Isocyanate modified polyimide resin, resin composition and hardened product thereof
Through the specific structural design of isocyanate modified polyimide resin, the problem of poor balance of multiple properties in existing resins is solved, and the high performance requirements of printed circuit boards are achieved, including low dielectric characteristics, excellent adhesion and heat resistance. sex.
Patent Information
- Application Number
- CN202180046713.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2020-12-22
- Filing Date
- 2021-06-25
- Publication Date
- 2024-11-05
- Estimated Expiration
- 2041-06-25
AI Technical Summary
Existing polyimide resins have excellent performance in low loss tangency, but the balance between processability, flexibility, heat resistance, adhesion and mechanical characteristics is poor, making it difficult to meet the requirements of printed circuit boards for multiple performances. .
Isocyanate modified polyimide resin is used to form a resin combination with a specific structure by reacting the polyimide resin with a diisocyanate compound, an aliphatic diamine compound, a tetrabasic dianhydride and an aromatic diamine compound. , optimize its terminal functional groups to improve the dielectric coefficient and loss characteristics of the hardened substance.
The resin composition has high processability, low dielectric properties, excellent adhesion, heat resistance and mechanical properties, and is suitable for high-performance printed circuit boards.
Smart Images

Figure FDA0005060175270000011 
Figure FDA0005060175270000012 
Figure FDA0005060175270000031
Abstract
Description
Technical Field
[0001] The present invention relates to an isocyanate-modified polyimide resin with a novel structure, a resin composition containing the polyimide resin, and a cured product of the resin composition. Background Art
[0002] Printed circuit boards are indispensable components of electronic devices such as smartphones and tablets, communication base station devices, computers, and car navigation systems. Printed circuit boards use various resin materials that have excellent properties such as adhesion to low-roughness metal foils, heat resistance, and flexibility.
[0003] In recent years, the development of high-speed and large-capacity next-generation high-frequency wireless printed circuit boards requires, in addition to the above characteristics, low transmission loss of resin materials, that is, low dielectric and low loss tangent.
[0004] Polyimide resins having excellent properties such as heat resistance, flame retardancy, flexibility, electrical properties, and chemical resistance are widely used in electrical / electronic parts, semiconductors, communication equipment and circuit parts thereof, peripheral equipment, etc. On the other hand, hydrocarbon compounds such as petroleum or natural oil are known to have high insulation and low dielectric constants, and Patent Documents 1 to 4 describe polyimide resins having a long-chain alkylene skeleton derived from dimer diamine introduced into the structure in order to exert such high insulation and low dielectric constant properties.
[0005] However, although the polyimide resins described in these patent documents are excellent in terms of low loss tangent, they are poorly balanced in various properties such as processability, flexibility, heat resistance, adhesion, and mechanical properties.
[0006] [Prior art literature]
[0007] [Patent Document]
[0008] Patent Document 1: Japanese Patent No. 5534378
[0009] Patent Document 2: Japanese Patent No. 6488170
[0010] Patent Document 3: Japanese Patent No. 6635403
[0011] Patent document 4: Japanese Patent No. 6082439. Summary of the invention
[0012] [Problems to be solved by the invention]
[0013] An object of the present invention is to provide a resin material suitable for a novel structure of a printed circuit board, and a resin composition containing the resin material, wherein the resin composition has excellent processability, and its cured product has low dielectric constant and loss tangent, and has excellent adhesion, heat resistance and mechanical properties.
[0014] [Methods to solve the problem]
[0015] As a result of intensive research, the present inventors have found that a resin composition containing a novel polyimide resin with a specific structure can solve the above-mentioned problems, thereby completing the present invention.
[0016] That is, the present invention is as follows.
[0017] (1) An isocyanate-modified polyimide resin, which is a reaction product of a polyimide resin and a diisocyanate compound (a) having an isocyanate group, and has an amine group and / or anhydride group at both ends. The polyimide resin is a reaction product of an aliphatic diamine compound (b), a tetrabasic acid dianhydride (c), and an aromatic diamine compound (d), and has an amine group and / or anhydride group.
[0018] (2) The isocyanate-modified polyimide resin according to the above item (1), wherein the diisocyanate compound (a) contains at least one selected from the group consisting of hexamethylene diisocyanate, trimethylhexamethylene diisocyanate, and isophorone diisocyanate.
[0019] (3) The isocyanate-modified polyimide resin according to the above item (1) or (2), wherein the aliphatic diamine compound (b) contains at least one aliphatic diamine compound having 6 to 36 carbon atoms.
[0020] (4) The isocyanate-modified polyimide resin according to any one of the above items (1) to (3), wherein the tetrabasic acid dianhydride (c) contains at least one selected from the group consisting of the following formulae (1) to (4).
[0021]
[0022] (In formula (4), Y represents C(CF3)2, SO2, CO, O, a direct bond, or a divalent linking group represented by the following formula (5))
[0023]
[0024] (5) The isocyanate-modified polyimide resin according to any one of the above items (1) to (4), wherein the aromatic diamine compound (d) contains at least one selected from the group consisting of the following formulae (6) and (8).
[0025]
[0026] (In formula (6), R1 represents a methyl group or a trifluoromethyl group, in formula (8), Z represents CH(CH3), C(CF3)2, SO2, CH2, O-C6H4-O, O, a direct bond, or a divalent linking group represented by the following formula (9), and R3 represents a hydrogen atom, a methyl group, an ethyl group, a hydroxyl group, or a trifluoromethyl group)
[0027]
[0028] (6) A terminal-modified isocyanate-modified polyimide resin, which is a reaction product of an isocyanate-modified polyimide resin having an amine group and / or an acid anhydride group at both ends as described in any one of the preceding items (1) to (5) and a compound having a functional group that can react with the aforementioned amine group or the aforementioned acid anhydride group.
[0029] (7) A resin composition comprising the isocyanate-modified polyimide resin according to any one of (1) to (5) above, and a compound reactive with the isocyanate-modified polyimide resin.
[0030] (8) A resin composition comprising the terminal-modified isocyanate-modified polyimide resin as described in the above item (6) and a compound that reacts with the terminal-modified isocyanate-modified polyimide resin.
[0031] (9) The resin composition as described in the above item (7) or (8), wherein the compound reactive with the aforementioned isocyanate-modified polyimide resin or the compound reactive with the aforementioned terminal-modified isocyanate-modified polyimide resin contains at least one compound having a maleimide group.
[0032] (10) A resin composition comprising the isocyanate-modified polyimide resin according to any one of (1) to (5) above, and a compound that does not react with the isocyanate-modified polyimide resin.
[0033] (11) A resin composition comprising the terminal-modified isocyanate-modified polyimide resin as described in the above item (6) and a compound that does not react with the terminal-modified isocyanate-modified polyimide resin.
[0034] (12) A cured product, which is a cured product of the resin composition according to any one of the above items (7) to (11).
[0035] (13) A substrate comprising the cured product according to the above item (12).
[0036] [Effects of the invention]
[0037] By using the resin composition containing the isocyanate-modified polyimide resin with a specific structure of the present invention, printed circuit boards and the like having excellent heat resistance, mechanical properties, low dielectric properties, and adhesiveness can be provided. Detailed Description of the Invention
[0038] The isocyanate-modified polyimide resin of the present invention is a reaction product of an amino group and / or an acid anhydride group present at both ends of a polyimide resin and an isocyanate group of a diisocyanate compound (a) (hereinafter also simply referred to as "(a) component"), and has an amino group and / or an acid anhydride group at both ends. The polyimide resin is a reaction product of an aliphatic diamine compound (b) (hereinafter also simply referred to as "(b) component"), a tetracarboxylic dianhydride (c) (hereinafter also simply referred to as "(c) component"), and an aromatic diamine compound (d) (hereinafter also simply referred to as "(d) component") (hereinafter, the polyimide resin of the reaction product of (b) to (d) components is referred to as "intermediate polyimide resin").
[0039] [Intermediate Polyimide Resin]
[0040] First, the intermediate polyimide resin will be described.
[0041] The reaction of (b) to (d) components includes a step of obtaining a polyamic acid by a copolymerization reaction of an amino group in (b) and (d) components and an acid anhydride group in (c) component; and a step of obtaining an intermediate polyimide resin by a dehydration cyclization reaction (imidization reaction) of the polyamic acid. The above two steps can be carried out separately, but it is more efficient to carry them out continuously at once.
[0042] When the molar number MB of (b) component, the molar number MC of (c) component, and the molar number MD of (d) component used in the copolymerization reaction satisfy the relationship of MB + MD > MC, the two ends of the obtained intermediate polyimide resin will be amino groups. When they satisfy the relationship of MB + MD < MC, the two ends of the obtained intermediate polyimide resin will be acid anhydride groups. In addition, when they satisfy the relationship of MB + MD = MC, the theoretically molecular weight of the obtained intermediate polyimide resin is infinite, and one amino group and one acid anhydride group are respectively present at both ends.
[0043] The amount of the component (b) used in the copolymerization reaction is not particularly limited, but is preferably in the range of 10 to 50% by mass of the total mass of the components (b) to (d) used in the synthesis step of the intermediate polyimide resin and the component (a) used in the synthesis step of the isocyanate-modified polyimide resin described later, excluding the mass of water generated in the dehydration cyclization reaction step during the synthesis of the intermediate polyimide resin (the mass is substantially equal to the mass of the isocyanate-modified polyimide resin finally obtained). If the amount of the component (b) is less than the above range, the proportion of aliphatic chains derived from the component (b) in the intermediate polyimide resin is too small, and the dielectric constant and loss tangent become high. If it is greater than the above range, the proportion of aliphatic chains derived from the component (b) in the intermediate polyimide resin is too large, and the heat resistance of the cured product is reduced.
[0044] The component (b) used in the synthesis of the intermediate polyimide resin is not particularly limited as long as it is an aliphatic compound having two amine groups in one molecule, but is preferably an aliphatic diamine compound having 6 to 36 carbon atoms. Specific examples of the component (b) include hexamethylenediamine, 1,3-bis(aminomethyl)cyclohexane, C14 branched diamine, C18 branched diamine, dimer diamine, and diaminopolysiloxane. These can be used alone or in combination of two or more.
[0045] The dimer diamine described in the specific example of component (b) is obtained by replacing two carboxyl groups of dimer acid of dimer of unsaturated fatty acid such as oleic acid with primary amino groups in this specification (see Japanese Patent Application Laid-Open No. 9-12712, etc.). Specific examples of commercially available dimer diamines include PRIAMINE 1074 and PRIAMINE 1075 (both manufactured by CRODA JAPAN Co., Ltd.), and VERSAMINE 551 (manufactured by Cognis JAPAN Co., Ltd.). These can be used alone or in combination of two or more.
[0046] The component (c) used in the synthesis of the intermediate polyimide resin is not particularly limited as long as it has two anhydride groups in one molecule. Specific examples of the component (c) include pyromelitic anhydride, ethylene glycol bis(anhydrotrimellitate), glycerol bis(anhydrotrimellitate) monoacetate, 1,2,3,4-butanetetracarboxylic dianhydride, 3,3',4,4'-diphenylsulfonetetracarboxylic dianhydride, 3,3',4,4'-diphenyl ketonetetracarboxylic dianhydride, 3,3',4,4'-biphenyltetracarboxylic dianhydride, 3,3',4,4'-diphenylethertetracarboxylic dianhydride, 5-(2,5-dioxotetrahydro-3-furanyl)-3-methylcyclohexene- 1,2-dicarboxylic anhydride, 3a,4,5,9b-tetrahydro-5-(tetrahydro-2,5-dioxo-3-furanyl)-1,3-dione, 1,2,4,5-cyclohexanetetracarboxylic anhydride, bicyclo(2,2,2)-oct-7-ene-2,3,5,6-tetracarboxylic anhydride and bicyclo[2.2.2]octane-2,3,5,6-tetracarboxylic anhydride, 5,5'-((propane-2,2-diylbis(4,1-phenylene))bis(oxy))bis(isobenzofuran-1,3-dione), and the like. Among them, 3,3',4,4'-diphenylsulfone tetracarboxylic dianhydride, 3,3',4,4'-diphenyl ketone tetracarboxylic dianhydride, 3,3',4,4'-biphenyl tetracarboxylic dianhydride or 3,3',4,4'-diphenyl ether tetracarboxylic dianhydride is more preferred in terms of solvent solubility, adhesion to substrates and photosensitivity.
[0047] The component (c) used for synthesizing the intermediate polyimide resin preferably contains at least one compound selected from the group consisting of the following formulae (1) to (4).
[0048]
[0049] In formula (4), Y represents C(CF3)2, SO2, CO, O, a direct bond, or a divalent linking group represented by the following formula (5). In addition, the two linking parts represented by formula (5) are parts that are respectively bonded to 2-benzofuran.
[0050]
[0051] The component (d) used in the synthesis of the intermediate polyimide resin is not particularly limited as long as it is an aromatic compound having two amine groups in one molecule. Specific examples of the component (d) include m-phenylenediamine, p-phenylenediamine, m-toluenediamine, 4,4'-diaminodiphenyl ether, 3,3'-dimethyl-4,4'-diaminodiphenyl ether, 3,4'-diaminodiphenyl ether, 4,4'-diaminodiphenyl sulfide, 3,3'-dimethyl-4,4'-diaminodiphenyl sulfide, 3,3'-diethoxy-4,4'-diaminodiphenyl sulfide, 3,3'-diaminodiphenyl ether, 4,4'-diaminodiphenyl sulfide, 3,3'-dimethyl-4,4'-diaminodiphenyl sulfide, 3,3'-diaminodiphenyl ether, 4,4'-diaminodiphenyl sulfide ... 4,4'-diaminodiphenyl ketone, 3,3'-dimethyl-4,4'-diaminodiphenyl ketone, 3,3'-diaminodiphenylmethane, 4,4'-diaminodiphenylmethane, 3,4'-diaminodiphenylmethane, 3,3'-dimethoxy-4,4'-diaminodiphenyl sulfide, 2,2'-bis(3-aminophenyl)propane, 2,2'-bis(4-aminophenyl)propane, 4,4 '-Diaminodiphenyl sulfoxide, 3,3'-diaminodiphenyl sulfone, 4,4'-diaminodiphenyl sulfone, benzidine, 3,3'-dimethylbenzidine, 3,3'-dimethoxybenzidine, 3,3'-diaminobiphenyl, p-xylenediamine, m-xylenediamine, o-xylenediamine, 2,2'-bis(3-aminophenoxyphenyl)propane, 2,2'-bis(4-aminophenoxyphenyl)propane, 1,3-bis( 4-aminophenoxyphenyl)benzene, 1,3'-bis(3-aminophenoxyphenyl)propane, bis(4-amino-3-methylphenyl)methane, bis(4-amino-3,5-dimethylphenyl)methane, bis(4-amino-3-ethylphenyl)methane, bis(4-amino-3,5-diethylphenyl)methane, bis(4-amino-3-propylphenyl)methane, and bis(4-amino-3,5-dipropylphenyl)methane. These may be used alone or in combination of two or more.
[0052] The component (d) used for synthesizing the intermediate polyimide resin preferably contains at least one compound selected from the group consisting of the following formulae (6) and (8).
[0053]
[0054] In formula (6), R1 represents a methyl group or a trifluoromethyl group, in formula (8), Z represents CH(CH3), SO2, CH2, O-C6H4-O, O, a direct bond, or a divalent linking group represented by the following formula (9), and R3 represents a hydrogen atom, a methyl group, an ethyl group, or a trifluoromethyl group. In addition, the two linking portions represented by formula (9) are each a portion bonded to 2-benzofuran.
[0055]
[0056] The intermediate polyimide resin can be synthesized by publicly known methods.
[0057] For example, a solvent, a dehydrating agent, and a catalyst are added to the mixture of components (b) to (d) used in the synthesis, and heated and stirred at 100 to 300°C in an inert gas environment such as nitrogen, thereby producing an imidization reaction (a ring-closing reaction accompanied by dehydration) through the polyamic acid to obtain an intermediate polyimide resin solution. At this time, the water produced by the imidization is distilled out of the system, and after the reaction is completed, the dehydrating agent and the catalyst are also distilled out of the system, thereby obtaining a high-purity intermediate polyimide resin without washing. Examples of the dehydrating agent include toluene and xylene, and examples of the catalyst include pyridine and triethylamine.
[0058] Solvents that can be used in the synthesis of the intermediate polyimide resin include methyl ethyl ketone, methyl propyl ketone, methyl isopropyl ketone, methyl butyl ketone, methyl isobutyl ketone, methyl n-hexyl ketone, diethyl ketone, diisopropyl ketone, diisobutyl ketone, cyclopentanone, cyclohexanone, methylcyclohexanone, acetylacetone, γ-butyrolactone, diacetone alcohol, cyclohexene-1-one, dipropyl ether, diisopropyl ether, dibutyl ether, tetrahydrofuran, tetrahydropyran, ethyl isopentyl ether, ethyl tert-butyl ether, ethyl benzyl ether, cresyl methyl ether, anisole, phenethyl ether, methyl acetate, ethyl acetate, propyl acetate, isopropyl acetate , butyl acetate, isobutyl acetate, amyl acetate, isoamyl acetate, 2-ethylhexyl acetate, cyclohexyl acetate, methylcyclohexyl acetate, benzyl acetate, methyl acetoacetate, ethyl acetoacetate, methyl propionate, ethyl propionate, butyl propionate, benzyl propionate, methyl butyrate, ethyl butyrate, isopropyl butyrate, butyl butyrate, isoamyl butyrate, methyl lactate, ethyl lactate, butyl lactate, ethyl isovalerate, isoamyl isovalerate, diethyl oxalate, dibutyl oxalate, methyl benzoate, ethyl benzoate, propyl benzoate, methyl salicylate, N-methylpyrrolidone, N,N-dimethylformamide, N,N-dimethylacetamide, dimethyl sulfoxide, etc., but are not limited to these. These can be used alone or in combination of two or more.
[0059] [Isocyanate modified polyimide resin]
[0060] Next, the isocyanate-modified polyimide resin of the present invention will be described.
[0061] The isocyanate-modified polyimide resin of the present invention is obtained by the reaction of an intermediate polyimide resin and component (a). The reaction of the intermediate polyimide resin and component (a) is a copolymerization reaction of an amine group or an acid anhydride group at the end of the intermediate polyimide resin and an isocyanate group of component (a), and a urea bond is formed by the reaction of the amine group and the isocyanate group, and an imide bond is formed by the reaction of the acid anhydride and the isocyanate group.
[0062] The amount of component (a) used in the copolymerization reaction of the intermediate polyimide resin and component (a) is preferably less than 1 equivalent of the isocyanate group of component (a), more preferably 0.50 to 0.99 equivalents, and even more preferably 0.67 to 0.98 equivalents relative to 1 equivalent of the terminal functional group of the intermediate polyimide resin. The amount of component (a) relative to the intermediate polyimide resin is within the above range, thereby making it possible to sufficiently increase the molecular weight of the isocyanate-modified polyimide resin, reduce the residual rate of unreacted raw materials, and improve the heat resistance and flexibility of the resin composition containing the isocyanate-modified polyimide resin and the polyimide resin after curing.
[0063] In addition, the terminal functional equivalent of the intermediate polyimide resin mentioned here is a value calculated from the usage amount of each raw material when synthesizing the intermediate polyimide resin.
[0064] The (a) component used in the synthesis of the isocyanate-modified polyimide resin of the present invention can be used as long as it has 2 isocyanate groups in the molecule, and can react with multiple diisocyanate compounds at the same time. (a) component is more preferably phenylene diisocyanate, toluene diisocyanate, xylene diisocyanate, tetramethylxylene diisocyanate, diphenylmethane diisocyanate, naphthalene diisocyanate, dimethylbiphenyl diisocyanate, hexamethylene diisocyanate, dicyclohexylmethane diisocyanate, isophorone diisocyanate, arylene sulfone ether diisocyanate, allyl cyanide diisocyanate, N-acyl diisocyanate, trimethylhexamethylene diisocyanate, 1,3-bis (isocyanate methyl) cyclohexane or norbornane diisocyanate methyl. Among them, it is more preferably hexamethylene diisocyanate, trimethylhexamethylene diisocyanate or isophorone diisocyanate with excellent balance of flexibility, adhesion, etc.
[0065] The reaction of the intermediate polyimide resin and the component (a) can be carried out by a publicly known synthesis method.
[0066] Specifically, the component (a) is added to the intermediate polyimide resin solution obtained by the above-mentioned synthesis method, and heated and stirred at 80 to 150° C., thereby obtaining the isocyanate-modified polyimide resin of the present invention. In addition, the synthesis reaction of the intermediate polyimide resin and the reaction time of the intermediate polyimide resin and the component (a) are greatly affected by the reaction temperature, but the viscosity increases as the reaction proceeds and a balance is reached. It is more preferred to react until the maximum molecular weight is obtained, which is usually several tens of minutes to 20 hours.
[0067] The isocyanate-modified polyimide resin solution obtained above is put into a poor solvent such as water, methanol and hexane to separate the generated polymer, and then the solid content of the isocyanate-modified polyimide resin of the present invention can be obtained by reprecipitation.
[0068] [Terminal modified isocyanate modified polyimide resin]
[0069] The isocyanate-modified polyimide resin of the present invention has an amine group and / or anhydride group at both ends, so it reacts with a compound having a functional group that can react with these functional groups, thereby modifying the ends and preparing a terminal-modified isocyanate-modified polyimide resin. The compound that can react with the amine group and / or anhydride group can be exemplified by compounds having an anhydride group such as maleic anhydride, compounds having an alcoholic hydroxyl group such as hydroxyethyl acrylate, compounds having a phenolic hydroxyl group such as phenol, compounds having an isocyanate group such as 2-methacryloyloxyethyl isocyanate, and compounds having an epoxy group such as glycidyl methacrylate.
[0070] By modifying the ends, the two ends of the isocyanate compound of the present invention can be changed to functional groups other than amine groups and acid anhydride groups (for example, when hydroxyethyl acrylate is used for terminal modification, the ends of the isocyanate-modified polyimide resin can be changed to acryloyl groups), so it can be combined with a compound that reacts with functional groups other than amine groups or acid anhydride groups to form a composition.
[0071] [Resin composition]
[0072] The resin composition of the present invention is roughly divided into: a first aspect containing the isocyanate-modified polyimide resin of the present invention and a compound other than the isocyanate-modified polyimide resin; and a second aspect containing the terminal-modified isocyanate-modified polyimide resin of the present invention and a compound other than the terminal-modified isocyanate-modified polyimide resin.
[0073] First, the resin composition according to the first aspect of the present invention, which contains an isocyanate-modified polyimide resin and a compound other than the isocyanate-modified polyimide resin, will be described.
[0074] The compounds other than the isocyanate-modified polyimide resin contained in the first-phase resin composition are not limited to any one of the compounds that react with the isocyanate-modified polyimide resin (hereinafter referred to as the "reactive compounds of the first phase") and the compounds that do not react with the isocyanate-modified polyimide resin (hereinafter referred to as the "non-reactive compounds of the first phase").
[0075] The reactive compound of the first aspect refers to a compound that reacts with anhydride groups and / or amine groups at the ends of the isocyanate-modified polyimide resin.
[0076] Examples of the reactive compound in the first aspect that reacts with an acid anhydride group include a compound having an epoxy group, a compound having a thiol group, and a compound having an amine group. A compound having an epoxy group is more preferred.
[0077] The compound having an epoxy group is not particularly limited as long as it has one or more epoxy groups in one molecule, but is preferably a compound having two or more epoxy groups in one molecule, and examples thereof include novolac epoxy resins, bisphenol epoxy resins, biphenyl epoxy resins, triphenylmethane epoxy resins, phenol aralkyl epoxy resins, etc. Specifically, examples thereof include NC-3000, NC-7000, XD-1000, EOCN-1020, EPPN-502H (all manufactured by Nippon Kayaku Co., Ltd.), jER828 (manufactured by Mitsubishi Chemical Co., Ltd.), and jER807 (manufactured by Mitsubishi Chemical Co., Ltd.), and NC-3000 or XD-1000 are more preferred.
[0078] In the resin composition of the present invention containing a compound having an epoxy group as the reactive compound of the first state, various heat-curing catalysts may be optionally added for the purpose of promoting the curing reaction of the compound having anhydride group and epoxy group. The heat-curing catalyst may include imidazoles such as 2-methylimidazole, 2-ethylimidazole, 2-ethyl-4-methylimidazole, 2-phenyl-4,5-dihydroxymethylimidazole and 2-phenyl-4-methyl-5-hydroxymethylimidazole, tertiary amines such as 2-(dimethylaminomethyl)phenol and 1,8-diaza-bicyclo (5,4,0) undecene-7, phosphines such as triphenylphosphine, metal compounds such as tin octoate, etc. In the resin composition of the present invention containing a compound having an epoxy group, the amount of the heat-curing catalyst added is 0.1 to 10% by mass relative to the compound having an epoxy group.
[0079] In the resin composition of the present invention containing a compound having an epoxy group as the first aspect of the reactive compound, a compound having a phenolic hydroxyl group, a compound having an amine group, a compound having an acid anhydride group, and the like, which is reactive with an epoxy group, may be used in combination.
[0080] The compound having a thiol group is not particularly limited as long as it is a compound having one or more thiol groups in one molecule, but is preferably a compound having two or more thiol groups in one molecule, and examples thereof include pentaerythritol tetrakis(3-mercaptobutyrate), 1,4-bis(3-mercaptobutyryloxy)butane, 1,3,5-tris(2-(3-mercaptobutyryloxy)ethyl)-1,3,5-triazinane-2,4,6-trione, trimethylolpropane tris(3-mercaptobutyrate), trimethylolpropane trithiopropionate, and pentaerythritol tetrathiopropionate. , ethylene glycol dithioacetate, 1,4-butanediol dithioacetate, trimethylolpropane trithioacetate, pentaerythritol tetrathioacetate, bis(2-mercaptoethyl) ether, 1,4-butanediol, 1,3,5-trimercaptomethylbenzene, 1,3,5-trimercaptomethyl-2,4,6-trimethylbenzene, a polyether containing a thiol group at the end, a polythioether containing a thiol group at the end, a thiol compound obtained by the reaction of an epoxy compound with hydrogen sulfide, a thiol compound having a thiol group at the end obtained by the reaction of a polythiol compound with an epoxy compound, and the like.
[0081] Commercially available products of the compound having a thiol group include Karenz MT PE1, Karenz MT NR1, and Karenz MT BD1 (all manufactured by Showa Denko KK).
[0082] The compound having an amino group is not particularly limited as long as it has one or more amino groups in one molecule, but is preferably a compound having two or more amino groups in one molecule. Specific examples of the compound having an amino group include hexamethylenediamine, naphthalene diamine, 1,3-bis(aminomethyl)cyclohexane, isophorone diamine, 4,4'-methylenebis(cyclohexylamine), norbornane diamine, and the like.
[0083] Examples of the first aspect of the reactive compound that reacts with an amine group include a compound having a maleimide group, a compound having an epoxy group, and a compound having a carboxyl group. A compound having a maleimide group is more preferred.
[0084] The compound having a maleimide group is not particularly limited as long as it is a compound having one or more maleimide groups in one molecule, but is preferably a compound having two or more maleimide groups in one molecule, and examples thereof include a polyfunctional maleimide compound obtained by reacting 3,4,4'-triaminodiphenylmethane, triaminophenol, etc. with maleic anhydride, a tri-(4-aminophenyl)-phosphate, a tri-(4-aminophenyl)-phosphate, a tri-(4-aminophenyl)-thiophosphate, a maleimide compound obtained by reacting maleic anhydride, and a tri-maleimide compound such as tri-(4-maleimidophenyl)methane. Imine compounds, bis(3,4-dimaleimidephenyl)methane, tetramaleimide diphenyl ketone, tetramaleimide naphthalene, maleimide obtained by reacting triethylenetetramine with maleic anhydride and other tetramaleimide compounds, phenol novolac type maleimide resins, isopropylidenebis(phenoxyphenylmaleimide)phenylmaleimide aralkyl resins, biphenylene type phenylmaleimide aralkyl resins, etc. Commercially available products include MIR-3000, MIR-5000 (all manufactured by Nippon Kayaku Co., Ltd.), BMI-70, BMI-80 (all manufactured by K.I Chemical Industry Co., Ltd.), BMI-1000, BMI-2000, BMI-3000 (all manufactured by Yamato Chemical Industry Co., Ltd.), etc.
[0085] The compound having a maleimide group can self-crosslink the maleimide groups by the action of a free radical initiator. Therefore, a resin composition using an isocyanate-modified polyimide resin having an amine group at the end, a compound having a maleimide group, and a free radical initiator can self-crosslink the maleimide group by heating, and can form a cured product of a copolymer of the polyimide resin and the maleimide resin.
[0086] The free radical initiator that can be used for the self-crosslinking of maleimide groups includes peroxides such as diisopropylbenzene peroxide and dibutyl peroxide, and azo compounds such as 2,2'-azobis(isobutyronitrile) and 2,2'-azobis(2,4-dimethylvaleronitrile). In the resin composition of the present invention containing a compound having a maleimide group, the amount of the free radical initiator added is 0.1 to 10% by mass relative to the compound having a maleimide group.
[0087] Examples of the compound having an epoxy group include the same compounds as those in the above-mentioned "compound having an epoxy group in the first aspect of the reactive compound that reacts with an acid anhydride group", and the catalysts and compounds that can be used in combination are also the same.
[0088] The compound having a carboxyl group is not particularly limited as long as it is a compound having one or more carboxyl groups in one molecule, and is preferably a compound having two or more carboxyl groups in one molecule. Specific examples of the compound having a carboxyl group include straight-chain alkyl diacids such as butane dioic acid, pentane dioic acid, hexane dioic acid, heptane dioic acid, octanedioic acid, nonane dioic acid, decanedioic acid, and malic acid, alkyl tricarboxylic acids such as 1,3,5-pentanetricarboxylic acid and citric acid, phthalic acid, hexahydrophthalic acid, methylhexahydrophthalic acid, tetrahydrophthalic acid, methyltetrahydrophthalic acid, cyclohexanetricarboxylic acid, nadic acid, methylnadic acid, and the like.
[0089] The content of the reactive compound of the first aspect in the resin composition of the present invention is preferably such that the reactive group equivalent of the reactive compound of the first aspect is 0.1 to 500 equivalents relative to 1 equivalent of the terminal functional group of the isocyanate-modified polyimide resin. By making the reactive group equivalent of the reactive compound of the first aspect within the aforementioned range, a cured product of the resin composition having good properties and a good crosslinking density can be obtained. The equivalents described herein are values calculated from the amounts of the raw materials used when synthesizing the isocyanate-modified polyimide resin.
[0090] When the isocyanate-modified polyimide resin has both an acid anhydride group and an amine group at both ends, the reactive compound of the first aspect that reacts with the acid anhydride group and the reactive composition of the first aspect that reacts with the amine group may be used in combination.
[0091] The non-reactive compound of the first aspect is not particularly limited as long as it is a compound that does not react with the isocyanate-modified polyimide resin. Organic solvents and the like are also included in this category, but a resin composition containing an organic solvent is also called a "varnish", which is a more preferred aspect in applications such as improving the handling properties of the resin composition by diluting it with an organic solvent.
[0092] Specific examples of the organic solvent include amide solvents such as γ-butyrolactone, N-methylpyrrolidone, N,N-dimethylformamide, N,N-dimethylacetamide and N,N-dimethylimidazolidinone, sulfones such as tetramethylene sulfone, ether solvents such as diethylene glycol dimethyl ether, diethylene glycol diethyl ether, propylene glycol, propylene glycol monomethyl ether, propylene glycol monomethyl ether monoacetate and propylene glycol monobutyl ether, ketone solvents such as methyl ethyl ketone, methyl isobutyl ketone, cyclopentanone and cyclohexanone, and aromatic solvents such as toluene and xylene.
[0093] Usually, the organic solvent is used so that the solid content concentration in the resin composition excluding the organic solvent becomes 10 to 80 mass %, and more preferably 20 to 70 mass %.
[0094] The compound having a thiol group and the compound having an amine group described in the paragraph "The first reactive compound that reacts with an acid anhydride group" do not react with the amine group, so these compounds can be used together as the first non-reactive compound in the isocyanate-modified polyimide resin having an amine group at the end to form a resin composition. The compound having a maleimide group and the compound having a carboxyl group described in the paragraph "The first reactive compound that reacts with an amine group" do not react with the acid anhydride group, so they can be used together as the first non-reactive compound in the isocyanate-modified polyimide resin having an acid anhydride group at the end to form a resin composition.
[0095] In addition, similar to the description of the first aspect of the reactive compound having a maleimide group and the first aspect of the reactive compound having an epoxy group, the first aspect of the non-reactive compound self-crosslinking or the first aspect of the non-reactive compound copolymerizing with each other is also a preferred aspect of the resin composition of the present invention. The first aspect of the non-reactive compound is self-crosslinked or copolymerized in the resin composition to obtain a cured product of the non-reactive compound containing a non-bonded isocyanate-modified polyimide resin.
[0096] Next, a resin composition according to a second aspect of the present invention, which contains a terminally modified isocyanate-modified polyimide resin and a compound other than the terminally modified isocyanate-modified polyimide resin, will be described.
[0097] The compounds other than the terminal-modified isocyanate-modified polyimide resin contained in the resin composition of the second embodiment are not limited to any one of the compounds that react with the terminal-modified isocyanate-modified polyimide resin (hereinafter referred to as the "reactive compound of the second embodiment") and the compounds that do not react with the terminal-modified isocyanate-modified polyimide resin (hereinafter referred to as the "non-reactive compound of the second embodiment").
[0098] The second type of reactive compound refers to a compound that reacts with the functional group at the end of the terminal-modified isocyanate-modified polyimide resin. The functional group at the end of the terminal-modified isocyanate-modified polyimide resin depends on the compound used for the terminal modification. Therefore, the second type of reactive compound is a compound that takes into account the terminal functional group of the terminal-modified isocyanate-modified polyimide resin and selects a compound that reacts with it.
[0099] For example, when both ends of an isocyanate-modified polyimide resin having an amino group are modified with a tetrabasic acid dianhydride, both ends of the terminal-modified isocyanate-modified polyimide resin become anhydride groups, so the second type of reactive compound that reacts with it can be the same compound as the first type of reactive compound that reacts with the terminal anhydride group of the isocyanate-modified polyimide resin, and the catalyst or compound that can be used in combination is also the same.
[0100] In addition, when the two ends of the isocyanate-modified polyimide resin having an acid anhydride group are modified with a diamine compound, amino groups are formed at the two ends of the terminal-modified isocyanate-modified polyimide resin. Therefore, the second type of reactive compound that reacts with it can be the same compound as the first type of reactive compound that reacts with the terminal amine group of the isocyanate-modified polyimide resin.
[0101] As another example, the terminal modification of the isocyanate-modified polyimide resin uses epoxy resin, a compound having a maleimide group (including maleimide resin), isocyanate resin, allyl resin, benzoxazine resin, and acryl resin to obtain a terminal-modified isocyanate-modified polyimide resin, wherein the terminals thereof respectively form an epoxy group, a maleimide group, an isocyanate group, an allyl group, a benzoxazine group, and an acryl group, so that the compound that reacts with these terminal functional groups can be used as the reactive compound of the second state, and a catalyst generally used when the aforementioned terminal functional groups react with the reactive compound can be used in combination.
[0102] In the terminal modified isocyanate modified polyimide resin having an acryloyl group at the end, the reactive compound of the second aspect is preferably a compound having an acryloyl group. Specific examples thereof include (meth)acrylic acid alkyl esters such as 2-ethylhexyl (meth)acrylate and cyclohexyl (meth)acrylate; (meth)acrylic acid hydroxyalkyl esters such as 2-hydroxyethyl (meth)acrylate and 2-hydroxypropyl (meth)acrylate; mono- or di-(meth)acrylates of alkylene oxide derivatives such as ethylene glycol, propylene glycol, diethylene glycol, and dipropylene glycol; polyols such as hexanediol, trimethylolpropane, pentaerythritol, ditrimethylolpropane, dipentaerythritol, trihydroxyethyl isocyanurate, or ethylene oxide derivatives thereof. The invention also includes polyvalent (meth)acrylates of ethylene oxide or propylene oxide adducts of phenols such as phenoxyethyl (meth)acrylate and polyethoxy di(meth)acrylate of bisphenol A; (meth)acrylates of glycidyl ethers such as glycerol diglycidyl ether, trimethylolpropane triglycidyl ether and triglycidyl isocyanurate; and melamine (meth)acrylate, etc., and polymerization initiators that can be used for the (co)polymerization of compounds having an acryloyl group can be used in combination.
[0103] The content of the reactive compound of the second aspect in the resin composition of the present invention is preferably an amount that makes the reactive group equivalent of the reactive compound of the second aspect 0.1 to 500 equivalents relative to 1 equivalent of the terminal functional group of the terminal-modified isocyanate-modified polyimide resin. By making the reactive group equivalent of the reactive compound of the second aspect within the aforementioned range, a cured product of the resin composition having good properties and a good crosslinking density can be obtained. The equivalents described herein are values calculated from the amounts of the raw materials used when synthesizing the terminal-modified isocyanate-modified polyimide resin.
[0104] When the terminal-modified isocyanate-modified polyimide resin has different functional groups at both terminals, a plurality of reactive compounds of the second aspect that react with the respective functional groups may be used in combination.
[0105] The non-reactive compound of the second aspect is not particularly limited as long as it is a compound that does not react with the terminal modified isocyanate modified polyimide resin. Organic solvents and the like are also included in this category, but a resin composition containing an organic solvent is also called a "varnish", which is a more preferred aspect in the use of improving the handling properties of the resin composition by diluting it with an organic solvent.
[0106] Specific examples of the organic solvent and the content of the organic solvent in the resin composition are the same as the organic solvent and the content described in the paragraph of the non-reactive compound of the first aspect.
[0107] The resin composition of the present invention may optionally be used in combination with publicly known additives. Specific examples of additives that can be used in combination include epoxy resin hardeners, polybutadiene and modified products thereof, modified products of acrylonitrile copolymers, polyphenylene ethers, polystyrene, polyethylene, polyimides, fluororesins, maleimide compounds, cyanate compounds, silicone gels, silicone oils, and inorganic fillers such as silica, alumina, calcium carbonate, quartz powder, aluminum powder, graphite, talc, clay, iron oxide, titanium oxide, aluminum nitride, asbestos, mica, and glass powder, surface treatment agents for fillers such as silane coupling agents, mold release agents, carbon black, phthalocyanine blue, phthalocyanine green, and other colorants. The amount of these additives blended is preferably 1,000 parts by mass or less, and more preferably 700 parts by mass or less, relative to 100 parts by mass of the resin composition.
[0108] The curing temperature and curing time of the resin composition of the present invention can be selected by considering the combination of the functional groups at both ends of the (terminal-modified) isocyanate-modified polyimide resin and the reactive groups of the reactive compound. For example, the curing temperature of a resin composition containing a maleimide resin or a resin composition containing an epoxy resin is preferably 120 to 250° C., and the curing time is approximately tens of minutes to several hours.
[0109] The preparation method of the resin composition of the present invention is not particularly limited, and the components may be simply mixed uniformly or prepolymerized. For example, the (terminal modified) isocyanate-modified polyimide resin of the present invention and the reactive compound are heated in the presence or absence of a catalyst and in the presence or absence of a solvent, thereby prepolymerizing. The mixing or prepolymerization of the components can be carried out in the absence of a solvent, for example, using an extruder, a kneader, a roller, etc., and in the presence of a solvent, using a reaction kettle with a stirring device, etc.
[0110] The resin composition of the present invention is heated and melted to reduce viscosity, and then impregnated with reinforcing fibers such as glass fiber, carbon fiber, polyester fiber, polyamide fiber, and alumina fiber to obtain a prepreg. In addition, the varnish is impregnated with reinforcing fibers and heated and dried to obtain a prepreg.
[0111] By cutting the above-mentioned prepreg into the desired shape and optionally stacking it with copper foil, etc., applying pressure to the stack by press molding, autoclave molding, sheet winding molding, etc., while heating and curing the resin composition, a substrate of the present invention such as a laminated board (printed circuit board) for electrical and electronic use or a carbon fiber reinforced material can be obtained.
[0112] Alternatively, the substrate of the present invention may be obtained by applying a solvent to a copper foil and drying it, laminating a polyimide film or LCP (liquid crystal polymer), and then heat-pressing and curing it. Optionally, the substrate of the present invention may be obtained by applying it to a polyimide film or LCP side and laminating it with a copper foil.
[0113] (Example)
[0114] The present invention is further described in detail below by way of examples and comparative examples. In addition, the present invention is not limited to these examples. In addition, "parts" in the examples are parts by mass, and "%" is % by mass.
[0115] Example 1 (Synthesis of isocyanate-modified polyimide resin of the present invention)
[0116] In a 300 ml reactor equipped with a thermometer, a reflux cooler, a Dean Stark apparatus, a raw material inlet, a nitrogen inlet, and a stirring device, 5.28 parts of BAFL (9,9-bis(4-aminophenyl)fluorene, manufactured by JFE Chemical Co., Ltd., molecular weight 348.45 g / mol), 13.28 parts of PRIAMINE1075 (C36 dimer diamine, manufactured by CRODA JAPAN Co., Ltd., molecular weight 534.38 g / mol), 14.89 parts of ODPA (oxydiphthalic anhydride, manufactured by Manac Co., Ltd., molecular weight 310.22 g / mol), 74.45 parts of anisole, 0.97 parts of triethylamine, and 19.80 parts of toluene were added, and the raw materials were dissolved by heating to 120° C. The reaction was carried out at 135° C. for 4 hours while removing water generated by the ring closure of the amic acid by azeotropic removal with toluene. After the generation of water stops, the remaining triethylamine and toluene are removed at 140° C. to obtain an intermediate polyimide resin solution. The molar ratio (number of moles of the acid anhydride component / number of moles of the diamine component) of the diamine component (component (b) and component (d)) and the acid anhydride component (component (c)) used in the synthesis of the intermediate polyimide resin is 1.20.
[0117] Then, 1.48 parts of TMDI (trimethylhexamethylene diisocyanate, manufactured by Degussa-Huels, molecular weight 210.28 g / mol) and 3.30 parts of anisole were added to the intermediate polyimide resin solution obtained above, and heated at 130° C. for 3 hours to obtain an isocyanate-modified polyimide resin solution (A-1) (non-volatile matter 30.1%). The molar ratio of the final raw material components of the isocyanate-modified polyimide resin obtained above (the number of moles of the acid anhydride component / (the number of moles of the diamine component+the number of moles of the diisocyanate component)) was 1.02.
[0118] Example 2 (Synthesis of isocyanate-modified polyimide resin of the present invention)
[0119] In a 300 ml reactor equipped with a thermometer, a reflux cooler, a Dean Stark apparatus, a raw material inlet, a nitrogen inlet, and a stirring device, 5.37 parts of BAFL (9,9-bis(4-aminophenyl)fluorene, manufactured by JFE Chemical Co., Ltd., molecular weight 348.45 g / mol), 13.14 parts of PRIAMINE1075 (C36 dimer diamine, manufactured by CRODA JAPAN Co., Ltd., molecular weight 534.38 g / mol), 14.89 parts of ODPA (oxydiphthalic anhydride, manufactured by Manac Co., Ltd., molecular weight 310.22 g / mol), 74.35 parts of anisole, 0.97 parts of triethylamine, and 19.79 parts of toluene were added, and the raw materials were dissolved by heating to 120° C. The reaction was carried out at 135° C. for 4 hours while removing water generated by the ring closure of the amic acid by azeotropic removal with toluene. After the generation of water stops, the remaining triethylamine and toluene are removed at 140° C. to obtain an intermediate polyimide resin solution. The molar ratio (number of moles of the acid anhydride component / number of moles of the diamine component) of the diamine component (component (b) and component (d)) and the acid anhydride component (component (c)) used in the synthesis of the intermediate polyimide resin is 1.20.
[0120] Then, 1.19 parts of HDI (hexamethylene diisocyanate, manufactured by Asahi Kasei Co., Ltd., molecular weight 168.20 g / mol) and 2.64 parts of anisole were added to the intermediate polyimide resin solution obtained above, and heated at 130° C. for 3 hours to obtain an isocyanate-modified polyimide resin solution (A-2) (non-volatile matter 30.0%). The molar ratio of the final raw material components of the isocyanate-modified polyimide resin obtained above (the number of moles of the acid anhydride component / (the number of moles of the diamine component+the number of moles of the diisocyanate component)) was 1.02.
[0121] Example 3 (Synthesis of isocyanate-modified polyimide resin of the present invention)
[0122] In a 300 ml reactor equipped with a thermometer, a reflux cooler, a Dean Stark apparatus, a raw material inlet, a nitrogen inlet, and a stirring device, 5.25 parts of BAFL (9,9-bis(4-aminophenyl)fluorene, manufactured by JFE Chemical Co., Ltd., molecular weight 348.45 g / mol), 13.32 parts of PRIAMINE1075 (C36 dimer diamine, manufactured by CRODA JAPAN Co., Ltd., molecular weight 534.38 g / mol), 14.89 parts of ODPA (oxydiphthalic anhydride, manufactured by Manac Co., Ltd., molecular weight 310.22 g / mol), 74.48 parts of anisole, 0.97 parts of triethylamine, and 19.80 parts of toluene were added, and the raw materials were dissolved by heating to 120° C. The reaction was carried out at 135° C. for 4 hours while removing water generated by the ring closure of the amic acid by azeotropic removal with toluene. After the generation of water stops, the remaining triethylamine and toluene are removed at 140° C. to obtain an intermediate polyimide resin solution. The molar ratio (number of moles of the acid anhydride component / number of moles of the diamine component) of the diamine component (component (b) and component (d)) and the acid anhydride component (component (c)) used in the synthesis of the intermediate polyimide resin is 1.20.
[0123] Then, 1.57 parts of IPDI (isophorone diisocyanate, manufactured by Degussa-Huels, molecular weight 222.29 g / mol) and 3.49 parts of anisole were added to the intermediate polyimide resin solution obtained above, and heated at 130° C. for 3 hours to obtain an isocyanate-modified polyimide resin solution (A-3) (non-volatile matter 30.0%). The molar ratio of the final raw material components of the isocyanate-modified polyimide resin obtained above (the number of moles of the acid anhydride component / (the number of moles of the diamine component+the number of moles of the diisocyanate component)) was 1.02.
[0124] Example 4 (Synthesis of isocyanate-modified polyimide resin of the present invention)
[0125] In a 300 ml reactor equipped with a thermometer, a reflux cooler, a Dean Stark apparatus, a raw material inlet, a nitrogen inlet and a stirring apparatus, 10.16 parts of BAPP (2,2-bis[4-(4-aminophenoxy)phenyl]propane, manufactured by Wakayama Seika Industries Co., Ltd., molecular weight 410.52 g / mol), 12.42 parts of PRIAMINE1075 (C36 dimer diamine, manufactured by CRODA JAPAN Co., Ltd., molecular weight 534.38 g / mol), 8.73 parts of PMDA (pyromellitic acid dianhydride, manufactured by Mitsubishi Gas Chemical Co., Ltd., molecular weight 218.12 g / mol), 69.69 parts of anisole, 0.81 parts of triethylamine and 19.16 parts of toluene were added, and the raw materials were dissolved by heating to 120° C. The reaction was carried out at 135° C. for 4 hours while removing water generated by the ring closure of the amic acid with toluene by azeotropic removal. After the generation of water stops, the remaining triethylamine and toluene are removed at 140° C. to obtain an intermediate polyimide resin solution. The molar ratio (number of moles of diamine component / number of moles of anhydride component) of the diamine component (component (b) and component (d)) and the acid anhydride component (component (c)) used in the synthesis of the intermediate polyimide resin is 1.20.
[0126] Then, 1.19 parts of HDI (hexamethylene diisocyanate, manufactured by Asahi Kasei Co., Ltd., molecular weight 168.20 g / mol) and 2.64 parts of anisole were added to the intermediate polyimide resin solution obtained above, and heated at 130° C. for 3 hours to obtain an isocyanate-modified polyimide resin solution (A-4) (non-volatile matter 30.1%). The molar ratio of the final raw material components of the isocyanate-modified polyimide resin obtained above (the number of moles of the diamine component / (the number of moles of the anhydride component+the number of moles of the diisocyanate component)) was 1.02.
[0127] Example 5 (Synthesis of terminal-modified isocyanate-modified polyimide resin of the present invention)
[0128] In a 300 ml reactor equipped with a thermometer, a reflux cooler, a Dean Stark apparatus, a raw material inlet, a nitrogen inlet, and a stirring apparatus, 9.13 parts of BAPP (2,2-bis[4-(4-aminophenoxy)phenyl]propane, manufactured by Wakayama Seika Industries Co., Ltd., molecular weight 410.52 g / mol), 13.76 parts of PRIAMINE1075 (C36 dimer diamine, manufactured by CRODA JAPAN Co., Ltd., molecular weight 534.38 g / mol), 11.77 parts of BPDA (biphenyltetracarboxylic dianhydride, manufactured by Mitsubishi Chemical Co., Ltd., molecular weight 294.22 g / mol), 77.15 parts of anisole, 0.81 parts of triethylamine, and 20.14 parts of toluene were added, and the raw materials were dissolved by heating to 120° C. The reaction was carried out at 135° C. for 4 hours while removing water generated by the ring closure of the amic acid by azeotropic distillation with toluene. After the generation of water stops, the remaining triethylamine and toluene are removed at 140° C. to obtain an intermediate polyimide resin solution. The molar ratio (number of moles of diamine component / number of moles of anhydride component) of the diamine component (component (b) and component (d)) and the acid anhydride component (component (c)) used in the synthesis of the intermediate polyimide resin is 1.20.
[0129] Then, 1.19 parts of HDI (hexamethylene diisocyanate, manufactured by Asahi Kasei Co., Ltd., molecular weight 168.20 g / mol) and 2.64 parts of anisole were added to the intermediate polyimide resin solution obtained above, and heated at 130°C for 3 hours to obtain an isocyanate-modified polyimide resin solution (A-5). The molar ratio of the final raw material components of the isocyanate-modified polyimide resin obtained above (the number of moles of diamine component / (the number of moles of anhydride component+the number of moles of diisocyanate component)) was 1.02. Then, 0.08 parts of maleic anhydride (molecular weight 98.06 g / mol), 0.3 parts of triethylamine and 5.2 parts of toluene were further added to the isocyanate-modified polyimide resin solution (A-5), and reacted at 135°C for 4 hours. After the generation of water stopped, the remaining triethylamine and toluene were removed at 140° C., thereby obtaining a terminal-modified isocyanate-modified polyimide resin solution (B-5) (non-volatile matter 30.2%) in which both ends of the isocyanate-modified polyimide resin were modified with maleic anhydride.
[0130] Example 6 (Synthesis of isocyanate-modified polyimide resin of the present invention)
[0131] In a 300 ml reactor equipped with a thermometer, a reflux cooler, a Dean Stark apparatus, a raw material inlet, a nitrogen inlet and a stirring device, BAFL (9,9-bis (4-aminophenyl) fluorene, manufactured by JFE Chemical Co., Ltd., molecular weight 348.45 g / mol) 1.22 parts, diamine18 (C18 diamine, manufactured by Okamura Oil Manufacturing Co., Ltd., molecular weight 284.53 g / mol) 10.38 parts, ODPA (oxydiphthalic anhydride, manufactured by Manac Co., Ltd., molecular weight 310.22 g / mol) 14.89 parts, anisole 58.98 parts, triethylamine 0.97 parts and toluene 17.78 parts were added, and heated to 120 ° C to dissolve the raw materials. While removing the water generated by the ring closure of the amic acid and toluene azeotropically, the reaction was carried out at 135 ° C for 4 hours. After the generation of water stopped, the remaining triethylamine and toluene were removed at 140 ° C, thereby obtaining an intermediate polyimide resin solution. The molar ratio (number of moles of the acid anhydride component / number of moles of the diamine component) of the diamine component (component (b) and component (d)) and the acid anhydride component (component (c)) used in the synthesis of the intermediate polyimide resin was 1.20.
[0132] Then, 1.19 parts of HDI (hexamethylene diisocyanate, manufactured by Asahi Kasei Co., Ltd., molecular weight 168.20 g / mol) and 2.64 parts of anisole were added to the intermediate polyimide resin solution obtained above, and heated at 130° C. for 3 hours to obtain an isocyanate-modified polyimide resin solution (A-6) (non-volatile matter 30.0%). The molar ratio of the final raw material components of the isocyanate-modified polyimide resin obtained above (molar number of anhydride component / (molar number of diamine component+molar number of diisocyanate component)) was 1.02.
[0133] Comparative Example 1 (Synthesis of Comparative Polyimide Resin)
[0134] In a 300 ml reactor equipped with a thermometer, a reflux cooler, a Dean Stark apparatus, a raw material inlet, a nitrogen inlet, and a stirring device, 7.53 parts of BAPP (2,2-bis[4-(4-aminophenoxy)phenyl]propane, manufactured by Wakayama Seika Industries Co., Ltd., molecular weight 410.52 g / mol), 12.43 parts of PRIAMINE1075 (C36 dimer diamine, manufactured by CRODA JAPAN Co., Ltd., molecular weight 534.38 g / mol), 12.41 parts of ODPA (oxydiphthalic anhydride, manufactured by Manac Co., Ltd., molecular weight 310.22 g / mol), 72.37 parts of anisole, 0.81 parts of triethylamine, and 19.51 parts of toluene were added, and the raw materials were dissolved by heating to 120° C. The reaction was carried out at 135° C. for 4 hours while removing water generated by the ring closure of the amic acid with toluene by azeotropic distillation. After the generation of water stopped, the remaining triethylamine and toluene were removed at 140°C to obtain a comparative polyimide resin solution (R-1) (non-volatile matter 30.0%). The molar ratio of the final raw material components of the comparative polyimide resin obtained above (the number of moles of the anhydride component / the number of moles of the diamine component) was 1.05.
[0135] Comparative Example 2 (Synthesis of Comparative Polyimide Resin)
[0136] In a 300 ml reactor equipped with a thermometer, a reflux cooler, a Dean Stark apparatus, a raw material inlet, a nitrogen inlet, and a stirring device, 6.45 parts of BAFL (9,9-bis(4-aminophenyl)fluorene, manufactured by JFE Chemical Co., Ltd., molecular weight 348.45 g / mol), 11.71 parts of PRIAMINE1075 (C36 dimer diamine, manufactured by CRODA JAPAN Co., Ltd., molecular weight 534.38 g / mol), 12.41 parts of ODPA (oxydiphthalic anhydride, manufactured by Manac Co., Ltd., molecular weight 310.22 g / mol), 68.34 parts of anisole, 0.81 parts of triethylamine, and 18.99 parts of toluene were added, and the raw materials were dissolved by heating to 120° C. The reaction was carried out at 135° C. for 4 hours while removing water generated by the ring closure of the amic acid by azeotropic distillation with toluene. After the generation of water stopped, the remaining triethylamine and toluene were removed at 140°C to obtain a comparative polyimide resin solution (R-2) (non-volatile matter 30.2%). The molar ratio of the final raw material components of the comparative polyimide resin obtained above (the number of moles of the anhydride component / the number of moles of the diamine component) was 1.02.
[0137] Examples 7 to 12, Comparative Examples 3 and 4 (Adjustment of Resin Composition)
[0138] The polyimide resin solutions (A-1) to (A-4), (B-5) and (A-6) obtained in Examples 1 to 6, the comparative polyimide resin solutions (R-1) and (R-2) obtained in Comparative Examples 1 and 2, MIR3000-70MT (maleimide resin containing a biphenyl skeleton, non-volatile matter 70.0%) manufactured by Nippon Kayaku as a compound having a maleimide group, diisopropylbenzene peroxide (DCP) as a free radical initiator, NC-3000 (epoxy resin containing a biphenyl skeleton, epoxy group equivalent 277 g / eq, softening point 60°C) manufactured by Nippon Kayaku as an epoxy resin, and C11Z-A manufactured by Shikoku Chemical Industries, Ltd. as a hardening accelerator were mixed in the blending amounts shown in Table 1 (the unit is "parts", the parts of the polyimide resin and the compound having a maleimide group are the parts of the solution including the solvent) to obtain the resin composition of the present invention and the comparative resin composition.
[0139] Table 1 Composition of resin composition
[0140] Example 7 Example 8 Example 9 Example 10 Embodiment 11 Example 12 Comparative Example 3 Comparative Example 4 A-1 50 A-2 50 A-3 50 A-4 50 B-5 50 A-6 50 R-1 50 R-2 50 MIR3000-70MT 9.18 9.18 9.18 9.18 9.18 9.18 9.18 9.18 DCP 0.21 0.21 0.21 0.21 0.21 0.21 0.21 0.21 NC-3000 0.2 0.2 0.2 0.2 C11Z-A 0.002 0.002 0.002 0.002
[0141] (Evaluation of Adhesion Strength)
[0142] The resin compositions obtained in Examples 7 to 12 and Comparative Examples 3 and 4 were used to evaluate the adhesive strength and thermal properties of the cured products of the resin compositions to copper foil.
[0143] The rough surface of copper foil CF-T4X-SV-18 (hereinafter referred to as "T4X") manufactured by Futian Metal Foil Powder Industry Co., Ltd. was coated with the above-obtained resin composition using an automatic dispenser, and heated and dried at 120°C for 10 minutes. The coating thickness after drying is 30μm. The coating on the above-obtained copper foil overlaps the rough surface of T4X, and vacuum pressing is performed under the conditions of 200°C, 60 minutes, and 3MPa. The obtained test piece was cut into a width of 10mm, and the 90° peel strength between the copper foils was measured using Autograph AGS-X-500N (manufactured by Shimadzu Corporation) (peeling speed is 50mm / min) to evaluate the bonding strength of the copper foil. In addition, it was visually confirmed that all samples had cohesion failure after the test. The results are shown in Tables 2 and 3.
[0144] (Evaluation of thermal characteristics)
[0145] The test piece prepared in the same manner as in the above "Evaluation of Adhesion Strength" was flowed in a solder bath heated to 288°C using POT-200C (manufactured by Taiyo Electric Industry Co., Ltd.), and the thermal characteristics were evaluated based on the time until expansion occurred. The results are shown in Tables 2 and 3.
[0146] (Evaluation of mechanical and dielectric properties)
[0147] In addition to changing the coating thickness of the automatic dispenser, a coating film with a thickness of 100 μm after drying was formed on the rough surface of T4X in the same manner as in the above-mentioned "Evaluation of Adhesion Strength", and heated and cured at 200°C for 60 minutes. The copper foil was etched and removed with an iron (III) chloride solution with a liquid specific gravity of 45 degrees Baume, washed with ion exchange water, and dried at 105°C for 10 minutes to obtain a film-like cured product. The film-like cured product was measured for the rupture point stress, rupture point elongation, and elastic modulus using Autograph AGS-X-500N (manufactured by Shimadzu Corporation), and the dielectric properties at 10 GHz were measured using a network analyzer 8719ET (manufactured by Agilent Technologies) by the cavity resonance method. The results are shown in Tables 2 and 3.
[0148] Table 2 Evaluation results of resin compositions
[0149]
[0150] Table 3 Evaluation results of resin compositions
[0151]
[0152] From the results in Tables 2 and 3, it can be seen that the resin composition of the present invention has excellent bonding strength, mechanical properties, thermal properties and dielectric constant. In contrast, the resin composition of the comparative example has poor mechanical properties, high loss tangent, and poor bonding strength or thermal properties.
[0153] Example 13 (Synthesis of isocyanate-modified polyimide resin of the present invention)
[0154] In a 300 ml reactor equipped with a thermometer, a reflux cooler, a Dean Stark apparatus, a raw material inlet, a nitrogen inlet, and a stirring device, BAFL (9,9-bis (4-aminophenyl) fluorene, manufactured by JFE Chemical Co., Ltd., molecular weight 348.45 g / mol) 7.70 parts, PRIAMINE1075 (C36 dimer diamine, manufactured by CRODA JAPAN Co., Ltd., molecular weight 534.38 g / mol) 10.64 parts, ODPA (oxydiphthalic anhydride, manufactured by Manac Co., Ltd., molecular weight 310.22 g / mol) 12.41 parts, anisole 68.43 parts, triethylamine 0.81 parts, and toluene 19.00 parts were added, and the raw materials were dissolved by heating to 120 ° C. The reaction was carried out at 135 ° C for 4 hours while removing water generated by the ring closure of the amic acid and toluene azeotropically. After the generation of water stops, the remaining triethylamine and toluene are removed at 140° C. to obtain an intermediate polyimide resin solution. The molar ratio (number of moles of diamine component / number of moles of anhydride component) of the diamine component (component (b) and component (d)) and the acid anhydride component (component (c)) used in the synthesis of the intermediate polyimide resin is 1.05.
[0155] Then, 0.26 parts of IPDI (isophorone diisocyanate, manufactured by Degussa-Huels, molecular weight 222.29 g / mol) and 0.58 parts of anisole were added to the intermediate polyimide resin solution obtained above, and heated at 130° C. for 3 hours to obtain an isocyanate-modified polyimide resin solution (A-7) (non-volatile matter 30.1%). The molar ratio of the final raw material components of the isocyanate-modified polyimide resin obtained above (the number of moles of the diamine component / (the number of moles of the anhydride component+the number of moles of the diisocyanate component)) was 1.02.
[0156] Examples 14 to 19 (Adjustment of resin composition)
[0157] The polyimide resin solutions (A-1), (A-3) and (A-7) obtained in Examples 1, 3 and 13, the maleimide group-containing compounds MIR3000-70MT (maleimide resin containing a biphenyl skeleton, non-volatile matter 70.0%) and MIR5000-60T (phenolic varnish type maleimide resin, non-volatile matter 60.0%) manufactured by Nippon Kayaku, and diisopropylbenzene peroxide (DCP) as a free radical initiator are mixed in the amounts shown in Table 4 (the units are "parts", the parts of the polyimide resin and the maleimide resin are the parts of the solution including the solvent) to obtain the resin composition of the present invention.
[0158] Table 4 Composition of resin composition
[0159] Embodiment 14 Embodiment 15 Example 16 Embodiment 17 Embodiment 18 Embodiment 19 A-1 57.1 50 A-3 57.1 57.1 A-7 57.1 50 MIR3000-70MT 6.12 9.18 6.12 6.12 9.18 MIR5000-60T 6.12 DCP 0.21 0.21 0.21 0.21 0.21 0.21
[0160] (Evaluation of adhesion strength, thermal properties, mechanical properties and dielectric properties)
[0161] The resin compositions obtained in Examples 14 to 19 were used to prepare evaluation samples in the same manner as above, and the bonding strength, thermal properties, mechanical properties, and dielectric properties were evaluated in the same manner as above.
[0162] Table 5 Evaluation results of resin compositions
[0163]
[0164] From the results in Table 5, it can be seen that the resin composition of the present invention has excellent bonding strength, mechanical properties, thermal properties and dielectric constant.
[0165] (Industrial availability)
[0166] The resin composition containing the isocyanate-modified polyimide resin or terminal-modified isocyanate-modified polyimide resin of the present invention having a specific structure can provide a printed wiring board having excellent properties such as heat resistance, mechanical properties, low dielectric properties and adhesion.
Claims
1. An isocyanate-modified polyimide resin, which is a reaction product of a polyimide resin and a diisocyanate compound (a) having an isocyanate group, and has anhydride groups at both ends, The polyimide resin is a reaction product of an aliphatic diamine compound (b), a tetrabasic acid dianhydride (c), and an aromatic diamine compound (d), and has an acid anhydride group at both ends. The aromatic diamine compound (d) includes a compound represented by the following formula (8): In formula (8), Z represents a divalent linking group represented by the following formula (9), R3 represents a hydrogen atom, a methyl group, an ethyl group, a hydroxyl group or a trifluoromethyl group, The mass of the aliphatic diamine compound (b) is 10 to 50% by mass of the total mass of the components (b) to (d) used in the synthesis step of the polyimide resin and the component (a) used in the synthesis step of the isocyanate-modified polyimide resin, excluding the mass of water generated in the dehydration cyclization reaction step during the synthesis of the polyimide resin. The isocyanate group of the component (a) is in an amount of 0.50 to 0.99 equivalents per 1 equivalent of the terminal functional group of the polyimide resin.
2. The isocyanate-modified polyimide resin according to claim 1, wherein the diisocyanate compound (a) contains at least one selected from the group consisting of hexamethylene diisocyanate, trimethylhexamethylene diisocyanate, and isophorone diisocyanate. 3 . The isocyanate-modified polyimide resin according to claim 1 , wherein the aliphatic diamine compound (b) comprises at least one aliphatic diamine compound having 6 to 36 carbon atoms.
4. The isocyanate-modified polyimide resin according to any one of claims 1 to 3, wherein the tetrabasic acid dianhydride (c) contains at least one selected from the group consisting of the following formulas (1) to (4): In formula (4), Y represents C(CF3)2, SO2, CO, O, a direct bond, or a divalent linking group represented by the following formula (5):
5. A terminal-modified isocyanate-modified polyimide resin, which is a reaction product of the isocyanate-modified polyimide resin having acid anhydride groups at both ends according to any one of claims 1 to 4 and a compound having one functional group that can react with the acid anhydride groups. 6 . A resin composition comprising the isocyanate-modified polyimide resin according to claim 1 , and a compound reactive with the isocyanate-modified polyimide resin.
7. A resin composition comprising the terminal-modified isocyanate-modified polyimide resin according to claim 5 and a compound that reacts with the terminal-modified isocyanate-modified polyimide resin.
8. The resin composition according to claim 7, wherein the terminal-modified isocyanate-modified polyimide resin has amine groups at both ends, and the compound reacting with the terminal-modified isocyanate-modified polyimide resin contains at least one compound having a maleimide group. 9 . A resin composition comprising the isocyanate-modified polyimide resin according to claim 1 , and a compound that does not react with the isocyanate-modified polyimide resin.
10. A resin composition comprising the terminal-modified isocyanate-modified polyimide resin according to claim 5 and a compound that does not react with the terminal-modified isocyanate-modified polyimide resin. 11 . A cured product, which is a cured product of the resin composition according to claim 6 .
12. A substrate comprising the cured product according to claim 11.
Citation Information
Patent Citations
Process for preparing butyl-p-benzoylbenzoates
EP0000502A1
Polyamide resin originated from dimer diamine and optical material made of synthetic resin containing the polyamide
JP1997012712A
Polyimide resin
CN101501093A
Novel polyimide precursor composition and use thereof
CN101657482A
Novel polyimide precursor composition, use of the same, and production method of the same
CN102037043A