Boron-doped metal ion pillared layered titanate / carbon composite material and preparation method and application thereof
Through boron-doped metal ion pillar-supported layered titanate/carbon composite, the problems of poor conductivity of layered titanate and small sodium ion diffusion coefficient are solved, and the conductivity and sodium storage of sodium ion battery negative electrode materials are improved Performance, achieving better application results.
Patent Information
- Application Number
- CN202211575215.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-12-08
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2042-12-08
AI Technical Summary
The poor conductivity of layered titanate and the small diffusion coefficient of sodium ion limit their energy storage applications in the negative electrode materials of sodium ion batteries.
Using boron-doped metal ion pillar-supported titanate/carbon composite material, potassium titanate or sodium titanate is produced by reacting TiO2 with KOH or NaOH, and reacting with aqueous metal ion solution, sodium alginate and ionic liquid are added for Cross-linking and calcining to form a composite material with excellent electrical conductivity.
It improves the conductivity and sodium storage properties of the negative electrode materials of sodium ion battery, and enhances the cycle stability and application potential.
Smart Images

Figure CN115763763B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of inorganic material preparation, and in particular relates to a boron-doped metal ion pillared layered titanate / carbon composite material and a preparation method and application thereof. Background Art
[0002] With the continuous consumption of fossil resources and the increasing prominence of environmental problems, the utilization of clean energy such as wind and solar energy and the development of large-scale grid energy storage have led to an increasingly urgent demand for secondary energy storage devices. Secondary batteries, such as lithium-ion batteries, have the characteristics of high energy density, small size and green environmental protection, and have been widely used in portable electronic devices and electric vehicles. However, limited lithium resources cannot meet the huge demand for lithium-ion batteries. Sodium reserves are abundant and evenly distributed. Sodium-ion batteries have the same working principle as lithium-ion batteries, as well as the advantages of high safety and excellent high and low temperature performance, making them an ideal substitute for lithium-ion batteries.
[0003] As the negative electrode material of sodium-ion batteries, layered titanates have gradually attracted people's attention due to their advantages such as low cost, easy preparation, and low sodium storage potential. However, layered titanates have low electrical conductivity and their limited interlayer spacing makes the diffusion of sodium ions slow, thus limiting their large-scale application in energy storage.
[0004] Therefore, it is currently necessary to solve the problems of poor conductivity and small sodium ion diffusion coefficient of layered titanates when used as negative electrode materials for sodium ion batteries. Summary of the invention
[0005] The purpose of the present invention is to overcome the problems of poor conductivity and small sodium ion diffusion coefficient of layered titanate when used as a negative electrode material for sodium ion batteries, and provide a boron-doped metal ion pillared layered titanate / carbon composite material and a preparation method and application thereof, thereby obtaining a boron-doped metal ion pillared layered titanate / carbon composite material, which has improved conductivity and sodium storage performance, and is a negative electrode material for sodium ion batteries with good application prospects.
[0006] In order to achieve the above object, the present invention adopts the following technical scheme:
[0007] A method for preparing a boron-doped metal ion pillared layered titanate / carbon composite material comprises the following steps:
[0008] 1) Take TiO 2 The powder is added into a KOH aqueous solution or a NaOH aqueous solution, stirred evenly, and then heated for reaction. The product is filtered and washed with deionized water, and dried to obtain powder I;
[0009] 2) adding a metal salt into water to prepare a metal ion aqueous solution, adding the powder I obtained in step 1) into the metal ion aqueous solution and stirring, filtering and washing the product with deionized water, and drying to obtain a powder II;
[0010] 3) adding sodium alginate to water, stirring at room temperature until the sodium alginate is dissolved, then adding ionic liquid, stirring to obtain a sodium alginate / ionic liquid aqueous solution, adding the powder II obtained in step 2) to the sodium alginate / ionic liquid aqueous solution, stirring to react, and after the reaction is completed, filtering and washing the product with deionized water, and drying to obtain powder III;
[0011] 4) calcining the powder III prepared in step 3) to obtain a boron-doped metal ion pillared layered titanate / carbon composite material.
[0012] Furthermore, in step 1), 0.1 g of TiO 2 The powder is subjected to the heating reaction at a temperature ranging from room temperature to 200° C. for 5 to 24 hours.
[0013] Furthermore, in step 1), the concentration of the KOH aqueous solution or the NaOH aqueous solution is 1 to 10 mol / L.
[0014] Furthermore, in step 2), the metal salt is one of manganese chloride, magnesium chloride, tin chloride and bismuth chloride, and the metal ion concentration of the metal ion aqueous solution is 0.1-1 mol / L.
[0015] Furthermore, the ionic liquid in step 3) is one of 1-butyl-3-methylimidazolium tetrafluoroborate, 1-hexadecyl-3-methylimidazolium tetrafluoroborate and 1-(2-hydroxyethyl)-3-imidazole tetrafluoroborate.
[0016] Furthermore, in step 3), 1 to 10 g of sodium alginate is added to every 500 mL of water, the mass of the ionic liquid is 0.1 to 1% of the mass of the sodium alginate, the stirring time for obtaining the sodium alginate / ionic liquid aqueous solution is 10 min, and the powder II is added to the sodium alginate / ionic liquid aqueous solution and the stirring reaction time is 1 to 10 h.
[0017] Furthermore, the drying conditions in steps 1), 2) and 3) are drying at 80° C. for 24 hours.
[0018] Furthermore, the calcination in step 4) is carried out in an argon or nitrogen atmosphere at a temperature of 500 to 900° C., the heating rate of the calcination is 3° C. / min, and the holding time is 1 to 5 hours.
[0019] A boron-doped metal ion pillared layered titanate / carbon composite material is prepared by the above-mentioned preparation method.
[0020] An application of the boron-doped metal ion pillared layered titanate / carbon composite material on a negative electrode of a sodium ion battery is disclosed. The boron-doped metal ion pillared layered titanate / carbon composite material is mixed with acetylene black and PVDF in a mass ratio of 8:1:1 to prepare a negative electrode for a sodium ion battery.
[0021] Compared with the prior art, the present invention has the following beneficial technical effects:
[0022] The present invention provides a method for preparing a boron-doped metal ion pillared layered titanate / carbon composite material, using sodium alginate as a carbon source and a crosslinking agent, an ionic liquid as a dopant, and an inorganic metal salt as a pillaring agent to prepare the boron-doped metal ion pillared layered titanate / carbon composite material. 2 Potassium titanate or sodium titanate can be obtained by reacting with KOH or NaOH, and the metal ions can replace part of the potassium ions or sodium ions in the titanate by reacting with a metal ion aqueous solution, thereby obtaining a metal ion-pillared layered titanate; sodium alginate can be used as a cross-linking agent to undergo a cross-linking reaction with metal ions, and powder II is added to the sodium alginate / ionic liquid aqueous solution and stirred for reaction for 1 to 10 hours, so that the metal ions and sodium alginate are fully cross-linked; sodium alginate is used as a carbon source, and after calcination in an inert atmosphere, a uniformly distributed carbon material is obtained, which can not only improve electron transport, but also increase the cycle stability of the electrode material; boron-containing ionic liquids can effectively dope titanates with boron, thereby improving their electrical conductivity and sodium storage properties, so that the prepared boron-doped metal ion-pillared layered titanate / carbon composite electrode shows good application potential in the field of sodium ion batteries.
[0023] Furthermore, compounding with carbon materials with excellent conductivity and doping (such as boron, phosphorus, etc.) are common methods for improving the sodium storage performance of layered titanates. At the same time, the use of ion pillaring materials embedded in the interlayer of layered titanates can effectively regulate their interlayer spacing and electronic structure, resulting in faster sodium storage kinetics, and prevent interlayer stacking to enhance cycle stability. In addition, the synergistic effect of metal ions and layered titanates can effectively enhance sodium storage kinetics. Therefore, in view of the shortcomings of layered titanates, the present invention uses sodium alginate as a carbon source, ionic liquids as dopants, and metal ions as pillaring materials to prepare a boron-doped metal ion pillared layered titanate / carbon composite material with excellent sodium storage performance.
[0024] The present invention provides an application of a boron-doped metal ion pillared layered titanate / carbon composite material on a negative electrode of a sodium ion battery. The obtained boron-doped metal ion pillared layered titanate / carbon composite material has the characteristics of a simple preparation method and adjustable layered titanate interlayer spacing. The sodium ion battery negative electrode prepared by mixing with acetylene black and PVDF shows good rate performance. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] The drawings in the specification are used to provide further understanding of the present invention and constitute a part of the present invention. The schematic embodiments of the present invention and their descriptions are used to explain the present invention and do not constitute improper limitations on the present invention.
[0026] Figure 1 This is a rate performance diagram of the boron-doped manganese ion-pillared layered titanate / carbon prepared in Example 1 as the negative electrode of a sodium ion battery.
[0027] Figure 2 This is a scanning electron microscope image of the boron-doped tin ion pillared layered titanate / carbon composite material prepared in Example 5. DETAILED DESCRIPTION
[0028] The embodiments of the present invention are described in further detail below:
[0029] A method for boron-doped metal ion pillared layered titanate / carbon composite material, characterized by comprising the following steps:
[0030] 1) Take 0.1g of commercial TiO 2 The powder is added into 50 mL of 1-10 mol / L KOH aqueous solution or NaOH aqueous solution and stirred evenly, and then reacted at room temperature to 200°C for 5-24 h. The white precipitate is filtered and washed with deionized water for 3 times, and then dried at 80°C for 24 h to obtain powder I.
[0031] 2) Add one of the metal salts selected from manganese chloride, magnesium chloride, tin chloride, bismuth chloride, etc., to 50 mL of water to prepare a solution having a metal ion concentration of 0.1 to 1 mol / L, add the powder I obtained in step 1) to the metal ion aqueous solution and stir for 1 to 10 h, filter and wash the precipitate with deionized water for 3 times, and dry it at 80° C. for 24 h to obtain powder II.
[0032] 3) Add 1-10 g of sodium alginate to 500 mL of water, stir at room temperature until the sodium alginate is dissolved, then add ionic liquid: one of 1-butyl-3-methylimidazolium tetrafluoroborate, 1-hexadecyl-3-methylimidazolium tetrafluoroborate, 1-(2-hydroxyethyl)-3-imidazole tetrafluoroborate, etc., the mass of the ionic liquid is 0.1-1% of the sodium alginate, stir for 10 minutes to obtain a sodium alginate / ionic liquid aqueous solution, add the powder II obtained in step 2) to the sodium alginate / ionic liquid aqueous solution, stir and react for 1-10 hours, so that the metal ions and sodium alginate are fully cross-linked, after the reaction is completed, the precipitate is filtered and washed with deionized water for 3 times, and then dried at 80° C. for 24 hours to obtain powder III.
[0033] 4) The powder III prepared in step 3) is calcined in an argon or nitrogen atmosphere at a temperature of 500-900° C., with a heating rate of 3° C. / min and a holding time of 1-5 h to obtain a boron-doped metal ion pillared layered titanate / carbon composite material.
[0034] 5) The prepared boron-doped metal ion pillared layered titanate / carbon composite material is mixed with acetylene black and PVDF in a mass ratio of 8:1:1 to prepare a negative electrode, and a sodium ion battery is assembled.
[0035] 6) Conduct electrochemical performance tests on the assembled sodium ion battery.
[0036] The boron-doped metal ion pillared layered titanate / carbon composite material prepared by the above method has the characteristics of simple preparation method and adjustable layer spacing of layered titanate, and shows good application potential in the field of sodium ion batteries.
[0037] The present invention is described in further detail below in conjunction with embodiments:
[0038] Example 1
[0039] 1) Take 0.1g of commercial TiO 2 The powder was added into 50 mL of 1 mol / L KOH aqueous solution or NaOH aqueous solution and stirred evenly, and then reacted at 200°C for 24 h. The white precipitate was filtered and washed with deionized water for 3 times, and then dried at 80°C for 24 h to obtain powder I.
[0040] 2) manganese chloride was added to 50 mL of water to prepare a solution with a metal ion concentration of 0.1 mol / L, the powder I prepared in step 1) was added to the metal ion aqueous solution and stirred for 10 h, the precipitate was filtered and washed three times with deionized water, and then dried at 80° C. for 24 h to obtain powder II.
[0041] 3) Add 10 g of sodium alginate to 500 mL of water, stir at room temperature until the sodium alginate is dissolved, then add 1-butyl-3-methylimidazolium tetrafluoroborate, the mass of which is 0.1% of the sodium alginate, and stir for 10 min to obtain a sodium alginate / 1-butyl-3-methylimidazolium tetrafluoroborate aqueous solution. Add the powder II obtained in step 2) to the sodium alginate / 1-butyl-3-methylimidazolium tetrafluoroborate aqueous solution and stir to react for 10 h to allow the manganese ions and sodium alginate to be fully cross-linked. After the reaction, filter and wash the precipitate with deionized water for 3 times, and then dry it at 80° C. for 24 h to obtain powder III.
[0042] 4) The powder III prepared in step 3) is calcined in an argon atmosphere at a temperature of 500° C., with a heating rate of 3° C. / min and a holding time of 5 h to obtain a boron-doped manganese ion-pillared layered titanate / carbon composite material.
[0043] 5) The prepared boron-doped manganese ion-pillared layered titanate / carbon composite material is mixed with acetylene black and PVDF in a mass ratio of 8:1:1 to prepare a negative electrode, and a sodium ion battery is assembled.
[0044] 6) Conduct electrochemical performance tests on the assembled sodium ion battery.
[0045] Figure 1 This is a rate performance diagram of the boron-doped manganese ion pillared layered titanate / carbon composite material prepared in Example 1 as a sodium ion battery. It can be seen from the figure that the material exhibits excellent sodium storage performance.
[0046] Example 2
[0047] 1) Take 0.1g of commercial TiO 2 The powder was added into 50 mL of 10 mol / L KOH aqueous solution or NaOH aqueous solution and stirred evenly, and then reacted at room temperature for 24 h. The white precipitate was filtered and washed with deionized water for 3 times, and then dried at 80 °C for 24 h to obtain powder I.
[0048] 2) bismuth chloride was added to 50 mL of water to prepare a solution with a metal ion concentration of 1 mol / L, the powder I obtained in step 1) was added to the metal ion aqueous solution and stirred for 1 h, the precipitate was filtered and washed 3 times with deionized water, and then dried at 80° C. for 24 h to obtain powder II.
[0049] 3) Add 10 g of sodium alginate to 500 mL of water, stir at room temperature until the sodium alginate is dissolved, then add 1-butyl-3-methylimidazolium tetrafluoroborate, the mass of which is 0.1% of the sodium alginate, and stir for 10 minutes to obtain a sodium alginate / 1-butyl-3-methylimidazolium tetrafluoroborate aqueous solution. Add the powder II obtained in step 2) to the sodium alginate / ionic liquid aqueous solution and stir for 1 hour to allow the bismuth ions and sodium alginate to be fully cross-linked. After the reaction is completed, the precipitate is filtered and washed with deionized water for 3 times, and then dried at 80° C. for 24 hours to obtain powder III.
[0050] 4) The powder III prepared in step 3) is calcined in an argon atmosphere at a temperature of 500° C., with a heating rate of 3° C. / min and a holding time of 2 h to obtain a boron-doped bismuth ion-pillared layered titanate / carbon composite material.
[0051] 5) The prepared boron-doped bismuth ion-pillared layered titanate / carbon composite material is mixed with acetylene black and PVDF in a mass ratio of 8:1:1 to prepare a negative electrode, and a sodium ion battery is assembled.
[0052] 6) Conduct electrochemical performance tests on the assembled sodium ion battery.
[0053] Example 3
[0054] 1) Take 0.1g of commercial TiO 2 The powder was added into 50 mL of 2 mol / L KOH aqueous solution or NaOH aqueous solution and stirred evenly, and then reacted at 150°C for 12 h. The white precipitate was filtered and washed with deionized water for 3 times, and then dried at 80°C for 24 h to obtain powder I.
[0055] 2) Magnesium chloride was added to 50 mL of water to prepare a solution with a metal ion concentration of 0.5 mol / L. The powder I prepared in step 1) was added to the metal ion aqueous solution and stirred for 5 h. The precipitate was filtered and washed three times with deionized water, and then dried at 80° C. for 24 h to obtain powder II.
[0056] 3) Add 5 g of sodium alginate to 500 mL of water, stir at room temperature until the sodium alginate is dissolved, then add 1-hexadecyl-3-methylimidazolium tetrafluoroborate, the mass of which is 0.5% of the sodium alginate, and stir for 10 min to obtain a sodium alginate / 1-hexadecyl-3-methylimidazolium tetrafluoroborate aqueous solution. Add the powder II obtained in step 2) to the sodium alginate / ionic liquid aqueous solution and stir for 5 h to allow the magnesium ions and sodium alginate to fully crosslink. After the reaction, filter and wash the precipitate with deionized water for 3 times, and then dry it at 80° C. for 24 h to obtain powder III.
[0057] 4) The powder III prepared in step 3) was calcined in a nitrogen atmosphere at 550° C., with a heating rate of 3° C. / min and a holding time of 2 h to obtain a boron-doped magnesium ion-pillared layered titanate / carbon composite material.
[0058] 5) The prepared boron-doped magnesium ion pillared layered titanate / carbon composite material is mixed with acetylene black and PVDF in a mass ratio of 8:1:1 to prepare a negative electrode, and a sodium ion battery is assembled.
[0059] 6) Conduct electrochemical performance tests on the assembled sodium ion battery.
[0060] Example 4
[0061] 1) Take 0.1g of commercial TiO 2 The powder was added into 50 mL of 2 mol / L KOH aqueous solution or NaOH aqueous solution and stirred evenly, and then reacted at 150°C for 5 h. The white precipitate was filtered and washed with deionized water for 3 times, and then dried at 80°C for 5 h to obtain powder I.
[0062] 2) Add tin chloride to 50 mL of water to prepare a solution with a metal ion concentration of 0.5 mol / L, add the powder I prepared in step 1) to the metal ion aqueous solution and stir for 5 h, filter and wash the precipitate with deionized water for 3 times, and dry it at 80° C. for 24 h to obtain powder II.
[0063] 3) 1 g of sodium alginate was added to 500 mL of water, and the mixture was stirred at room temperature until the sodium alginate was dissolved. Then, 1-(2-hydroxyethyl)-3-imidazole tetrafluoroborate was added, the mass of which was 1% of the sodium alginate. After stirring for 10 min, a sodium alginate / 1-(2-hydroxyethyl)-3-imidazole tetrafluoroborate aqueous solution was obtained. The powder II obtained in step 2) was added to the sodium alginate / ionic liquid aqueous solution and stirred for reaction for 5 h to allow the tin ions and the sodium alginate to be fully cross-linked. After the reaction, the precipitate was filtered and washed with deionized water for 3 times, and then dried at 80° C. for 24 h to obtain powder III.
[0064] 4) The powder III prepared in step 3) is calcined in a nitrogen atmosphere at 600° C., with a heating rate of 3° C. / min and a holding time of 2 h to obtain a boron-doped tin ion-pillared layered titanate / carbon composite material.
[0065] 5) The prepared boron-doped tin ion pillared layered titanate / carbon composite material is mixed with acetylene black and PVDF in a mass ratio of 8:1:1 to prepare a negative electrode, and a sodium ion battery is assembled.
[0066] 6) Conduct electrochemical performance tests on the assembled sodium ion battery.
[0067] Example 5
[0068] 1) Take 0.1g of commercial TiO 2 The powder was added into 50 mL of 2 mol / L KOH aqueous solution or NaOH aqueous solution and stirred evenly, and then reacted at room temperature for 5 h. The white precipitate was filtered and washed with deionized water for 3 times, and then dried at 80 °C for 5 h to obtain powder I.
[0069] 2) Add tin chloride to 50 mL of water to prepare a solution with a metal ion concentration of 0.5 mol / L, add the powder I prepared in step 1) to the metal ion aqueous solution and stir for 5 h, filter and wash the precipitate with deionized water for 3 times, and dry it at 80° C. for 24 h to obtain powder II.
[0070] 3) Add 2 g of sodium alginate to 500 mL of water, stir at room temperature until the sodium alginate is dissolved, then add 1-hexadecyl-3-methylimidazolium tetrafluoroborate, the mass of which is 0.8% of the sodium alginate, and stir for 10 minutes to obtain a sodium alginate / 1-hexadecyl-3-methylimidazolium tetrafluoroborate aqueous solution. Add the powder II obtained in step 2) to the sodium alginate / ionic liquid aqueous solution and stir for 5 hours to allow the tin ions and sodium alginate to fully crosslink. After the reaction, filter and wash the precipitate with deionized water for 3 times, and then dry it at 80° C. for 24 hours to obtain powder III.
[0071] 4) The powder III prepared in step 3) is calcined in a nitrogen atmosphere at 900° C., with a heating rate of 3° C. / min and a holding time of 1 h to obtain a boron-doped tin ion-pillared layered titanate / carbon composite material.
[0072] 5) The prepared boron-doped tin ion pillared layered titanate / carbon composite material is mixed with acetylene black and PVDF in a mass ratio of 8:1:1 to prepare a negative electrode, and a sodium ion battery is assembled.
[0073] 6) Conduct electrochemical performance tests on the assembled sodium ion battery.
[0074] Figure 2 This is a scanning electron microscope image of the boron-doped tin ion pillared layered titanate / carbon composite material prepared in Example 5. From the image, it can be seen that the obtained composite is in the form of nanoparticles with uniform size.
[0075] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention rather than to limit its protection scope. Although the present invention has been described in detail with reference to the above embodiments, ordinary technicians in the field should understand that after reading the present invention, those skilled in the art can still make various changes, modifications or equivalent substitutions to the specific implementation methods of the invention, but these changes, modifications or equivalent substitutions are all within the protection scope of the pending claims of the invention.
Claims
1. A method for preparing a boron-doped metal ion pillared layered titanate / carbon composite material, characterized in that: The following steps are involved: 1) Take TiO2 powder, add it into KOH aqueous solution or NaOH aqueous solution, stir evenly and heat to react, filter and wash the product with deionized water, and dry it to obtain powder I; 2) adding a metal salt into water to prepare a metal ion aqueous solution, adding the powder I obtained in step 1) into the metal ion aqueous solution and stirring, filtering and washing the product with deionized water, and drying to obtain a powder II; 3) adding sodium alginate to water, stirring at room temperature until the sodium alginate is dissolved, then adding ionic liquid, stirring to obtain a sodium alginate / ionic liquid aqueous solution, adding the powder II obtained in step 2) to the sodium alginate / ionic liquid aqueous solution, stirring to react, and after the reaction is completed, filtering and washing the product with deionized water, and drying to obtain powder III; 4) calcining the powder III prepared in step 3) to obtain a boron-doped metal ion pillared layered titanate / carbon composite material; The ionic liquid in step 3) is one of 1-butyl-3-methylimidazolium tetrafluoroborate, 1-hexadecyl-3-methylimidazolium tetrafluoroborate and 1-(2-hydroxyethyl)-3-imidazole tetrafluoroborate; Step 3) 1-10 g of sodium alginate is added to every 500 mL of water, the mass of the ionic liquid is 0.1-1% of the mass of the sodium alginate, the stirring time for obtaining the sodium alginate / ionic liquid aqueous solution is 10 min, and the powder II is added to the sodium alginate / ionic liquid aqueous solution and the stirring reaction time is 1-10 h.
2. The method for preparing a boron-doped metal ion pillared layered titanate / carbon composite material according to claim 1, characterized in that: In step 1), 0.1 g of TiO2 powder is added to every 50 mL of KOH aqueous solution or NaOH aqueous solution, and the heating reaction is carried out at a temperature between room temperature and 200° C. for 5 to 24 hours.
3. The method for preparing a boron-doped metal ion pillared layered titanate / carbon composite material according to claim 1, characterized in that: The concentration of the KOH aqueous solution or the NaOH aqueous solution in step 1) is 1-10 mol / L.
4. The method for preparing a boron-doped metal ion pillared layered titanate / carbon composite material according to claim 1, characterized in that: In step 2), the metal salt is one of manganese chloride, magnesium chloride, tin chloride and bismuth chloride, and the metal ion concentration of the metal ion aqueous solution is 0.1-1 mol / L.
5. The method for preparing a boron-doped metal ion pillared layered titanate / carbon composite material according to claim 1, characterized in that: The drying conditions in steps 1), 2) and 3) are drying at 80° C. for 24 hours.
6. The method for preparing a boron-doped metal ion pillared layered titanate / carbon composite material according to claim 1, characterized in that: The calcination in step 4) is carried out in an argon or nitrogen atmosphere at a temperature of 500 to 900° C., the heating rate of the calcination is 3° C. / min, and the holding time is 1 to 5 hours.
7. A boron-doped metal ion pillared layered titanate / carbon composite material, characterized in that: The method is prepared by the preparation method according to any one of claims 1 to 6.
8. Use of the boron-doped metal ion pillared layered titanate / carbon composite material according to claim 7 in a negative electrode of a sodium ion battery, characterized in that: The boron-doped metal ion pillared layered titanate / carbon composite material was mixed with acetylene black and PVDF in a mass ratio of 8:1:1 to prepare a sodium ion battery negative electrode.