Aggregation-induced gold-silver alloy nanoclusters and preparation methods and applications thereof
The aggregation-induced yellow-green fluorescent gold-silver alloy nanoclusters are prepared by an ultrasound-assisted method, which solves the problem of adding additional organic solvents and reducing agents in the existing technology, achieves high quantum yield and high sensitivity, and is suitable for quercelain. Detection of hormones.
Patent Information
- Application Number
- CN202211303504.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-10-24
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2042-10-24
AI Technical Summary
The existing preparation method of gold-silver bimetallic nanoclusters requires the addition of additional organic solvents and reducing agents, and high quantum yields are difficult to obtain, which limits its application in quercetin detection.
Using L-cysteine as a protective agent and reducing agent, it was mixed evenly with silver nitrate and chloroauric acid through ultrasound-assisted method to prepare an aggregation-induced yellow-green fluorescent gold-silver alloy nanocluster aqueous solution without the need for additional Simple and fast synthesis with the addition of organic solvents or reducing agents.
The obtained gold-silver alloy nanoclusters have high quantum yield, strong resistance to photobleaching, good water solubility, fluorescence emission around 560nm, showing yellow-green fluorescence, high sensitivity and selectivity, and are suitable for the production of quercetin. Detection, the detection limit is 0.179 μM.
Smart Images

Figure CN115780818B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the preparation of gold-silver bimetallic nanoclusters, and in particular to an aggregation-induced yellow-green fluorescent gold-silver alloy nanocluster, a preparation method and application thereof. Background Art
[0002] Flavonoids are a class of natural products widely found in vegetables, fruits, and herbs. Due to the differences in the number of phenolic rings, hydroxyl types, and the presence of double bonds, flavonoids can be divided into three categories: flavonols, flavonoids, and isoflavones. As a type of flavonol, quercetin has antioxidant properties in the 3, 3', 4', 5, and 7 positions of hydroxyl groups and catechol rings, which enable it to scavenge free radicals and affect the redox state in cells. Quercetin can kill senescent cells and significantly prolong the life of animals; it can also be used to treat allergies, coughs, hypertension, coronary heart disease, diabetes, chronic bronchitis, cancer, and other diseases. Therefore, highly sensitive detection of quercetin is of great significance for pharmacological research and the evaluation of nutritional quality in food chemistry. The methods that have been reported to detect quercetin include: liquid chromatography, spectrophotometry, mass spectrometry, Raman spectroscopy, molecular imprinting, electrochemical method, etc. However, the application of these methods is limited by the large amount of time consumed, high instrument costs, complex operating techniques, and the use of toxic solvents. Therefore, there is still huge room for developing low-cost, simple-operation, and highly selective detection methods.
[0003] In recent years, fluorescence analysis has been widely studied in the field of analytical detection as an alternative method for detecting various organic and inorganic analytes. This fluorescence-based analytical detection method mainly relies on the luminescence behavior of organic fluorescent dyes, quantum dots, and metal nanoclusters. Driven by the rapid development of single-component metal nanoclusters, bimetallic nanoclusters integrate the chemical and physical properties of two metals into one nanocluster through a synergistic effect, thereby showing higher stability, enhanced fluorescence, better catalytic activity, and high sensitivity in sensing applications. Ungor et al. used aggregation-induced fluorescence to synthesize gold-silver bimetallic nanoclusters by using AMP as a protective agent, reacting at 80 ° C for 12 h, and finally purifying with acetone with a quantum yield of 7.3% (Journal of Molecular Liquids, 2021, 338, 116695). The interaction between the bimetallic nanoclusters and the capping agent restricts the intramolecular vibration and rotation of the capping ligand, reduces the radiative relaxation of the corresponding excited state, and enhances the aggregation-induced emission (AIE) of the gold-silver bimetallic nanoclusters, thereby enhancing the emission of the gold-silver bimetallic nanoclusters, and the emission peak tends to be blue-shifted.
[0004] In the existing preparation method of gold-silver bimetallic nanoclusters, additional organic solvents and reducing agents need to be added, and high quantum yields are difficult to obtain. Summary of the invention
[0005] The technical problem to be solved by the present invention is to provide an aggregation-induced gold-silver alloy nanocluster and a preparation method and application thereof. The obtained product is applied to the detection of quercetin and has high sensitivity and selectivity.
[0006] To solve the above technical problems, according to one aspect of the present invention, a method for preparing aggregation-induced gold-silver alloy nanoclusters is provided, which comprises mixing L-cysteine solution, silver nitrate solution and chloroauric acid solution evenly, and then using ultrasound to assist in preparing an aggregation-induced yellow-green fluorescent gold-silver alloy nanocluster aqueous solution, wherein L-cysteine is a protective agent and a reducing agent, and silver nitrate and chloroauric acid are used as matrices.
[0007] Furthermore, 10-30 mmol / L of L-cysteine solution, 10 mmol / L of chloroauric acid solution and 5-30 mmol / L of silver nitrate solution were evenly mixed, and the ultrasonic power was controlled to be 100-300 W. After complete reaction, an aggregation-induced yellow-green fluorescent gold-silver alloy nanocluster aqueous solution was obtained.
[0008] Furthermore, after the L-cysteine solution was evenly mixed with the chloroauric acid solution and the silver nitrate solution, ultrasonic power was controlled at 150 W for 10 min.
[0009] Furthermore, the volume ratio of the L-cysteine solution, the chloroauric acid solution and the silver nitrate solution is 3:2:2.
[0010] Furthermore, the concentration of the L-cysteine solution is 20 mmol / L.
[0011] Furthermore, the concentration of the silver nitrate solution is 10 mmol / L.
[0012] According to another aspect of the present invention, provided is an aggregation-induced gold-silver alloy nanocluster obtained according to the above method.
[0013] According to another aspect of the present invention, provided is the use of the above-mentioned aggregation-induced gold-silver alloy nanoclusters in quercetin detection.
[0014] According to another aspect of the present invention, a method for detecting quercetin is provided, wherein the aqueous solution of the aggregation-induced gold-silver alloy nanoclusters and the Tris-HCl buffer solution described above are added to a fluorescence cuvette, and then quercetin solutions of different concentrations are added, and the fluorescence spectrum is measured at 340 nm as the excitation wavelength to obtain a linear relationship between the fluorescence intensity and the quercetin concentration; based on the linear relationship, the quercetin content in the sample to be tested is quantitatively detected.
[0015] Furthermore, 100 μL of an aqueous solution of aggregation-induced gold-silver alloy nanoclusters and 1 mL of a 50 mM, pH 7 Tris-HCl buffer solution were added to a fluorescence cuvette.
[0016] Compared with the prior art, the technical effects of the present invention include:
[0017] (1) The present invention uses L-cysteine as a protective agent and a reducing agent to prepare an aggregation-induced yellow-green fluorescent gold-silver alloy nanocluster solution by an ultrasound-assisted method. The synthesis method is simple and rapid, and no additional organic solvent or reducing agent (such as corrosive sodium hydroxide) is required during the synthesis process, which is in line with the theme of green chemistry.
[0018] (2) The synthesized gold-silver alloy nanoclusters have the characteristics of aggregation-induced emission, large Stocks shift, strong resistance to photobleaching, and good water solubility. Compared with single metal gold nanoclusters, the fluorescence intensity is significantly enhanced, and the quantum yield is also improved.
[0019] (3) The synthesized aggregation-induced gold-silver alloy nanoclusters have good optical properties. Their fluorescence emission is around 560nm. When observed under ultraviolet light against a black background, they exhibit yellow-green fluorescence and have good resistance to photobleaching.
[0020] (4) The aggregation-induced yellow-green fluorescent gold-silver alloy nanoclusters prepared by the present invention show high sensitivity and selectivity to quercetin and can be applied to the detection of quercetin with a detection limit of 0.179 μM. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Figure 1 The ultraviolet absorption spectrum and the fluorescence excitation and emission spectra of the aggregation-induced yellow-green fluorescent gold-silver alloy nanoclusters described in Example 7;
[0022] Figure 2 is a photostability graph of the aggregation-induced yellow-green fluorescent gold-silver alloy nanoclusters described in Example 7;
[0023] Figure 3 is an infrared spectrum of the aggregation-induced yellow-green fluorescent gold-silver alloy nanoclusters and L-cysteine described in Example 7;
[0024] Figure 4 is a fluorescence spectrum of the aggregation-induced yellow-green fluorescent gold-silver alloy nanoclusters and gold nanoclusters described in Example 7;
[0025] Figure 5 is the working curve of the aggregation-induced yellow-green fluorescent gold-silver alloy nanoclusters responding to quercetin described in Example 7;
[0026] Figure 6The linear relationship between the logarithmic change of the fluorescence intensity of the aggregation-induced yellow-green fluorescent gold-silver alloy nanoclusters described in Example 7 and the quercetin concentration;
[0027] Figure 7 This is a fluorescence bar graph of the aggregation-induced yellow-green fluorescent gold-silver alloy nanoclusters described in Example 7 after interacting with various interferents. DETAILED DESCRIPTION
[0028] The technical scheme claimed in the present invention is further described below by some examples. However, the examples and comparative examples are used to explain the embodiments of the present invention and do not exceed the scope of the subject matter of the present invention. The protection scope of the present invention is not limited by the examples. Unless otherwise specified, the materials and reagents used in the present invention can be obtained from commercial products in the art.
[0029] Example 1
[0030] A method for preparing aggregation-induced yellow-green fluorescent gold-silver alloy nanoclusters comprises the following steps: 3 mL of 10 mmol / L L-cysteine solution, 2 mL of 10 mmol / L chloroauric acid solution and 2 mL of 30 mmol / L silver nitrate solution are mixed and shaken evenly, and ultrasonic power is controlled to be 150 W for 10 min to obtain an aggregation-induced luminescent gold-silver alloy nanocluster aqueous solution. The fluorescence emission peak of the luminescent gold-silver alloy nanocluster is about 560 nm, and when observed under ultraviolet light with a black background, it exhibits very weak yellow-green fluorescence, and the quantum yield is 5.60%.
[0031] Example 2
[0032] A method for preparing aggregation-induced yellow-green fluorescent gold-silver alloy nanoclusters comprises the following steps: 3 mL of 20 mmol / L L-cysteine solution, 2 mL of 10 mmol / L chloroauric acid solution and 2 mL of 20 mmol / L silver nitrate solution are mixed and shaken evenly, and ultrasonic power is controlled to be 250 W for 10 min to obtain an aggregation-induced luminescent gold-silver alloy nanocluster aqueous solution. The fluorescence emission peak of the luminescent gold-silver alloy nanocluster is about 560 nm, and when observed under ultraviolet light with a black background, it exhibits weak yellow-green fluorescence, and the quantum yield is 7.50%.
[0033] Example 3
[0034] A method for preparing aggregation-induced yellow-green fluorescent gold-silver alloy nanoclusters comprises the following steps: 3 mL of 20 mmol / L L-cysteine solution, 2 mL of 10 mmol / L chloroauric acid solution and 2 mL of 5.0 mmol / L silver nitrate solution are mixed and shaken evenly, and ultrasonic power is controlled to be 100 W for 10 min to obtain an aggregation-induced luminescent gold-silver alloy nanocluster aqueous solution. The fluorescence emission peak of the luminescent gold-silver alloy nanocluster is about 570 nm, and when observed under ultraviolet light with a black background, it exhibits yellow-green fluorescence, and the quantum yield is 10.0%.
[0035] Example 4
[0036] A method for preparing aggregation-induced yellow-green fluorescent gold-silver alloy nanoclusters comprises the following steps: 3 mL of 20 mmol / L L-cysteine solution, 2 mL of 10 mmol / L chloroauric acid solution and 2 mL of 5.0 mmol / L silver nitrate solution are mixed and shaken evenly, and ultrasonic power is controlled to be 150 W for 10 min to obtain an aggregation-induced luminescent gold-silver alloy nanocluster aqueous solution. The fluorescence emission peak of the luminescent gold-silver alloy nanocluster is about 590 nm, and when observed under ultraviolet light with a black background, it exhibits yellow-green fluorescence, and the quantum yield is 12.5%.
[0037] Example 5
[0038] A method for preparing aggregation-induced yellow-green fluorescent gold-silver alloy nanoclusters comprises the following steps: 3 mL of 15 mmol / L L-cysteine solution, 2 mL of 10 mmol / L chloroauric acid solution and 2 mL of 10 mmol / L silver nitrate solution are mixed and shaken evenly, and ultrasonic power is controlled to be 150 W for 10 min to obtain an aggregation-induced luminescent gold-silver alloy nanocluster aqueous solution. The fluorescence emission peak of the luminescent gold-silver alloy nanocluster is about 570 nm, and when observed under ultraviolet light with a black background, it exhibits yellow-green fluorescence, and the quantum yield is 19.0%.
[0039] Example 6
[0040] A method for preparing aggregation-induced yellow-green fluorescent gold-silver alloy nanoclusters comprises the following steps: 3 mL of 30 mmol / L L-cysteine solution, 2 mL of 10 mmol / L chloroauric acid solution and 2 mL of 10 mmol / L silver nitrate solution are mixed and shaken evenly, and ultrasonic power is controlled to be 300 W for 10 min to obtain an aggregation-induced luminescent gold-silver alloy nanocluster aqueous solution. The fluorescence emission peak of the luminescent gold-silver alloy nanocluster is about 560 nm, and when observed under ultraviolet light with a black background, it exhibits yellow-green fluorescence, and the quantum yield is 24.0%.
[0041] Example 7
[0042] A method for preparing aggregation-induced yellow-green fluorescent gold-silver alloy nanoclusters comprises the following steps: 3 mL of 20 mmol / L L-cysteine solution, 2 mL of 10 mmol / L chloroauric acid solution and 2 mL of 10 mmol / L silver nitrate solution are mixed and shaken evenly, and ultrasonic power is controlled to be 150 W for 10 min to obtain an aggregation-induced luminescent gold-silver alloy nanocluster aqueous solution. The fluorescence emission peak of the luminescent gold-silver alloy nanocluster is about 560 nm, and when observed under ultraviolet light with a black background, it exhibits yellow-green fluorescence, and the quantum yield is 30.0%.
[0043] 100 mL of aggregation-induced yellow-green fluorescent gold-silver alloy nanocluster aqueous solution and 1 mL of Tris-HCl buffer (pH=7, 50 mmol / L) were added to a fluorescence cuvette, and its ultraviolet absorption spectrum and fluorescence excitation and emission spectra were measured. Figure 1 As shown, the maximum fluorescence excitation peak of the aggregation-induced yellow-green fluorescent gold-silver alloy nanoclusters is at 340 nm, and the emission peak is around 560 nm. The larger Stokes shift (220 nm) can avoid the overlap of the excitation and emission peaks.
[0044] The prepared aggregation-induced yellow-green fluorescent gold-silver alloy nanoclusters were subjected to anti-photobleaching experiments. Figure 2 As shown in the figure, the luminescence performance can still be maintained after continuous UV irradiation for 30 min, and the fluorescence intensity remains basically unchanged, indicating that it has good resistance to photobleaching.
[0045] The vibrational energy level and rotational energy level changes of the molecules in the prepared aggregation-induced yellow-green fluorescent gold-silver alloy nanoclusters were investigated. The aggregation-induced yellow-green fluorescent gold-silver alloy nanocluster solution prepared in Example 7 was freeze-dried, and the aggregation-induced yellow-green fluorescent gold-silver alloy nanocluster powder was obtained after removing the solvent water. A small amount of aggregation-induced yellow-green fluorescent gold-silver alloy nanocluster solid powder and L-cysteine powder were weighed and mixed with a certain amount of potassium bromide powder, respectively, and the tablets were pressed and placed in an infrared spectrometer for 4000-400 cm -1 The absorption spectrum is scanned within the wave number range. Figure 3 As shown in the figure, comparing the FTIR spectra of the two, the OH stretching vibration band overlaps with the NH stretching vibration band of the primary amine, appearing at ~3445 cm -1 The absorption peak at 2990 cm-1 indicates the presence of saturated CH, and the main related peak υCH of —CH2— appears at 2920 cm -1, υC=O of L-cysteine and Au / Ag alloy nanoclusters appear at 1595 cm -1 and 1388cm -1 The shift of the absorption peak may be related to the interaction between the Au-Ag alloy nanoclusters and L-cysteine. The SH stretching vibration band of L-cysteine (2549 cm -1 ) disappears in the infrared spectrum of the gold-silver alloy nanoclusters, indicating that the L-cysteine molecules protect the gold-silver alloy nanoclusters in the form of thiolate.
[0046] Comparative Example 1
[0047] A method for preparing silver nanoclusters protected by L-cysteine comprises the following steps: mixing 3 mL of a 20 mmol / L L-cysteine aqueous solution and 2 mL of a 10 mmol / L silver nitrate aqueous solution, and controlling the ultrasonic power to be 150 W for 10 min to obtain a silver nanocluster aqueous solution. The silver nanocluster does not show fluorescence when observed under ultraviolet light with a black background.
[0048] This comparative example is a comparative example of Example 7. In order to further illustrate the advantages of the method of the present invention, silver nanoclusters were synthesized using L-cysteine and silver nitrate aqueous solution as raw materials. By comparison, it can be seen that the silver nanoclusters prepared in this comparative example do not emit fluorescence.
[0049] Comparative Example 2
[0050] A method for preparing L-cysteine-protected gold nanoclusters comprises the following steps: 3 mL of a 20 mmol / L L-cysteine aqueous solution and 2 mL of a 10 mmol / L chloroauric acid aqueous solution are mixed and shaken evenly, and the ultrasonic power is controlled to be 150 W for 10 min to obtain a gold nanocluster aqueous solution. The gold nanocluster exhibits red fluorescence when observed under ultraviolet light with a black background, and the fluorescence intensity is relatively weak, and its quantum yield is measured to be 8.0%.
[0051] This comparative example is a comparative example of Example 5. In order to further illustrate the advantages of the method of the present invention, gold nanoclusters were synthesized using L-cysteine and chloroauric acid aqueous solution as raw materials. By comparison, it can be obtained that Figure 4 As shown, the gold-silver alloy nanoclusters prepared by the present invention greatly improve the fluorescence intensity and blue-shift the emission peak through aggregation-induced synergy, and the fluorescence quantum yield is increased by nearly 4 times.
[0052] Example 8
[0053] Application of aggregation-induced yellow-green fluorescent gold-silver alloy nanoclusters in quercetin detection
[0054] The aggregation-induced yellow-green fluorescent gold-silver alloy nanocluster solution prepared in Example 7 and 1 mL of Tris-HCl buffer (pH=7, 50 mmol / L) were added to a fluorescence cuvette, and quercetin solutions of different concentrations were added. The fluorescence spectra were measured at 340 nm as the excitation wavelength. Figure 5 As shown in Figure 2, with the increase of quercetin concentration, the fluorescence intensity of nanoclusters gradually decreased; Figure 6 As shown, the change in fluorescence intensity is linearly related to the concentration of quercetin, and the detection limit is 0.179 μmol / L (calculated according to the formula LOD=3σ / k). The regression equation obtained by linear fitting is: y=0.00806+0.00705x, and the linear coefficient is R2=0.994. The aggregation-induced yellow-green fluorescent gold-silver alloy nanoclusters can be used for the detection of quercetin in grape juice samples.
[0055] Example 9
[0056] The aggregation-induced yellow-green fluorescent gold-silver alloy nanocluster solution prepared in Example 7 and 1 mL of Tris-HCl buffer (pH=7, 50 mmol / L) were added to a fluorescence cuvette, and the fluorescence intensity was measured as a blank control; then common anions, cations, substances with similar structures to quercetin and other potential interfering substances were added, and the fluorescence intensity was measured and recorded; in the presence of the above potential interfering substances, quercetin was added, and the fluorescence intensity was measured and recorded. Figure 7 As shown; experiments have shown that only the addition of quercetin can quench the fluorescence of nanoclusters, and other interfering substances have almost no interference with the detection of quercetin.
[0057] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement or combination made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A method for preparing aggregation-induced yellow-green fluorescent gold-silver alloy nanoclusters, characterized in that: In terms of volume, 3 parts of 20 mmol / L L-cysteine solution, 2 parts of 10 mmol / L chloroauric acid solution, and 2 parts of 10 mmol / L silver nitrate solution were mixed and shaken, and the ultrasonic power was controlled to 150 W for 10 min to obtain an aggregation-induced yellow-green fluorescent gold-silver alloy nanocluster aqueous solution.
2. Aggregation-induced gold-silver alloy nanoclusters obtained according to the method of claim 1.
3. A method for detecting quercetin, characterized in that: 100 μL of the aqueous solution of the aggregation-induced gold-silver alloy nanoclusters according to claim 2 and 1 mL of a 50 mM Tris-HCl buffer solution with a pH of 7 are added to a fluorescence cuvette, and then different concentrations of quercetin solutions are added. The fluorescence spectrum is measured at 340 nm as the excitation wavelength to obtain a linear relationship between the fluorescence intensity and the quercetin concentration; based on the linear relationship, the quercetin content in the sample to be tested is quantitatively detected.
Citation Information
Patent Citations
Gold and silver bimetal nanocluster as well as preparation method and application thereof
CN114558569A