Homogeneous epitaxial gan hemt device with trench filling dielectric isolation leakage and manufacturing method thereof

By etching grooves in GaN HEMT devices and filling them with high thermal conductivity materials to block parasitic leakage channels, the problems of dislocations and leakage in heteroepitaxial structures are solved, improving the breakdown voltage and output power of the devices and achieving better high-frequency characteristics and high-temperature applications.

CN115763533BActive Publication Date: 2026-11-10XIDIAN UNIV
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202211623684.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-12-16
Publication Date
2026-11-10
Estimated Expiration
2042-12-16

AI Technical Summary

Technical Problem

Existing GaN HEMT devices suffer from problems such as high-density dislocations, vertical leakage channels, parasitic leakage channels, poor material repeatability and consistency, and low thermal conductivity of self-supporting gallium nitride substrates in heteroepitaxial growth, which limit the breakdown voltage, output power and high-temperature applications of the devices.

Method used

The homoepitaxial GaN HEMT device structure employs a groove-filled dielectric to isolate leakage current. By etching a groove between the GaN substrate and the buffer layer and filling it with a high thermal conductivity material, the parasitic leakage current channel at the homoepitaxial interface is blocked. Furthermore, the source electrode is led to the back side of the substrate through a via, thereby reducing the parasitic capacitance of the device.

Benefits of technology

It improves the device's breakdown voltage, output power density, and high-frequency characteristics, enhances the device's heat dissipation efficiency and reliability, and is suitable for normal operation at higher temperatures.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115763533B_ABST
    Figure CN115763533B_ABST
Patent Text Reader

Abstract

This invention discloses a homoepitaxial GaN HEMT device with groove-filled dielectric isolation and its fabrication method, mainly solving the problem of interface leakage in existing homoepitaxial devices. From bottom to top, it includes a GaN substrate, a GaN buffer layer, a back barrier layer, a channel layer, an AlN insertion layer, a barrier layer, and an insulating gate dielectric. Ohmic contact regions are located on both sides of the AlN insertion layer and the barrier layer, with source and drain electrodes disposed on these regions. A gate electrode is disposed on the insulating gate dielectric. Grooves are formed on the GaN buffer layer and the GaN substrate, and both the grooves and the back side of the GaN substrate are filled and covered with a high thermal conductivity material as a leakage isolation layer. A via is provided below the ohmic contact region of the source electrode to the leakage isolation layer, and a back electrode is formed by depositing metal in the via and below the leakage isolation layer. This invention eliminates interface leakage, achieves high output current and power density, and has high heat dissipation efficiency, making it suitable for microwave power amplifiers and RF integrated circuit chips.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of semiconductor device technology, and specifically relates to a homoepitaxial GaN high electron mobility transistor (HEMT), which can be used to fabricate microwave power amplifiers and radio frequency integrated circuit chips. Background Technology

[0002] GaN, a third-generation wide-bandgap semiconductor material, has important applications in high-frequency, high-power, and high-efficiency solid-state microwave and millimeter-wave devices and power amplifiers, becoming a research hotspot and strategic competitive area in the field of microelectronic devices in recent years. GaN materials possess strong spontaneous polarization and piezoelectric polarization effects, and the high areal density and high mobility of the two-dimensional electron gas in its heterojunction materials are key to achieving efficient switching and high-frequency, high-power applications. As a mainstream device structure, GaN HEMTs have achieved commercial applications in broadband communication and information sensing fields after nearly thirty years of structural innovation and process improvement.

[0003] To further improve the operating frequency, output power, and efficiency of GaN HEMT devices, innovative device structure design, the application of new materials, and the development of device processes have become the main approaches to enhance device performance. Among these, epitaxy has evolved from heteroepitaxial growth to homoepitaxial growth on self-supporting gallium nitride substrates. When GaN HEMT devices are heteroepitaxially grown on Si, SiC, or sapphire substrates, the high density of dislocation defects in the material can cause vertical leakage current and reduced reliability. Furthermore, parasitic leakage channels at the homoepitaxial interface become the main factor limiting the breakdown voltage. Conventional GaN HEMT device structures are as follows: Figure 1 As shown, the structure from bottom to top consists of: substrate, nucleation layer, GaN buffer layer, channel layer, insertion layer, and barrier layer. A gate electrode is located on the barrier layer, and source and drain electrodes are located on the ohmic contacts of the source and drain regions, respectively. This device structure has the following drawbacks:

[0004] First, in the GaN buffer layer of heteroepitaxial layer, high-density dislocations caused by lattice mismatch will enter the active region of the device along the epitaxial direction of the material, scattering the carrier transport and forming a vertical leakage channel, which reduces the breakdown voltage of the device and degrades the reliability of the device.

[0005] Secondly, the heteroepitaxial GaN buffer layer requires a nucleation layer structure. The growth process, material quality, and thickness of this structure directly determine the crystal quality and transport characteristics of the GaN epitaxial material on it. The process control is difficult and the repeatability and consistency are poor.

[0006] Third, when using homoepitaxial GaN buffer layers, there is a high concentration of n-type Si impurities at the homoepitaxial interface between the self-supporting gallium nitride substrate and the GaN material. These impurities are difficult to completely remove and will introduce parasitic leakage channels, which will severely reduce the breakdown voltage and output power density of homoepitaxial GaN HEMT devices.

[0007] Fourth, when using homoepitaxial GaN buffer layers, in order to solve the problem of parasitic leakage at the homoepitaxial interface, in-situ growth is used to introduce Fe or C impurities for compensation. This will cause impurity diffusion and memory effect, and C impurities, as deep level acceptors, are not suitable for use in microwave power devices.

[0008] Fifth, the low thermal conductivity of self-supporting gallium nitride single crystal substrates limits the normal operation of homoepitaxial GaN HEMT devices at higher temperatures, and cannot meet the requirements of high-power and high-temperature applications. Summary of the Invention

[0009] The purpose of this invention is to address the shortcomings of the existing technologies by proposing a homoepitaxial GaN HEMT device with groove-filled dielectric isolation and a method for fabricating the same, so as to block the parasitic leakage current channel at the homoepitaxial interface, achieve epitaxial growth of gallium nitride material with extremely low defects, and improve the device's heat dissipation efficiency, output power density and reliability.

[0010] The technical solution of this invention is implemented as follows:

[0011] 1. A homoepitaxial GaN HEMT device with groove-filled dielectric isolation for leakage current, comprising, from bottom to top, a GaN substrate, a GaN buffer layer, a back barrier layer, a channel layer, an AlN insertion layer, a barrier layer, and an insulating gate dielectric, wherein ohmic contacts are respectively provided on the left and right sides of the AlN insertion layer and the barrier layer, and source and drain electrodes are respectively provided on the ohmic contacts, and a gate electrode is provided on the insulating gate dielectric, characterized in that:

[0012] A groove is etched between the GaN substrate and the GaN buffer layer. The groove and the back side of the GaN substrate are filled and covered with a high thermal conductivity material as a leakage isolation layer to block the parasitic leakage channel at the homoepitaxial interface.

[0013] The source electrode ohmic contact area is provided with a through hole leading to the leakage isolation layer. Both the through hole and the lower part of the leakage isolation layer are provided with back electrodes to reduce the parasitic capacitance of the device and achieve better high-frequency characteristics.

[0014] Furthermore, the GaN substrate is a self-supporting gallium nitride substrate;

[0015] Furthermore, the GaN buffer layer has a thickness of 300nm-6000nm;

[0016] Furthermore, the back barrier layer adopts any one of the following: graded composition AlGaN, AlGaN / GaN superlattice, and AlGaN / AlN superlattice, with a thickness of 50nm-100nm;

[0017] Furthermore, the channel layer uses In x Ga 1-xN, where the component 0≤x≤1, has a thickness of 10nm-30nm;

[0018] Furthermore, the AlN insertion layer has a thickness of 1nm-2nm;

[0019] Furthermore, the barrier layer is made of any one of AlN, AlGaN, InAlN, ScAlN, AlPN, BAlN, BPN, and YAlN, and its thickness is 3nm-30nm.

[0020] Furthermore, the groove extends into the GaN buffer layer to a thickness of 100-200 nm;

[0021] Furthermore, the leakage current isolation layer is made of any one of diamond, c-BN, and AlN, and its thickness is 10μm-20μm;

[0022] Furthermore, the insulating gate dielectric layer is any one of Al2O3, HfO2, and HfAlO dielectric layers, and its thickness is 3nm-20nm.

[0023] 2. A method for fabricating a homoepitaxial GaN HEMT device with groove-filled dielectric isolation, comprising the following steps:

[0024] 1) On a GaN substrate, a GaN buffer layer with a thickness of 300nm-6000nm is grown using metal-organic chemical vapor deposition or molecular beam epitaxy.

[0025] 2) A back barrier layer with a thickness of 50nm-100nm is grown on the GaN buffer layer using metal-organic chemical vapor deposition or molecular beam epitaxy.

[0026] 3) A channel layer with a thickness of 10 nm-30 nm is grown on the back barrier layer using metal-organic chemical vapor deposition or molecular beam epitaxy.

[0027] 4) An AlN insertion layer with a thickness of 1 nm-2 nm is grown on the channel layer using metal-organic chemical vapor deposition or molecular beam epitaxy.

[0028] 5) A barrier layer with a thickness of 3nm-30nm is grown on the AlN insertion layer using metal-organic chemical vapor deposition or molecular beam epitaxy.

[0029] 6) The thickness of the GaN substrate was reduced to 50μm-150μm from the back side using chemical mechanical polishing.

[0030] 7) Select the area to be etched on the back of the GaN substrate using photolithography, and etch the GaN substrate and GaN buffer layer using dry etching process to etch a groove with a depth of 100nm-200nm into the GaN buffer layer.

[0031] 8) Deposit a leakage isolation layer with a thickness of 10μm-20μm in the etched groove and on the back of the GaN substrate, and perform chemical mechanical polishing on the surface of the leakage isolation layer after deposition to flatten the material surface;

[0032] 9) The source and drain ohmic contact regions of the device are selected at both ends of the barrier layer using photolithography, and then dry etched to the top of the channel layer to form the ohmic contact region groove.

[0033] 10) Using metal-organic chemical vapor deposition or molecular beam epitaxy, grow a Si-doped n-type GaN layer with a thickness of 4 nm-32 nm in the groove of the ohmic contact region, wherein the Si doping concentration is (1-5) × 10⁻⁶. 20 cm -3 This forms an ohmic contact region;

[0034] 11) Using electron beam evaporation, ohmic contact metal Ti / Al / Ni / Au is deposited in the ohmic contact region of the source electrode and the drain electrode, and then annealed at 830℃ in a nitrogen atmosphere to form the source electrode and the drain electrode.

[0035] 12) An insulating gate dielectric layer with a thickness of 3nm-20nm is deposited on the barrier layer using atomic layer deposition technology;

[0036] 13) The gate electrode pattern is selected on the surface of the insulating gate dielectric layer using photolithography, and then Ni / Au metal combination is deposited on the pattern using electron beam evaporation to form the gate electrode;

[0037] 14) Back-channel etching is performed under the leakage isolation layer using a back-channel process to form a through-hole from the leakage isolation layer to the ohmic contact area below the source electrode;

[0038] 15) The hole walls are filled with TiW as an alloy barrier layer by magnetic sputtering, and then Au is filled into the through hole. Au with a thickness of 8μm-10μm is then electroplated on the leakage isolation layer by electroplating. A back electrode is formed at the bottom of the leakage isolation layer to complete the device fabrication.

[0039] Compared with the prior art, the present invention has the following advantages:

[0040] 1. This invention utilizes a self-supporting GaN substrate for homoepitaxial GaN HEMT material, enabling zero-stress epitaxy of GaN heterojunction materials. This effectively reduces the dislocation density in heteroepitaxial GaN materials, improves the crystal quality of the material, reduces vertical leakage channels, and increases the device breakdown voltage and output power.

[0041] 2. The present invention uses a groove-filled dielectric leakage isolation layer to effectively block the parasitic leakage channel formed at the homogeneous epitaxial interface between the GaN buffer layer and the GaN substrate, thereby improving the breakdown voltage of GaN HEMT devices.

[0042] 3. Because the present invention uses a groove-filled dielectric leakage isolation layer to block the parasitic leakage channel formed at the homoepitaxial interface, and does not introduce in-situ Fe or C doping to compensate for parasitic Si impurities at the homoepitaxial interface, the material growth process is simple and there is no memory effect or microwave RF loss.

[0043] 4. By leading the source electrode to the back side of the substrate through a via, this invention reduces the parasitic capacitance of the device and achieves better high-frequency characteristics. At the same time, it can be used as a metal heat sink material to bond to other substrates, realizing the transfer of GaN HEMT devices.

[0044] 5. By filling the groove with a high thermal conductivity leakage isolation layer material and combining it with the back electrode metal on the back of the leakage isolation layer, the present invention can efficiently dissipate the heat generated in the active region of the device, achieve better high-temperature characteristics of the device, and improve the device reliability and upper limit of operating temperature. Attached Figure Description

[0045] Figure 1 This is a diagram of a traditional GaN HEMT device structure;

[0046] Figure 2 This is a structural diagram of the homoepitaxial GaN HEMT device with groove-filled dielectric isolation for leakage current according to the present invention;

[0047] Figure 3 This is a schematic diagram of the process flow for fabricating a homogeneous epitaxial GaN HEMT device with groove-filled dielectric isolation for leakage current according to the present invention. Detailed Implementation

[0048] Reference Figure 2 The present invention discloses a homoepitaxial GaN HEMT device structure with groove-filled dielectric isolation for leakage current, comprising a GaN substrate 1, a GaN buffer layer 2, a back barrier layer 3, a channel layer 4, an AlN insertion layer 5, a barrier layer 6, a groove 7, a leakage isolation layer 8, an insulating gate dielectric 9, and a back electrode 10. Ohmic contact regions are respectively provided on the left and right sides of the AlN insertion layer 5 and the barrier layer 6, and source and drain electrodes are respectively provided on the ohmic contact regions. A gate electrode is provided on the insulating gate dielectric. Wherein:

[0049] The GaN substrate 1 is a self-supporting gallium nitride substrate;

[0050] The GaN buffer layer 2 is located above the GaN substrate 1, and its thickness is 300nm-6000nm;

[0051] A groove 7 is provided between the GaN substrate 1 and the GaN buffer layer 2, and the groove penetrates into the GaN buffer layer 2 to a depth of 100nm-200nm.

[0052] The groove 7 is filled with and covered by the back side of the GaN substrate 1 by the leakage isolation layer 8 to block the parasitic leakage channel at the homoepitaxial interface.

[0053] The leakage current isolation layer 8 is made of any one of diamond, c-BN, and AlN, and its thickness is 10μm-20μm.

[0054] The back barrier layer 3 is located above the GaN buffer layer 2. It adopts any one of the gradient composition AlGaN, AlGaN / GaN superlattice, and AlGaN / AlN superlattice, and has a thickness of 50nm-100nm.

[0055] The aforementioned channel layer 4 is located above the back barrier layer 3, and it employs In... x Ga 1-x N, composition 0≤x≤1, thickness 10nm-30nm;

[0056] The AlN insertion layer 5 is located above the channel layer 4, and its thickness is 1nm-2nm;

[0057] The barrier layer 6 is located above the AlN insertion layer 5 and is made of any one of AlN, AlGaN, InAlN, ScAlN, AlPN, BAlN, BPN, and YAlN, with a thickness of 3nm-30nm.

[0058] The insulating gate dielectric layer 9 is located above the barrier layer 6, and it adopts any one of Al2O3, HfO2, and HfAlO dielectric layers, with a thickness of 3nm-20nm;

[0059] The source electrode is formed by etching a via from the back of the leakage isolation layer to the ohmic contact area using a back-channel process, and filling the via with metal and electroplating metal on the leakage isolation layer 8 to form the back electrode 10.

[0060] Reference Figure 3 The present invention provides a method for fabricating a homogeneous epitaxial GaN HEMT device with groove-filled dielectric isolation leakage current, and gives the following three embodiments.

[0061] Example 1: Fabrication using a self-supporting gallium nitride substrate, a diamond leakage isolation layer, a graded-composition AlGaN back barrier layer with a thickness of 100 nm, a GaN channel thickness of 30 nm, and Al... 0.25 Ga 0.75 Homoetropic GaNHEMT devices with an N-barrier layer thickness of 30 nm.

[0062] Step 1: Deposit a GaN buffer layer, such as... Figure 3 (a).

[0063] A GaN buffer layer with a thickness of 6000 nm was deposited on a GaN substrate using metal-organic chemical vapor deposition (MOCVD). The deposition process conditions were: temperature 1250℃, pressure 50 Torr, ammonia flow rate 2000 sccm, gallium source flow rate 150 sccm, and hydrogen flow rate 3000 sccm.

[0064] Step 2: Deposit a graded-component AlGaN back barrier layer, such as... Figure 3 (b)

[0065] A 100 nm thick gradient AlGaN back barrier layer was deposited on a GaN buffer layer using metal-organic chemical vapor deposition (MOCVD). The deposition conditions were: 1250 °C, 50 Torr pressure, 2000 sccm ammonia flow rate, 150 sccm gallium source flow rate, 20 sccm aluminum source flow rate, and 3000 sccm hydrogen flow rate.

[0066] Step 3: Deposit the GaN channel layer, such as... Figure 3 (c)

[0067] A 30 nm thick GaN channel layer was deposited on a graded composition AlGaN back barrier layer using metal-organic chemical vapor deposition (MOCVD). The deposition process conditions were: a temperature of 1250 °C, a pressure of 50 Torr, a gallium source flow rate of 150 sccm, an ammonia flow rate of 2000 sccm, and a hydrogen flow rate of 3000 sccm.

[0068] Step four, deposit the AlN insertion layer, such as Figure 3 (d)

[0069] A 1 nm thick AlN insertion layer was deposited on the GaN channel layer using metal-organic chemical vapor deposition (MOCVD). The deposition process conditions were: temperature 1250 °C, pressure 50 Torr, aluminum source flow rate 20 sccm, ammonia flow rate 2000 sccm, and hydrogen flow rate 3000 sccm.

[0070] Step 5: Deposit an AlGaN barrier layer, such as... Figure 3 (e).

[0071] A 30 nm thick Al layer was deposited on the AlN insertion layer using metal-organic chemical vapor deposition (MOCVD). 0.25 Ga 0.75 The deposition process conditions for the N-barrier layer are: temperature 1250℃, pressure 50 Torr, ammonia flow rate 2000 sccm, gallium source flow rate 60 sccm, aluminum source flow rate 20 sccm, and hydrogen flow rate 3000 sccm.

[0072] Step 6: Thin the GaN substrate, such as... Figure 3 (f).

[0073] The GaN substrate was thinned to 50 μm using chemical mechanical polishing. First, coarse grinding was performed at high speed for thinning, followed by fine grinding to improve the flatness of the GaN substrate's back side.

[0074] Step 7: Etch the GaN substrate and GaN buffer layer to form a trench, such as... Figure 3 (g)

[0075] The etching area was selected on the back side of the GaN substrate using photolithography, and the GaN substrate and GaN buffer layer were etched using a dry etching process to create a groove with a depth of 100 nm into the GaN buffer layer.

[0076] Step 8: Deposit a diamond leakage current isolation layer, such as... Figure 3 (h).

[0077] A 10 μm thick diamond leakage current isolation layer was deposited in the groove and on the back side of the GaN substrate using microwave plasma chemical vapor deposition (IPV). The surface of the diamond leakage current isolation layer was then chemically and mechanically polished. The deposition conditions were: microwave power 1400 W, gas pressure 21 kPa, and plasma power density 700 W / cm². 3 Temperature 850℃, CH4 volume fraction 1.0%, H2 flow rate 200ml / min.

[0078] Step nine, dry etching, to form grooves in the source / drain ohmic contact region, such as... Figure 3 (i).

[0079] Using photolithography in Al 0.25 Ga 0.75 The source and drain ohmic contact regions were selected on both sides of the N-barrier layer. The two ends of the barrier layer were processed to the top of the channel layer using RIE dry etching technology to form the source and drain ohmic contact region grooves. The etching process conditions were: Cl2 flow rate of 15 sccm, reaction chamber pressure of 12 mTorr, and electrode power of 180 W.

[0080] Step 10: Create the ohmic contact area, such as... Figure 3 (j).

[0081] A 31 nm thick Si-doped n-type GaN layer was deposited in the ohmic contact region groove using metal-organic chemical vapor deposition (MOCVD), with a Si doping concentration of 1 × 10⁻⁶. 20 cm -3 The deposition process conditions are as follows: temperature 1250℃, pressure 50 Torr, ammonia flow rate 2000 sccm, gallium source flow rate 150 sccm, hydrogen flow rate 3000 sccm, and silane flow rate 500 sccm, forming left and right ohmic contact regions.

[0082] Step 11: Fabricate the source and drain electrodes, as follows Figure 3 (k).

[0083] Electron beam evaporation was used to deposit Ti / Al / Ni / Au metal composites with thicknesses of 0.02 μm / 0.05 μm / 0.04 μm / 0.04 μm on the ohmic contact regions of the source and drain electrodes, respectively. These were then rapidly thermally annealed for 30 s at 830 °C in a nitrogen atmosphere to form the source and drain electrodes. The deposition conditions were: vacuum degree less than 1.2 × 10⁻⁶. -3 Pa, power is 400W, evaporation rate is

[0084] Step 12: Deposit an Al2O3 insulating gate dielectric layer, such as... Figure 3 (l).

[0085] Atomic layer deposition process is used in Al 0.25 Ga 0.75 An Al2O3 insulating gate dielectric layer with a thickness of 10 nm is grown on the N-barrier layer.

[0086] Step thirteen, fabricate the gate electrode, such as Figure 3 (m).

[0087] A mask was fabricated on an Al2O3 insulating gate dielectric layer using photolithography. Electron beam evaporation was then used to deposit metal on selected areas of the Al2O3 insulating gate dielectric layer to create the gate electrode. The deposited metal was a Ni / Au metal combination with a thickness of 0.02 μm / 0.3 μm. The deposition process conditions were: vacuum level less than 1.4 × 10⁻⁶. -3 Pa, power range of 400-800W, evaporation rate of

[0088] Step fourteen: Use a back-path etching process to form through-holes, such as... Figure 3 (n).

[0089] A back-channel process is used, employing inductively coupled plasma etching (ICP-C) to form a via from the leakage isolation layer to the ohmic contact area below the source electrode.

[0090] Step 15: Fill the through-hole with metal and electroplate metal onto the leakage current isolation layer, such as... Figure 3 (o).

[0091] TiW was used to fill the hole walls as an alloy barrier layer by magnetic sputtering, and Au was then filled into the through holes. Au with a thickness of 8 μm was then electroplated on the leakage isolation layer to form a back electrode at the bottom of the leakage isolation layer, thus completing the device fabrication.

[0092] Example 2: Fabrication using a self-supporting gallium nitride substrate, a c-BN leakage isolation layer, an 80nm thick AlGaN / GaN superlattice back barrier layer, and an In... 0.1 Ga 0.9 The N-channel layer thickness is 20 nm, and the Sc layer thickness is 20 nm. 0.18 Al 0.82 GaN HEMT devices with an N-barrier layer thickness of 10 nm.

[0093] Step 1: Deposit a GaN buffer layer on the GaN substrate, such as... Figure 3 (a).

[0094] Using metal-organic chemical vapor deposition (MOCVD), a 3000 nm thick GaN buffer layer was deposited on a GaN substrate under the following process conditions: temperature 1150 °C, pressure 60 Torr, ammonia flow rate 2000 sccm, gallium source flow rate 90 sccm, and hydrogen flow rate 3000 sccm.

[0095] Step 2: Deposit an AlGaN / GaN superlattice back barrier layer on the GaN buffer layer, such as... Figure 3 (b)

[0096] Using metal-organic chemical vapor deposition (MOCVD), under the following process conditions: temperature 1150℃, pressure 60 Torr, ammonia flow rate 2000 sccm, gallium source flow rate 90 sccm, aluminum source flow rate 25 sccm, and hydrogen flow rate 3000 sccm, Al₂O₃ substrates with a period of 20 and a thickness of 80 nm were grown on a GaN substrate. 0.2 Ga 0.8 N / GaN superlattice back barrier layer.

[0097] Step 3: Deposit In on the AlGaN / GaN superlattice back barrier layer 0.1 Ga 0.9 N-channel layer, such as Figure 3 (c)

[0098] Using metal-organic chemical vapor deposition (MOCVD), under the following process conditions: temperature 700℃, pressure 300 Torr, ammonia flow rate 2000 sccm, indium source flow rate 120 sccm, gallium source flow rate 60 sccm, and nitrogen flow rate 3000 sccm, a 20 nm thick In layer was deposited on the AlGaN / GaN superlattice back barrier layer. 0.1 Ga 0.9 N-channel layer.

[0099] Step 4, in In 0.1 Ga 0.9 An AlN insertion layer is deposited on the N-channel layer, such as Figure 3 (d)

[0100] Using metal-organic chemical vapor deposition (MOCVD), under process conditions of 700°C, 300 Torr, aluminum source flow rate of 25 sccm, ammonia flow rate of 2000 sccm, and nitrogen flow rate of 3000 sccm, in In... 0.1 Ga 0.9 An AlN insertion layer with a thickness of 1.5 nm is deposited on the N-channel layer.

[0101] Step 5: Deposit Sc on the AlN insertion layer 0.18 Al 0.82 N-barrier layer, such as Figure 3 (e).

[0102] Using metal-organic chemical vapor deposition (MOCVD), under the following process conditions: temperature 1000℃, pressure 300 Torr, aluminum source flow rate 25 sccm, scandium source flow rate 10 sccm, ammonia flow rate 2000 sccm, and nitrogen flow rate 3000 sccm, a 10 nm thick Scandium layer was deposited on the AlN insertion layer. 0.18 Al 0.82 N-barrier layer.

[0103] Step 6, thin the GaN substrate, such as... Figure 3 (f).

[0104] Using chemical mechanical polishing, the GaN substrate is first coarsely ground at high speed to reduce its thickness, and then finely ground to improve the flatness of the back side, reducing its thickness to 100 μm.

[0105] Step 7: Etch the GaN substrate and GaN buffer layer to form a groove, such as... Figure 3 (g)

[0106] The etching area was selected on the back side of the GaN substrate using photolithography, and the GaN substrate and GaN buffer layer were etched using dry etching to create a groove with a depth of 150 nm into the GaN buffer layer.

[0107] Step 8: Deposit a leakage isolation layer on the back side of the GaN substrate, such as... Figure 3 (h).

[0108] Using metal-organic chemical vapor deposition (MOCVD), a 15 μm thick cubic boron nitride (c-BN) layer was deposited in a groove and on the back side of a GaN substrate under the conditions of 1300 °C, 400 Torr, 20 μmol / min boron source flow rate, 3000 sccm ammonia flow rate, and 2000 sccm hydrogen flow rate. After deposition, the surface of the c-BN leakage isolation layer was chemically mechanically polished.

[0109] Step 9, dry etching, to form grooves in the source / drain ohmic contact region, such as... Figure 3 (i).

[0110] Using photolithography on Sc 0.18 Al 0.82 The source and drain ohmic contact regions were patterned on the surface of the N-barrier layer. Using RIE dry etching technology, under the process conditions of Cl2 flow rate of 20 sccm, reaction chamber pressure of 15 mTorr, and electrode power of 200 W, the two ends of the barrier layer were processed to the top of the channel layer to form the source and drain ohmic contact region grooves.

[0111] Step 10, create the source-drain ohmic contact region, such as... Figure 3 (j).

[0112] Using metal-organic chemical vapor deposition (MOCVD), a Si-doped n-type GaN layer with a thickness of 11.5 nm was deposited in the ohmic contact trench region under the following process conditions: temperature 1150 °C, pressure 60 Torr, ammonia flow rate 2000 sccm, gallium source flow rate 90 sccm, hydrogen flow rate 3000 sccm, and silane flow rate 800 sccm. The Si ion concentration was 3 × 10⁻⁶. 20 cm -3 This forms an ohmic contact region.

[0113] Step 11, fabricate the source and drain electrodes, as follows: Figure 3 (k).

[0114] Electron beam evaporation was employed at a vacuum level of less than 1.2 × 10⁻⁶. -3 Pa, power is 400W, evaporation rate is Under the specified process conditions, Ti / Al / Ni / Au metal composites with thicknesses of 0.02μm / 0.05μm / 0.04μm / 0.04μm were deposited on the ohmic contact regions of the source and drain electrodes, respectively, and then rapidly thermally annealed for 30s in a nitrogen atmosphere at a temperature of 830℃ to form the source and drain electrodes.

[0115] Step 12, using atomic layer deposition (ALD) technology, on the Sc 0.18 Al 0.82 A 20 nm thick HfO2 insulating gate dielectric layer is deposited on the N-barrier layer, such as Figure 3 (l).

[0116] Step 13, fabricate the gate electrode on the insulating gate dielectric, such as... Figure 3 (m).

[0117] The gate pattern was selected on the HfO2 insulating gate dielectric layer using photolithography, and electron beam evaporation was performed at a vacuum level of less than 1.2 × 10⁻⁶. -3 Pa, power is 600W, evaporation rate is Under the specified process conditions, metal is deposited on the HfO2 insulating gate dielectric layer to fabricate the gate, wherein the deposited metal is a Ni / Au metal combination with a metal thickness of 0.04μm / 0.5μm.

[0118] Step 14: Use a back-path etching process to form through-holes, such as... Figure 3 (n).

[0119] A back-channel process is used to perform via etching under the leakage isolation layer, and inductively coupled plasma etching technology is used to form vias from the leakage isolation layer to the ohmic contact area below the source electrode.

[0120] Step 15: Fill the through-hole with metal and electroplate metal onto the leakage current isolation layer, such as... Figure 3 (o).

[0121] TiW was used to fill the hole walls as an alloy barrier layer by magnetic sputtering, and Au was then filled into the through holes. Au with a thickness of 9 μm was then electroplated on the leakage isolation layer to form a back electrode at the bottom of the leakage isolation layer, thus completing the device fabrication.

[0122] Example 3: Fabrication of a GaN HEMT device using a self-supporting gallium nitride substrate, with an AlN leakage isolation layer, an AlGaN / AlN back barrier layer thickness of 50 nm, an InN channel layer thickness of 10 nm, and an AlN barrier layer thickness of 3 nm.

[0123] Step A: Select a self-supporting GaN substrate, set the temperature to 750℃, the nitrogen flow rate to 0.6 sccm, and the gallium beam equilibrium vapor pressure to 3.5 × 10⁻⁶. -7 Using a 350W nitrogen plasma RF source and a Torr process, a 300nm thick GaN buffer layer was deposited on a GaN substrate via molecular beam epitaxy. Figure 3 (a).

[0124] Step B: Set the temperature to 750℃, the nitrogen flow rate to 0.6 sccm, and the gallium beam equilibrium vapor pressure to 3.5 × 10⁻⁶. - 7 Torr, the equilibrium vapor pressure of the aluminum beam is 1.2 × 10⁻⁶. -7 Using a 350W nitrogen plasma RF source, a 50nm thick AlGaN / AlN superlattice back barrier layer was deposited on a GaN buffer layer via molecular beam epitaxy. Figure 3 (b)

[0125] Step C: Set the temperature to 550℃, the nitrogen flow rate to 0.6 sccm, and the indium beam equilibrium vapor pressure to 2.0 × 10⁻⁶. - 7 Torr, using a nitrogen plasma RF source with a power of 350W, employed molecular beam epitaxy to deposit a 10nm thick InN channel layer on an AlGaN / AlN superlattice back barrier layer. Figure 3 (c)

[0126] Step D: Set the temperature to 550℃, the nitrogen flow rate to 0.6 sccm, and the aluminum beam equilibrium vapor pressure to 1.2 × 10⁻⁶. - 7 Using a 350W nitrogen plasma RF source, a 2nm thick AlN insertion layer was deposited on the InN channel layer via molecular beam epitaxy. Figure 3 (d)

[0127] Step E: Set the temperature to 720℃, the nitrogen flow rate to 0.6 sccm, and the aluminum beam equilibrium vapor pressure to 1.2 × 10⁻⁶. - 7 Using a 350W nitrogen plasma RF source as the process condition, molecular beam epitaxy was employed to deposit a 3nm thick AlN barrier layer on the AlN insertion layer. Figure 3 (e).

[0128] Step F involves using chemical mechanical polishing (CMP) to first perform high-speed coarse grinding to thin the GaN substrate, followed by fine grinding to improve the flatness of the GaN substrate's back side, reducing its thickness to 150 μm. Figure 3 (f).

[0129] Step G: Using photolithography, an etching area is selected on the back side of the GaN substrate. A dry etching process is then used to etch the GaN substrate and GaN buffer layer from the back side, creating a groove 200 nm thick that penetrates into the GaN buffer layer. Figure 3 (g)

[0130] Step H: Set the temperature to 400℃ and the vacuum level to less than 10. -4Under the process conditions of Pa, pressure 40 Torr, DC sputtering power 5 kW, aluminum source flow rate 110 sccm, argon flow rate 45 sccm, and ammonia flow rate 1000 sccm, a 20 μm thick AlN leakage isolation layer was deposited in the groove and on the back side of the GaN substrate using physical vapor deposition (PVD). The AlN leakage isolation layer surface was then chemically and mechanically polished. Figure 3 (h).

[0131] Step I: Using photolithography, the ohmic contact regions of the source and drain electrodes are selected on the surface of the AlN barrier layer. The process conditions are set as follows: Cl2 flow rate of 10 sccm, reaction chamber pressure of 10 mTorr, and electrode power of 180 W. Using RIE dry etching technology, the two ends of the barrier layer are processed to above the channel layer, forming grooves in the source-drain ohmic contact region. Figure 3 (i).

[0132] Step J: Set the temperature to 750℃, the nitrogen flow rate to 0.6 sccm, and the gallium beam equilibrium vapor pressure to 3.5 × 10⁻⁶. - 7 Torr, the equilibrium vapor pressure of the silicon beam is 2.8 × 10⁻⁶. -8 Using a 350W nitrogen plasma RF source and molecular beam epitaxy (MBE) process, a 5nm thick Si-doped n-type GaN layer was deposited in the ohmic contact groove region. The Si ion concentration was 5 × 10⁻⁶. 20 cm -3 This forms an ohmic contact region, such as Figure 3 (j).

[0133] Step K: Set the vacuum level to less than 1.2 × 10⁻⁶. -3 Pa, power is 500W, evaporation rate is The process conditions were as follows: electron beam evaporation was used to deposit Ti / Al / Ni / Au metal composites with thicknesses of 0.02μm / 0.2μm / 0.05μm / 0.05μm on the ohmic contact regions of the source and drain electrodes, respectively. These were then rapidly thermally annealed for 30 seconds at 830℃ in a nitrogen atmosphere to form the source and drain electrodes. Figure 3 (k).

[0134] Step L involves depositing a 3nm thick HfAlO insulating gate dielectric layer on the AlN barrier layer using atomic layer deposition (ALD) technology, such as... Figure 3 (l).

[0135] Step M involves selecting the gate pattern on the HfAlO insulating gate dielectric layer using photolithography, with the vacuum level set to be less than 1.2 × 10⁻⁶. -3 Pa, power is 500W, evaporation rate is Under specific process conditions, electron beam evaporation technology was used to deposit a Ni / Au metal composite with a thickness of 0.03 μm / 0.4 μm on the HfAlO insulating gate dielectric layer to fabricate the gate, as shown below. Figure 3 (m).

[0136] Step N involves etching vias under the leakage isolation layer using a back-channel process, and forming vias from the leakage isolation layer to the ohmic contact region below the source electrode using inductively coupled plasma etching (ICP-C). Figure 3 (n).

[0137] Step O involves filling the hole walls with TiW as an alloy barrier layer using magnetic sputtering, then filling the through-holes with Au, and finally electroplating a 10μm thick layer of Au onto the leakage isolation layer. A back electrode is then formed at the bottom of the leakage isolation layer, completing the device fabrication. Figure 3 (o).

[0138] The above descriptions are merely three specific examples of the present invention and do not constitute any limitation on the present invention. Obviously, those skilled in the art, after understanding the content and principles of the present invention, may make various modifications and changes in form and details without departing from the principles and structure of the present invention. For example, in addition to AlN, AlGaN, and ScAlN, the barrier layer may also use any one of InAlN, AlPN, BAlN, BPN, or YAlN. However, these modifications and changes based on the ideas of the present invention are still within the scope of the claims of the present invention.

Claims

1. A homoepitaxial GaN HEMT device with groove-filled dielectric isolation for leakage current, comprising, from bottom to top, a GaN substrate (1), a GaN buffer layer (2), a back barrier layer (3), a channel layer (4), an AlN insertion layer (5), a barrier layer (6), and an insulating gate dielectric (9), wherein ohmic contact regions are respectively provided on the left and right sides of the AlN insertion layer (5) and the barrier layer (6), and source and drain electrodes are respectively provided on the ohmic contact regions, and a gate electrode is provided on the insulating gate dielectric (9), characterized in that: A groove (7) is etched between the GaN substrate (1) and the GaN buffer layer (2). The groove and the back side of the GaN substrate (1) are filled and covered with a high thermal conductivity material as a leakage isolation layer (8) to block the parasitic leakage channel at the homogeneous epitaxial interface. The back barrier layer (3) adopts any one of the graded composition AlGaN, AlGaN / GaN superlattice, and AlGaN / AlN superlattice, with a thickness of 50nm-100nm. The channel layer (4) adopts In x Ga 1-x N, where the component 0≤x≤1, has a thickness of 10 nm-30 nm; The barrier layer (6) is any one of AlN, AlGaN, InAlN, ScAlN, AlPN, BAlN, BPN, YAlN, and its thickness is 3 nm-30 nm. The groove (7) extends into the GaN buffer layer (2) with a thickness of 100-200 nm; The leakage current isolation layer (8) is made of any one of diamond, c-BN and AlN, and its thickness is 10 μm-20 μm. The insulating gate dielectric layer (9) is any one of Al2O3, HfO2, and HfAlO dielectric layers, and its thickness is 3 nm-20 nm. The source electrode has a through hole below its ohmic contact area leading to the leakage isolation layer (8). Both the through hole and the lower part of the leakage isolation layer have back electrodes (10) to reduce the parasitic capacitance of the device and achieve better high-frequency characteristics.

2. The device as described in claim 1, characterized in that: The GaN substrate (1) is a self-supporting gallium nitride substrate; The GaN buffer layer (2) has a thickness of 300 nm-6000 nm; The AlN insertion layer (5) has a thickness of 1 nm-2 nm.

3. A method for fabricating a homoepitaxial GaN HEMT device with groove-filled dielectric isolation as described in claim 1, characterized in that, Includes the following steps: 1) On a GaN substrate (1), a GaN buffer layer (2) with a thickness of 300 nm-6000 nm is grown using metal-organic chemical vapor deposition or molecular beam epitaxy. 2) A back barrier layer (3) with a thickness of 50 nm-100 nm is grown on the GaN buffer layer (2) using metal-organic chemical vapor deposition or molecular beam epitaxy. 3) Using metal-organic chemical vapor deposition or molecular beam epitaxy, a channel layer (4) with a thickness of 10 nm-30 nm is grown on the back barrier layer (3). 4) An AlN insertion layer (5) with a thickness of 1 nm-2 nm is grown on the channel layer (4) using metal-organic chemical vapor deposition or molecular beam epitaxy. 5) A barrier layer (6) with a thickness of 3 nm-30 nm is grown on the AlN insertion layer (5) using metal-organic chemical vapor deposition or molecular beam epitaxy. 6) The thickness of the GaN substrate (1) was reduced to 50 μm-150 μm from the back side using a chemical mechanical polishing method; 7) Select the area to be etched on the back side of the GaN substrate (1) using photolithography, and etch the GaN substrate (1) and buffer layer (2) using dry etching process to etch a groove (7) with a depth of 100 nm-200 nm into the GaN buffer layer (2). 8) A leakage isolation layer (8) with a thickness of 10 μm-20 μm is deposited in the etched groove (7) and on the back of the GaN substrate (1), and the surface of the leakage isolation layer (8) is chemically and mechanically polished after deposition to flatten the material surface; 9) The source and drain ohmic contact regions of the device are selected at both ends of the barrier layer using photolithography, and then dry etched to the top of the channel layer to form the ohmic contact region groove. 10) Using metal-organic chemical vapor deposition or molecular beam epitaxy, grow a Si-doped n-type GaN layer with a thickness of 4 nm-32 nm in the groove of the ohmic contact region, wherein the Si doping concentration is (1~5)×10⁻⁶. 20 cm -3 This forms an ohmic contact region; 11) Using electron beam evaporation, ohmic contact metal Ti / Al / Ni / Au is deposited in the ohmic contact region of the source electrode and the drain electrode, and then annealed at 830 °C in a nitrogen atmosphere to form the source electrode and the drain electrode. 12) An insulating gate dielectric layer with a thickness of 3 nm-20 nm was deposited on the barrier layer using atomic layer deposition (9). 13) A gate electrode pattern is selected on the surface of the insulating gate dielectric layer (9) using photolithography, and a Ni / Au metal combination is deposited on the pattern using electron beam evaporation to form the gate electrode; 14) Back-channel etching is performed under the leakage isolation layer (8) using a back-channel process to form a through-hole from the leakage isolation layer (8) to the ohmic contact area below the source electrode; 15) The hole wall is filled with TiW as an alloy barrier layer by magnetic sputtering process, and Au is filled into the through hole. Then, Au with a thickness of 8 μm-10 μm is electroplated on the leakage isolation layer (8) by electroplating process. A back electrode (10) is formed at the bottom of the leakage isolation layer (8) to complete the device fabrication.

4. The manufacturing method as described in claim 3, characterized in that, The process conditions for the organometallic chemical vapor deposition technique in steps 1)-5) are as follows: Temperature is 700 o C - 1250 o C; The pressure is 50 Torr - 300 Torr; The ammonia flow rate is 2000 sccm; The hydrogen flow rate is 3000 sccm; The nitrogen flow rate is 3000 sccm; The gallium source flow rate is 60 sccm - 150 sccm; The aluminum source flow rate is 2 sccm - 30 sccm; The indium source flow rate is 30 sccm - 120 sccm; The scandium source flow rate is 10 sccm - 20 sccm; The yttrium source flow rate is 4 sccm - 20 sccm; The boron source flow rate was 10 μmol / min - 30 μmol / min; The phosphorus source flow rate was 20 μmol / min - 50 μmol / min; The silane flow rate is 500 sccm - 1000 sccm.

5. The manufacturing method as described in claim 3, characterized in that, The molecular beam epitaxy method in steps 1)-5) has the following process conditions: The temperature is 550 o C - 750 o C; Nitrogen flow rate is 0.6 sccm - 2.8 sccm; The equilibrium vapor pressure of the scandium beam is 1.2 × 10⁻⁶. -8 Torr - 1.8×10 -8 Torr; The equilibrium vapor pressure of the yttrium beam is 1.0 × 10⁻⁶. -8 Torr - 1.5×10 -8 Torr; The equilibrium vapor pressure of the gallium beam is 3.5 × 10⁻⁶. -7 Torr - 8.5×10 -7 Torr; The equilibrium vapor pressure of the aluminum beam is 0.6 × 10⁻⁶. -7 Torr - 2.8×10 -7 Torr; The equilibrium vapor pressure of the indium beam is 2.0 × 10⁻⁶. -7 Torr - 6.0×10 -7 Torr; The equilibrium vapor pressure of the silicon beam is 2.8 × 10⁻⁶. -8 Torr; The equilibrium vapor pressure of the boron beam is 1.2 × 10⁻⁶. -8 Torr - 3.0×10 -8 Torr; The equilibrium vapor pressure of the phosphorus beam is 0.8 × 10⁻⁶. -8 Torr - 2.0×10 -8 Torr; The nitrogen plasma radio frequency source has a power of 350 W.

6. The manufacturing method as described in claim 4, characterized in that: The scandium source is tricyclopentadienyl scandium Cp3Sc or dimethylcyclopentadienyl scandium chloride (MCp)2ScCl.

7. The manufacturing method as described in claim 4, characterized in that: The boron source is selected from triethylboron.

8. The manufacturing method as described in claim 4, characterized in that: The phosphorus source is selected from tertiary phosphine R-3P.

Citation Information

Patent Citations

  • High-breakdown voltage InAlN / AlGaN high-electron mobility transistor and manufacturing method thereof

    CN104393038A

  • Homoepitaxial gallium nitride high-electron-mobility transistor based on P-type GaN electric leakage isolation layer and manufacturing method of homoepitaxial gallium nitride high-electron-mobility transistor

    CN113555431A

  • Semiconductor device and method for fabricating same

    US20130146946A1