI Technical Summary
During the use of the electrolytic cell, the bonding between the catalyst layer and the proton exchange membrane is prone to deterioration, resulting in an increase in resistance, affecting the activity of the membrane electrode, and restricting the performance of the SPE electrolytic cell.
By passing deionized water at 80-100°C to the anode side of the electrolytic cell, the load is applied to run in constant current and constant voltage modes, then switching the constant current mode, performing a series of steps to activate the membrane electrode, and finally performing performance tests.
The ohmic impedance and material transport impedance are significantly reduced, allowing the proton exchange membrane water electrolytic cell to perform optimal performance.
Smart Images

Figure BDA0003939639850000041 
Figure BDA0003939639850000051
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of hydrogen production by water electrolysis, and in particular to an activation method for a proton exchange membrane water electrolyzer. Background Art
[0002] Hydrogen energy is a clean, efficient and renewable energy source. Replacing fossil energy with hydrogen energy is considered an effective way to solve the energy shortage and environmental pollution problems currently faced by the world. Water electrolysis is one of the most effective technologies for preparing high-purity hydrogen. Especially in combination with renewable energy power generation technology, it can not only effectively absorb "abandoned electricity" and has good economic efficiency, but also realize a cleaner way to produce hydrogen, and has broad application prospects. Solid polymer electrolyte electrolyzers have become a new generation of water electrolysis hydrogen production devices due to their advantages such as small size, compact structure, strong pressure resistance, large working current and high hydrogen production purity. The membrane electrode is the core of the electrolyzer, which consists of a proton exchange membrane and cathode and anode catalyst coating layers on both sides. During the hydrolysis process, water generates oxygen and hydrogen ions on the anode catalyst coating side of the membrane electrode, and the hydrogen ions are reduced to generate hydrogen through the proton exchange membrane on the cathode catalyst coating layer. Therefore, the membrane electrode is a key factor affecting the hydrolysis efficiency of the electrolyzer.
[0003] At present, electrolyzers are faced with the phenomenon that the bonding between the catalyst layer and the proton exchange membrane is easily deteriorated during activation or use, which increases the resistance, affects the activity of the membrane electrode, and restricts the performance of the SPE electrolyzer. Summary of the invention
[0004] In view of the problems existing in the background technology, the purpose of the present invention is to provide a proton exchange membrane water electrolyzer and an activation method thereof, which not only improves the preparation process of the membrane resistor, but also studies a targeted activation method to obtain an activation process with excellent effect.
[0005] In order to achieve the above-mentioned object, in the first aspect, the present invention provides a method for activating a proton exchange membrane water electrolyzer, comprising the following steps: (1) introducing deionized water at a temperature of 80-100° C. and a flow rate of 100-300 mL / min into the anode side of the electrolyzer; (2) applying a load to the electrolyzer, firstly in a constant current mode, running 3-6 working steps with a current density range of 1-7 A / cm 2 , time 0.5-2h; (3) then run 1-5 working steps in constant voltage mode, voltage range 1-3V, time 10-60min; (4) finally switch to constant current mode, 1-3A / cm 2 Run at the current density for 10-60 minutes; (5) After the activation step is completed, remove the load and leave it for about 10 minutes for performance testing.
[0006] Optionally, the electrolytic cell includes: a membrane electrode, an insulating plate, a guide plate, an external power supply and a water supply device; the anode side of the membrane electrode includes, from the inside to the outside, an anode gas diffusion layer, an anode guide plate and a cathode insulating plate, and the cathode side of the membrane electrode includes, from the inside to the outside, a cathode gas diffusion layer, a cathode guide plate and a cathode insulating plate; the positive and negative poles of the external power supply are respectively connected to the anode guide plate and the cathode guide plate; the water supply device is used to introduce deionized water into the anode side of the electrolytic cell; the anode gas diffusion layer is a titanium mesh, and the cathode gas diffusion layer is carbon paper.
[0007] The beneficial effects of the present invention are as follows:
[0008] The activation method of the present invention can construct transmission channels for protons, electrons, water and gas to a large extent, reduce ohmic impedance and material transmission impedance, and enable the proton exchange membrane water electrolyzer to exert optimal performance. DETAILED DESCRIPTION
[0009] In order to make the above-mentioned objects, features and advantages of the invention more obvious and easy to understand, the specific embodiments of the invention are described in detail below.
[0010] In the following description, many specific details are set forth to facilitate a full understanding of the present invention, but the present invention may also be implemented in other ways different from those described herein, and those skilled in the art may make similar generalizations without violating the connotation of the present invention. Therefore, the present invention is not limited to the specific embodiments disclosed below.
[0011] The activation method of the proton exchange membrane water electrolyzer according to the present invention comprises the following steps: (1) introducing deionized water at 80-100° C. and a flow rate of 100-300 mL / min into the anode side of the electrolyzer; (2) applying a load to the electrolyzer, firstly in a constant current mode, running 3-6 working steps with a current density range of 1-7 A / cm 2 , time 0.5-2h; (3) then run 1-5 working steps in constant voltage mode, voltage range 1-3V, time 10-60min; (4) finally switch to constant current mode, 1-3A / cm 2 Run at the current density for 10-60 minutes; (5) After the activation step is completed, remove the load and leave it for about 10 minutes for performance testing.
[0012] The electrolytic cell comprises: a membrane electrode, an insulating plate, a guide plate, an external power supply and a water supply device; the anode side of the membrane electrode comprises an anode gas diffusion layer, an anode guide plate and a cathode insulating plate from the inside to the outside, and the cathode side of the membrane electrode comprises a cathode gas diffusion layer, a cathode guide plate and a cathode insulating plate from the inside to the outside; the positive and negative electrodes of the external power supply are respectively connected to the anode guide plate and the cathode guide plate; the water supply device is used to pass deionized water into the anode side of the electrolytic cell; the anode gas diffusion layer is a titanium mesh, and the cathode gas diffusion layer is a carbon paper.
[0013] The membrane electrode of the present invention is described in detail below in conjunction with a specific embodiment, wherein the specific structure of the proton exchange membrane water electrolyzer composed thereof includes: a membrane electrode, an insulating plate, a guide plate, an external power supply and a water supply device; the anode side of the membrane electrode is sequentially an anode gas diffusion layer, an anode guide plate and a cathode insulating plate from the inside to the outside, and the cathode side of the membrane electrode is sequentially a cathode gas diffusion layer, a cathode guide plate and a cathode insulating plate from the inside to the outside; the positive and negative electrodes of the external power supply are respectively connected to the anode guide plate and the cathode guide plate; the water supply device is for passing deionized water into the anode side of the electrolyzer; the anode gas diffusion layer is a titanium mesh, and the cathode gas diffusion layer is a carbon paper. Except for the membrane electrode, the specific models of the above structure are available on the market, and the electrolyzer is assembled by oneself.
[0014] The process of preparing membrane electrode is as follows:
[0015] 1. Preparation of surface biomimetic proton exchange membrane
[0016] (1) The stripe structure of the bionic foxtail grass leaf is processed on the aluminum alloy substrate by using the electric spark precision machining technology to obtain the aluminum alloy template, and the polydimethylsiloxane glue is poured, degassed, and solidified to obtain the silicone reverse template;
[0017] (2) preparing a perfluorosulfonic acid resin solution with a mass concentration of 35% having a terminal -SO3Na, adding tetrabutylammonium and dopamine intercalation-modified montmorillonite, stirring evenly, introducing an inert gas into an autoclave, maintaining a pressure range of 1.8 MPa and a temperature of 130°C, keeping the temperature for 6 hours, and then cooling naturally to obtain a perfluorosulfonic acid resin solution doped with tetrabutylammonium and dopamine intercalation-modified montmorillonite; the weight volume ratio of the tetrabutylammonium and dopamine intercalation-modified montmorillonite to the terminal -SO3Na perfluorosulfonic acid resin aqueous solution is 18 g / L; the solvent of the perfluorosulfonic acid resin solution is composed of water and ethanol, with a mass ratio of 20:30;
[0018] (3) The perfluorosulfonic acid resin solution described in step (2) is applied to the surface of the silica gel counter template described in step (1), heated to 110° C., dried for 1.5 h, and separated from the template after natural cooling to obtain a surface biomimetic proton exchange membrane with a thickness of 80 μm.
[0019] 2. Preparation of membrane electrode
[0020] (1) treating the surface of the surface biomimetic proton exchange membrane with a dopamine hydrochloride solution, spraying a 2 mg / mL dopamine hydrochloride solution onto the surface of the surface biomimetic proton exchange membrane, and drying at 105° C. for 3 h to obtain a modified surface biomimetic proton exchange membrane;
[0021] (2) mixing iridium oxide and perfluorosulfonic acid resin solution to form an anode catalyst slurry with a concentration of 30 wt %; mixing Pt / C and perfluorosulfonic acid resin solution to form a cathode catalyst slurry with a concentration of 35 wt %;
[0022] (3) Spraying the cathode catalyst slurry described in step (2) on the cathode side of the modified surface biomimetic proton exchange membrane, and obtaining a cathode catalyst layer with a thickness of 80 μm after drying; spraying the anode catalyst slurry described in step (2) on the anode side of the modified surface biomimetic proton exchange membrane, and obtaining an anode catalyst layer with a thickness of 80 μm after drying, and finally obtaining a water electrolysis membrane electrode.
[0023] Example
[0024] The activation method of the proton exchange membrane water electrolyzer provided in the embodiment comprises the following steps:
[0025] (1) introducing deionized water at 80-100° C. and a flow rate of 100-300 mL / min into the anode side of the electrolytic cell;
[0026] (2) Apply a load to the electrolytic cell, first run 3-6 working steps in constant current mode, with a current density range of 1-7A / cm 2 , time 0.5-2h;
[0027] (3) Then, run 1 to 5 working steps in constant voltage mode, with a voltage range of 1 to 3 V and a time of 10 to 60 min;
[0028] (4) Finally switch to constant current mode, 1-3A / cm 2 Run at current density for 10-60min;
[0029] (5) After the activation step is completed, remove the load and let it sit for about 10 minutes for performance testing.
[0030] The specific process is shown in Table 1.
[0031] Table 1
[0032]
[0033]
[0034] Performance Testing
[0035] The performance before and after activation was tested, wherein the test conditions were as follows: the test conditions were 1.5V applied voltage frequency 0.01-10000Hz, amplitude 0.01mV, and the ohmic impedance was calculated based on numerical values such as cell voltage and circuit density to obtain the performance effect of the membrane electrode on the electrolyzer.
[0036] The performance test results of the products obtained in the above examples are shown in Table 2.
[0037] Table 2
[0038] Test items Ohm resistance (before activation) Ohm resistance (after activation) Example 1 0.141 0.131 Example 2 0.141 0.128 Example 3 0.141 0.120
[0039] It can be seen from Table 2 that the activation method of the present invention can significantly reduce the ohmic impedance of the electrolytic cell, especially Example 3 has the best effect.
[0040] Although some specific embodiments of the present invention have been described in detail by way of example, it will be appreciated by those skilled in the art that the above examples are for illustration only and are not intended to limit the scope of the present invention. It will be appreciated by those skilled in the art that the above embodiments may be modified without departing from the scope and spirit of the present invention. The scope of the present invention is defined by the appended claims.
Claims
1. A method for activating a proton exchange membrane water electrolyzer, characterized in that: The steps include: (1) introducing deionized water at 80-100°C at a flow rate of 100-300 mL / min into the anode side of the electrolytic cell; (2) Apply a load to the electrolytic cell. First, run 3-6 working steps in constant current mode with a current density range of 1-7 A / cm 2 , time 0.5-2h; (3) Then run 1-5 working steps in constant voltage mode, with a voltage range of 1-3 V and a time of 10-60 min; (4) Finally switch to constant current mode, 1-3A / cm 2 Run at current density for 10-60min; (5) After the activation step is completed, remove the load and let it sit for 10 minutes for performance testing; The electrolytic cell comprises: a membrane electrode, an insulating plate, a guide plate, an external power supply and a water supply device; the anode side of the membrane electrode comprises an anode gas diffusion layer, an anode guide plate and an anode insulating plate from the inside to the outside, and the cathode side of the membrane electrode comprises a cathode gas diffusion layer, a cathode guide plate and a cathode insulating plate from the inside to the outside; the positive and negative electrodes of the external power supply are respectively connected to the anode guide plate and the cathode guide plate; the water supply device is used to pass deionized water into the anode side of the electrolytic cell; the anode gas diffusion layer is a titanium mesh, and the cathode gas diffusion layer is a carbon paper; The preparation process of the membrane electrode is as follows: (1) treating the surface of the surface biomimetic proton exchange membrane with a dopamine hydrochloride solution, spraying a 2 mg / mL dopamine hydrochloride solution onto the surface of the surface biomimetic proton exchange membrane, and drying at 105° C. for 3 h to obtain a modified surface biomimetic proton exchange membrane; (2) Mixing iridium oxide and perfluorosulfonic acid resin solution to form an anode catalyst slurry with a concentration of 30wt%; mixing Pt / C and perfluorosulfonic acid resin solution to form a cathode catalyst slurry with a concentration of 35wt%; (3) spraying the cathode catalyst slurry described in step (2) on the cathode side of the modified surface biomimetic proton exchange membrane, and obtaining a cathode catalyst layer with a thickness of 80 μm after drying; spraying the anode catalyst slurry described in step (2) on the anode side of the modified surface biomimetic proton exchange membrane, and obtaining an anode catalyst layer with a thickness of 80 μm after drying, and finally obtaining a water electrolysis membrane electrode; The preparation process of the surface biomimetic proton exchange membrane is as follows: (1) The striped structure of the bionic foxtail grass leaf was machined on the aluminum alloy substrate by using the electric spark precision machining technology to obtain the aluminum alloy template, and the polydimethylsiloxane glue was poured, degassed, and solidified to obtain the silicone reverse template; (2) preparing a perfluorosulfonic acid resin solution with a mass concentration of 35% having a terminal -SO3Na, adding tetrabutylammonium and dopamine intercalated modified montmorillonite, stirring evenly, introducing an inert gas into an autoclave, maintaining a pressure range of 1.8 MPa and a temperature of 130°C, keeping the temperature for 6 hours, and then cooling naturally to obtain a perfluorosulfonic acid resin solution doped with tetrabutylammonium and dopamine intercalated modified montmorillonite; the weight volume ratio of the tetrabutylammonium and dopamine intercalated modified montmorillonite to the terminal -SO3Na perfluorosulfonic acid resin aqueous solution is 18 g / L; the solvent of the perfluorosulfonic acid resin solution is composed of water and ethanol, with a mass ratio of 20:30; (3) The perfluorosulfonic acid resin solution described in step (2) is applied to the surface of the silica gel counter template described in step (1), heated to 110° C., dried for 1.5 h, and separated from the mold after natural cooling to obtain a surface biomimetic proton exchange membrane with a thickness of 80 μm.