A continuous preparation method of carbon nanotube hollow fiber and its carbon nanotube hollow fiber and supercapacitor

By regulating coaxial wet spinning process parameters, the continuous preparation of carbon nanotube hollow fibers was successfully achieved, which solved the problem of insufficient fiber performance in the existing technology and achieved the preparation of high-performance carbon nanotube hollow fibers, which is suitable for super capacitor.

CN115787143BActive Publication Date: 2024-10-11SUZHOU INST OF NANO TECH & NANO BIONICS CHINESE ACEDEMY OF SCI
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211606473.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-12-14
Publication Date
2024-10-11
Estimated Expiration
2042-12-14

AI Technical Summary

Technical Problem

It is difficult to realize the continuous preparation of carbon nanotube hollow fibers with existing technology, and the mechanical properties and electrical properties of the prepared fibers are insufficient to effectively exert the excellent properties of carbon nanotubes.

Method used

By finely regulating the coaxial wet spinning process parameters, carbon nanotube spinning stock solution is used as the outer spinning solution and the inner coagulation bath for coaxial wet spinning to control the structure of the carbon nanotube fiber and ensure the continuity and performance of the fiber.

Benefits of technology

The continuous preparation of carbon nanotube hollow fibers is achieved, which has excellent mechanical properties and electrical properties and is suitable for supercapacitor materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115787143B_ABST
    Figure CN115787143B_ABST
Patent Text Reader

Abstract

The present invention provides a continuous preparation method of carbon nanotube hollow fiber and its carbon nanotube hollow fiber and supercapacitor. The preparation method comprises: using carbon nanotube spinning solution as the outer spinning solution, coaxially wet spinning with an internal coagulation bath to obtain the carbon nanotube hollow fiber; the internal coagulation bath comprises at least one of water, organic solvent or salt solution; the flow rate of the carbon nanotube spinning solution is 5 to 32 mL / h; the flow rate of the internal coagulation bath is 3 to 32 mL / h. In the present invention, the preparation method of the carbon nanotube hollow fiber realizes the controllable and continuous preparation of the hollow porous structure of the carbon nanotube fiber by adopting coaxial wet spinning, and the flow rates of the carbon nanotube spinning solution and the internal coagulation bath are within a specific range. The hollow structure provides a higher specific surface area and reduces the diffusion distance, so that the supercapacitor including the carbon nanotube fiber has excellent high specific capacitance and mechanical properties.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of preparation methods of nano-carbon materials, and specifically relates to a continuous preparation method of carbon nanotube hollow fibers and the carbon nanotube hollow fibers and supercapacitors. Background Art

[0002] Carbon nanotubes (CNTs) are made of sp 2 The tubular structure composed of hybrid carbon atoms has excellent tensile strength, modulus, electrical conductivity, thermal conductivity, conductivity and electron mobility, and is used to strengthen polymers, build field effect transistors, and improve electromagnetic shielding effectiveness. However, these excellent properties need to be displayed in the form of a macroscopic body, so how to construct a CNT macroscopic body and how to achieve the transfer of CNT microscopic properties to macroscopic properties are issues that need to be solved urgently.

[0003] CNT macroscopic bodies include films, fibers and foams, etc. CNT one-dimensional fibers can be prepared by floating catalytic chemical vapor deposition, wet spinning, electrospinning, etc. Hollow fibers are a form of one-dimensional fibers and have broad application prospects in many fields such as air and sewage filtration, catalysis, and energy. However, it is difficult to obtain continuous CNT hollow fibers using commonly used fiber preparation methods.

[0004] In the prior art, there are literature reports on the use of a coaxial spinning head to prepare CNT and polymer mixed fibers by electrospinning or wet spinning, and the polymer is quickly solidified into fibers during the spinning process to obtain hollow fibers (Wei, G.; Quan, X.; Fan, X.; Chen, S.; Zhang, Y., Carbon-nanotube-based sandwich-like hollow fiber membranes for expanded microcystin-LR removal applications. Chemical Engineering Journal 2017, 319, 212-218.). However, this hollow fiber is mainly composed of polymers and has a low CNT content, making it difficult to exert the excellent performance of CNTs.

[0005] In addition, the prior art discloses growing graphene and carbon nanotubes on the surface of nickel wires, and then removing the base nickel by solution etching to obtain graphene / carbon nanotube hollow fibers. This method has a complex process and is difficult to prepare continuously. In addition, the mechanical strength of the fibers after etching is low, which is difficult to meet application needs.

[0006] CN103031618A discloses a method for preparing graphene oxide and graphene hollow fiber, wherein the preparation method utilizes coaxial wet spinning method to prepare graphene fiber, and by controlling the inner layer and the outer layer solution to entangle the powder, the graphene hollow fiber can be obtained, which is simple to operate and can be produced continuously. After this, many works have published the work of preparing graphene hollow fiber based on coaxial wet spinning method, but the continuous preparation of carbon nanotube hollow fiber is still difficult to achieve. Because the solubility of carbon nanotube in water or solvent is much lower than that of graphene oxide, it is difficult to form a liquid crystal structure that is easy to form fiber like graphene. In addition, since the surface of graphene oxide carries a large amount of oxygen-containing groups, by changing the ion concentration in the coagulation bath, such as adding acid or adding salt ions, it is possible to make graphene oxide complex in the coagulation bath to form a fibrous structure. And these two points are not available in carbon nanotubes, and the preparation of CNT hollow fiber cannot be realized by copying the process of graphene hollow fiber.

[0007] A common shortcoming of the existing technology is that many methods can be used to prepare carbon nanotube hollow fibers, but most of them are polymer-type carbon nanotube hollow fibers, which limits the conductivity of the carbon nanotube hollow fibers, makes the fiber walls dense and lacks pores; in addition, some researchers have obtained pure carbon nanotube hollow fibers by etching away the polymer / metal core, but the hollow fibers prepared by this method have poor mechanical properties and cannot be prepared continuously.

[0008] Therefore, developing a carbon nanotube hollow fiber that has high orientation, excellent mechanical and electrical properties, and can be prepared continuously is an urgent problem to be solved in the art. Summary of the invention

[0009] In view of the shortcomings of the prior art, the present invention aims to provide a continuous preparation method of carbon nanotube hollow fibers and the carbon nanotube hollow fibers and supercapacitors thereof. The preparation method of the carbon nanotube hollow fibers finely controls the coaxial spinning process parameters, and through the coordination of various process parameters, the structure of the prepared carbon nanotube hollow fibers is controllable and can be produced continuously, so that the materials including the carbon nanotube hollow fibers have excellent electrical and mechanical properties.

[0010] To achieve this object, the present invention adopts the following technical solutions:

[0011] In a first aspect, the present invention provides a continuous preparation method of carbon nanotube hollow fibers, the preparation method comprising: using carbon nanotube spinning stock solution as the outer spinning solution, and coaxially wet spinning with an internal coagulation bath to obtain the carbon nanotube hollow fibers; the internal coagulation bath comprises at least one of water, an organic solvent or a salt solution; the flow rate of the carbon nanotube spinning stock solution is 5 to 32 mL / h; the flow rate of the internal coagulation bath is 3 to 32 mL / h.

[0012] In the present invention, wet spinning causes the carbon nanotubes to be subjected to a large shear force, which induces the carbon nanotubes to flip in the direction of the shear force in the fluid, so that the carbon nanotubes are oriented in the axial direction and are tightly bound through intermolecular interactions; and when the flow rates of the inner and outer pores of coaxial wet spinning (i.e., the flow rates of the inner coagulation bath and the outer spinning solution) are within a specific range, a hollow structure can be formed, so that the supercapacitor including the carbon nanotube hollow fiber has excellent mechanical and electrical properties.

[0013] Preferably, the flow rate of the carbon nanotube spinning solution is 5 to 32 mL / h, for example, it can be 6 mL / h, 8 mL / h, 10 mL / h, 12 mL / h, 14 mL / h, 16 ml / h, 18 mL / h, 20 mL / h, 22 mL / h, 24 mL / h, 26 mL / h, 28 mL / h, 30 mL / h, etc.

[0014] Preferably, the flow rate of the inner coagulation bath is 3 to 32 mL / h, for example, 4 mL / h, 6 mL / h, 8 mL / h, 10 mL / h, 12 mL / h, 14 mL / h, 16 mL / h, 18 mL / h, 20 mL / h, 22 mL / h, 24 mL / h, 26 mL / h, 28 mL / h, 30 mL / h, etc.

[0015] Preferably, the ratio of the flow rate of the carbon nanotube spinning solution to the flow rate of the internal coagulation bath is (1.2-5):1, for example, it can be 1.25:1, 1.3:1, 1.35:1, 1.4:1, 1.45:1, 1.5:1, 1.55:1, 1.6:1, 1.65:1, 1.7:1, 1.75:1, 1.8:1, 2:1, 2.2:1, 2.4:1, 2.6:1, 2.8:1, 3:1, 3.2:1, 3.4:1, 3.6:1, 3.8:1, 4:1, 4.2:1, 4.4:1, 4.6:1, 4.8:1, etc.

[0016] In the present invention, the flow rate of the carbon nanotube spinning solution and the flow rate of the internal coagulation bath are within a specific range, and the two are within a specific ratio, the pore distribution of the carbon nanotubes in the fiber is controllable, so that the electrical properties and mechanical properties of the capacitor including the hollow fiber are better; if the flow rate ratio of the internal coagulation bath to the carbon nanotube spinning solution is too small, fibers cannot be formed; if the flow rate ratio is too large, fibers cannot be prepared continuously.

[0017] Preferably, the method for preparing the carbon nanotube spinning stock solution comprises: mixing and dispersing carbon nanotubes with a solvent to obtain the carbon nanotube spinning stock solution.

[0018] Preferably, the mass percentage of carbon nanotubes in the carbon nanotube spinning solution is 0.4-1.5%, for example, it can be 0.5%, 0.6%, 0.7%, 0.8%, 0.9%, 1%, 1.1%, 1.2%, 1.3%, 1.4%, etc.

[0019] Preferably, the mixed material further comprises a dispersant.

[0020] Preferably, the dispersant comprises at least one of sodium cholate, sodium dodecyl sulfate or polyvinyl pyrrolidone.

[0021] Preferably, the mixing and dispersing method comprises at least one of ultrasonic dispersion, cell crushing or high-pressure homogenization.

[0022] Preferably, the mixing and dispersing further comprises a step of adding graphene oxide.

[0023] Preferably, the mass percentage of graphene oxide in the carbon nanotube spinning solution is 0.01-1%, for example, it can be 0.02%, 0.03%, 0.04%, 0.05%, 0.06%, 0.07%, 0.08%, 0.09%, 0.1%, 0.2%, 0.3%, 0.4%, 0.5%, 0.6%, 0.7%, 0.8%, 0.9% and the like.

[0024] Preferably, the flake diameter of the graphene oxide is 0.1-10 μm, for example, it can be 0.2 μm, 0.4 μm, 0.6 μm, 0.8 μm, 1 μm, 1.2 μm, 1.4 μm, 1.6 μm, 2 μm, 2.5 μm, 3 μm, 3.5 μm, 4 μm, 4.5 μm, 5 μm, 5.5 μm, 6 μm, 6.5 μm, 7 μm, 7.5 μm, 8 μm, 8.5 μm, 9 μm, 9.5 μm, etc.

[0025] In the present invention, the addition of graphene oxide helps to achieve the continuous preparation of carbon nanotube hollow fibers, and on the other hand is conducive to controlling the pore structure and distribution in the fibers, thereby obtaining continuous carbon nanotube hollow fibers with a hollow structure and multiple pores.

[0026] Preferably, the organic solvent comprises at least one of methanol, ethanol, isopropanol or acetone.

[0027] Preferably, the salt solution comprises calcium chloride solution and / or magnesium chloride solution.

[0028] Preferably, the internal coagulation bath comprises a combination of water and an organic solvent.

[0029] Preferably, the volume ratio of water to the organic solvent is (0.1-0.9):1, for example, it can be 0.12, 0.14, 0.16, 0.18, 0.2, 0.22:1, 0.24:1, 0.26:1, 0.28:1, 0.3:1, 0.32:1, 0.34:1, 0.36:1, 0.38:1, 0.4:1, 0.42:1, 0.44:1, 0.46:1, 0.48:1, 0.5:1, 0.52:1, 0.56:1, 0.6:1, 0.62:1, 0.66:1, 0.7:1, 0.74:1, 0.76:1, 0.78:1, 0.82:1, 0.84:1, 0.88:1, etc.

[0030] Preferably, the specific steps of the coaxial wet spinning include:

[0031] The carbon nanotube spinning stock solution and the internal coagulation bath are extruded and coagulated to obtain the carbon nanotube hollow fiber.

[0032] Preferably, the extrusion device comprises a coaxial syringe pump.

[0033] Preferably, the coagulation bath for coagulation comprises at least one of water, an organic solvent or a salt solution.

[0034] Preferably, in the coagulation bath, the organic solvent includes at least one of methanol, ethanol, isopropanol or acetone.

[0035] Preferably, in the coagulation bath, the salt solution includes a calcium chloride solution and / or a magnesium chloride solution.

[0036] Preferably, the coagulation bath comprises a combination of water and an organic solvent.

[0037] Preferably, in the coagulation bath, the volume ratio of water to the organic solvent is (0.1-0.9):1, for example, it can be 0.22:1, 0.24:1, 0.26:1, 0.28:1, 0.3:1, 0.32:1, 0.34:1, 0.36:1, 0.38:1, 0.4:1, 0.42:1, 0.44:1, 0.46:1, 0.48:1, 0.5:1, 0.52:1, 0.56:1, 0.6:1, 0.62:1, 0.66:1, 0.7:1, 0.74:1, 0.76:1, 0.78:1, 0.82:1, 0.84:1, 0.88:1, etc.

[0038] In the present invention, the coagulation bath is a mixed solution of an organic solvent and water, and the organic solvent and water are within a specific ratio, which can control the liquid exchange rate during the fiber formation process, thereby obtaining a hollow fiber with CNT as the main body. If the specific ratio is exceeded, the fiber cannot be continuously formed or a hollow structure cannot be formed.

[0039] Preferably, the coagulation bath comprises a rotating coagulation bath.

[0040] Preferably, the rotation speed of the coagulation bath is 800-1200 m / h, for example, it can be 820 m / h, 840 m / h, 860 m / h, 880 m / h, 900 m / h, 920 m / h, 940 m / h, 960 m / h, 980 m / h, 1000 m / h, 1050 m / h, 1100 m / h, 1150 m / h, 1180 m / h, etc.

[0041] Preferably, the step of rolling up and / or drying is further included after solidification.

[0042] Preferably, the winding speed is 1000-1600 m / h, for example, it can be 1050 m / h, 1100 m / h, 1150 m / h, 1200 m / h, 1250 m / h, 1300 m / h, 1350 m / h, 1400 m / h, 1450 m / h, 1500 m / h, 1550 m / h, etc., and more preferably 1000-1500 m / h.

[0043] Preferably, the drying temperature is 20-80°C, for example, 25°C, 30°C, 35°C, 40°C, 45°C, 50°C, 55°C, 60°C, 65°C, 70°C, 75°C, etc.

[0044] Preferably, the drying further includes a high-temperature calcination step.

[0045] Preferably, the temperature of the high temperature calcination is 500-1500°C, for example, it can be 550°C, 600°C, 650°C, 680°C, 700°C, 750°C, 800°C, 850°C, 900°C, 950°C, 1000°C, 1100°C, 1200°C, 1300°C, 1400°C, etc.

[0046] In the present invention, the purpose of the high temperature calcination is to reduce the graphene oxide to graphene and form a specific pore structure, thereby further improving the mechanical and electrical properties of the capacitor.

[0047] As a preferred technical solution of the present invention, the preparation method specifically comprises the following steps:

[0048] (1) mixing and dispersing carbon nanotubes with a solvent and an optional dispersant, and adding optional graphene oxide to obtain a carbon nanotube spinning solution;

[0049] (2) The carbon nanotube spinning stock solution obtained in step (1) is used as the outer spinning solution, extruded together with the inner coagulation bath through a coaxial injection pump, coagulated in the coagulation bath to form fibers, and wound up to obtain the carbon nanotube hollow fibers; the flow rate of the carbon nanotube spinning stock solution is 5 to 32 mL / h; the flow rate of the inner coagulation bath is 3 to 32 mL / h; the rotation speed of the coagulation bath is 800 to 1200 m / h; and the winding speed is 1000 to 1600 m / h.

[0050] In the present invention, the carbon nanotube fiber obtained by a specific preparation method has the characteristics of being hollow, porous and thin-walled. This characteristic avoids the defects of the skin-core structure of solid fibers, retains only an oriented, porous thin-walled layer, and improves the specific surface area and mechanical strength of the fiber. The solid fiber prepared by the traditional method has a skin-core structure with a dense skin layer and a loose core layer. The loose core layer has low load transfer efficiency and therefore contributes less to the mechanical and electrical properties of the fiber.

[0051] In a second aspect, the present invention provides a carbon nanotube hollow fiber, wherein the carbon nanotube hollow fiber is prepared by the preparation method according to the first aspect.

[0052] In the present invention, the wall thickness of the carbon nanotube hollow fiber is 2 to 100 μm, for example, 5 μm, 10 μm, 20 μm, 30 μm, 40 μm, 50 μm, 60 μm, 70 μm, 80 μm, 90 μm, etc.

[0053] In the present invention, a scanning electron microscope (model: S-4800) is used to characterize the wall thickness of the carbon nanotube hollow fiber.

[0054] In a third aspect, the present invention provides a supercapacitor, comprising an electrolyte and the carbon nanotube hollow fiber according to the first aspect.

[0055] Preferably, the supercapacitor comprises a fiber-shaped supercapacitor.

[0056] In the present invention, since the wall thickness of the carbon nanotube hollow fiber is relatively small, the distance for the electrolyte to enter the fiber is shortened. In the obtained supercapacitor, the electrolyte is evenly distributed in the hollow fiber wall, forming a structure in which the carbon nanotubes and the electrolyte are evenly distributed, thereby improving the performance of the supercapacitor. Traditional solid fibers have a dense cortex, and the electrolyte can only diffuse into the cortex, but is hindered and difficult to diffuse into the core layer. Only the outer surface provides surface area, thereby wasting a large amount of fiber volume capacity, resulting in poor capacitance performance.

[0057] The numerical range described in the present invention not only includes the point values ​​listed above, but also includes any point values ​​between the above numerical ranges that are not listed. Due to space limitations and for the sake of simplicity, the present invention no longer exhaustively lists the specific point values ​​included in the range.

[0058] Compared with the prior art, the present invention has the following beneficial effects:

[0059] The method for preparing the carbon nanotube hollow fiber provided by the present invention adopts coaxial wet spinning, and the flow rates of the carbon nanotube spinning stock solution and the internal coagulation bath are within a specific range, so that the microstructure and macrostructure of the carbon nanotube fiber can be effectively controlled, which is beneficial to the contact between the electrolyte and the carbon nanotube, so that the supercapacitor including the carbon nanotube fiber has excellent mechanical properties and electrical properties. BRIEF DESCRIPTION OF THE DRAWINGS

[0060] Figure 1 Cyclic voltammetry curves of the carbon nanotube hollow fiber (hollow fiber) obtained by the preparation method provided in Example 1 and the carbon nanotube fiber (solid fiber) obtained by the preparation method provided in Comparative Example 5 before and after treatment at 1500° C.;

[0061] Figure 2 The constant current charge and discharge curves of the carbon nanotube hollow fiber (hollow fiber) obtained by the preparation method provided in Example 1 and the carbon nanotube fiber (solid fiber) obtained by the preparation method provided in Comparative Example 5 before and after treatment at 1500°C.

[0062] Figure 3 This is a microscopic morphology of the carbon nanotube hollow fiber obtained by the preparation method provided in Example 1. DETAILED DESCRIPTION

[0063] The technical solution of the present invention is further described below by specific implementation methods. It should be understood by those skilled in the art that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention.

[0064] In the present invention, the materials used are as follows:

[0065] Carbon nanotubes: Manufacturer: OCSiAl; Brand: single-walled carbon nanotubes

[0066] Example 1

[0067] This embodiment provides a method for preparing a carbon nanotube hollow fiber, which specifically includes the following steps:

[0068] (1) uniformly mixing carbon nanotubes and sodium dodecyl sulfate in water, and ultrasonically dispersing the mixture to prepare a carbon nanotube dispersion; adding graphene oxide to the carbon nanotube dispersion to obtain a carbon nanotube spinning solution, wherein the mass fraction of the carbon nanotubes in the carbon nanotube spinning solution is 0.4 wt %, and the mass fraction of the graphene oxide is 0.1 wt %;

[0069] (2) The carbon nanotube spinning stock solution obtained in step (1) is used as the outer spinning solution, and a mixed solution of water and ethanol in a volume ratio of 0.5:1 is used as the inner coagulation bath, which are loaded into a coaxial syringe pump and extruded into the coagulation bath by the coaxial syringe pump to form fibers, and then the fibers are rolled up and dried at 60°C and calcined at a high temperature of 1500°C to obtain the carbon nanotube hollow fiber (wall thickness 25 μm); when the coaxial syringe pump is extruded, the flow rate of the carbon nanotube spinning stock solution is 5 mL / h, and the flow rate of the inner coagulation bath is 3 mL / h; the coagulation bath is a mixed solution of ethanol and water, and the mixing volume ratio is ethanol: water = 1:0.2, the speed of the coagulation bath is 1000 m / h, and the winding speed is 1500 m / h.

[0070] The morphology of the carbon nanotube hollow fibers obtained in Example 1 was characterized using a scanning electron microscope (model: S-4800). Figure 3 shown.

[0071] Example 2

[0072] This embodiment provides a method for preparing a carbon nanotube hollow fiber, which specifically includes the following steps:

[0073] (1) uniformly mixing carbon nanotubes and sodium dodecyl sulfate in water, and ultrasonically dispersing the mixture to prepare a carbon nanotube dispersion; adding graphene oxide to the carbon nanotube dispersion to obtain a carbon nanotube spinning stock solution, wherein the mass fraction of the carbon nanotubes in the carbon nanotube spinning stock solution is 1 wt %, and the mass fraction of the graphene oxide is 0.5 wt %;

[0074] (2) The carbon nanotube spinning stock solution obtained in step (1) is used as the outer spinning solution, and a mixed solution of water and isopropanol with a volume ratio of 0.3:1 is used as the inner coagulation bath, which are loaded into a coaxial syringe pump, and extruded into the coagulation bath by the coaxial syringe pump to form fibers, and then the fibers are rolled up and dried at 80°C and calcined at a high temperature of 600°C to obtain the carbon nanotube hollow fiber (wall thickness 50 μm); when the coaxial syringe pump is extruded, the flow rate of the carbon nanotube spinning stock solution is 10 mL / h, and the flow rate of the inner coagulation bath is 8 mL / h; the coagulation bath is a mixed solution of isopropanol and water, and the mixing volume ratio is isopropanol:water=1:0.15, the speed of the coagulation bath is 1200 m / h, and the winding speed is 1500 m / h.

[0075] Example 3

[0076] This embodiment provides a method for preparing a carbon nanotube hollow fiber, which specifically includes the following steps:

[0077] (1) uniformly mixing carbon nanotubes and sodium dodecyl sulfate in water, and ultrasonically dispersing the mixture to prepare a carbon nanotube dispersion; adding graphene oxide to the carbon nanotube dispersion to obtain a carbon nanotube spinning solution, wherein the mass fraction of the carbon nanotubes in the carbon nanotube spinning solution is 1.5 wt %, and the mass fraction of the graphene oxide is 1 wt %;

[0078] (2) The carbon nanotube spinning stock solution obtained in step (1) is used as the outer spinning solution, and a mixed solution of water and acetone with a volume ratio of 0.8:1 is used as the inner coagulation bath, which are loaded into a coaxial injection pump, and extruded into the coagulation bath by the coaxial injection pump to form fibers, and then the fibers are rolled up and dried at 80°C and calcined at a high temperature of 600°C to obtain the carbon nanotube hollow fiber (wall thickness 100 μm); when the coaxial injection pump is extruded, the flow rate of the carbon nanotube spinning stock solution is 20 mL / h, and the flow rate of the inner coagulation bath is 15 mL / h; the coagulation bath is a mixed solution of ethanol and water, and the mixing volume ratio is ethanol: water = 1:0.1, the speed of the coagulation bath is 800 m / h, and the winding speed is 1000 m / h.

[0079] Example 4

[0080] This embodiment provides a method for preparing carbon nanotube hollow fibers, which differs from Embodiment 1 only in that, during the coaxial injection pump extrusion in step (2), the flow rate of the carbon nanotube spinning solution is 30 mL / h, and the flow rate of the internal coagulation bath is 25 mL / h. The other steps and parameters are the same as those in Embodiment 1.

[0081] Example 5

[0082] This embodiment provides a method for preparing carbon nanotube hollow fibers, which differs from Embodiment 1 only in that, during the coaxial injection pump extrusion in step (2), the flow rate of the carbon nanotube spinning solution is 32 mL / h, and the flow rate of the internal coagulation bath is 6 mL / h. The other steps and parameters are the same as those in Embodiment 1.

[0083] Example 6

[0084] This embodiment provides a method for preparing a carbon nanotube hollow fiber, which differs from Embodiment 1 only in that in step (1), graphene oxide is not added, and the other steps and parameters are the same as those in Embodiment 1.

[0085] Example 7

[0086] This embodiment provides a method for preparing a carbon nanotube hollow fiber. The only difference between this method and Embodiment 1 is that the internal coagulation bath is a mixed solution of water and ethanol in a volume ratio of 1:1. The other steps and parameters are the same as those in Embodiment 1.

[0087] Example 8

[0088] This embodiment provides a method for preparing a carbon nanotube hollow fiber. The only difference between this method and Embodiment 1 is that the internal coagulation bath is a mixed solution of water and ethanol in a volume ratio of 0.1:1. The other steps and parameters are the same as those in Embodiment 1.

[0089] Example 9

[0090] This embodiment provides a method for preparing carbon nanotube hollow fibers, which differs from Embodiment 1 only in that, in step (2), the speed of the coagulation bath is 700 m / h, and the other steps and parameters are the same as those in Embodiment 1.

[0091] Example 10

[0092] This embodiment provides a method for preparing carbon nanotube hollow fibers, which differs from Embodiment 1 only in that, in step (2), the speed of the coagulation bath is 1600 m / h, and the other steps and parameters are the same as those in Embodiment 1.

[0093] Embodiment 11

[0094] This embodiment provides a method for preparing a carbon nanotube hollow fiber. The only difference between this method and the first embodiment is that in step (2), the coagulation bath is water. The other steps and parameters are the same as those in the first embodiment.

[0095] Example 12

[0096] This embodiment provides a method for preparing a carbon nanotube hollow fiber, which differs from Embodiment 1 only in that, in step (2), the ratio of ethanol to water in the coagulation bath is 1:0.5, and the other steps and parameters are the same as those in Embodiment 1.

[0097] Example 13

[0098] This embodiment provides a method for preparing a carbon nanotube hollow fiber, which differs from Embodiment 1 only in that in step (2), the winding speed is 2200 m / h, and the other steps and parameters are the same as those in Embodiment 1.

[0099] Comparative Example 1

[0100] This comparative example provides a method for preparing carbon nanotube hollow fibers, which differs from Example 1 only in that, during the coaxial syringe pump extrusion in step (2), the flow rate of the carbon nanotube spinning stock solution is 3 mL / h, and the other steps and parameters are the same as those in Example 1.

[0101] Comparative Example 2

[0102] This comparative example provides a method for preparing carbon nanotube hollow fibers, which differs from Example 1 only in that, during the coaxial injection pump extrusion in step (2), the flow rate of the carbon nanotube spinning solution is 40 mL / h, and the other steps and parameters are the same as those in Example 1.

[0103] Comparative Example 3

[0104] This comparative example provides a method for preparing carbon nanotube hollow fibers, which differs from Example 1 only in that, during the coaxial syringe pump extrusion in step (2), the flow rate of the internal coagulation bath is 1 mL / h, and the other steps and parameters are the same as those in Example 1.

[0105] Comparative Example 4

[0106] This comparative example provides a method for preparing carbon nanotube fibers, which differs from Example 1 only in that, during the coaxial syringe pump extrusion in step (2), the flow rate of the internal coagulation bath is 40 mL / h, and the other steps and parameters are the same as those in Example 1.

[0107] Comparative Example 5

[0108] This comparative example provides a method for preparing carbon nanotube fibers, which differs from Example 1 only in that the coaxial injection pump is replaced by a uniaxial injection pump in step (2), the extrusion flow rate of the carbon nanotube spinning solution is 5 mL / h, and the other steps and parameters are the same as those in Example 1.

[0109] Application Examples

[0110] A supercapacitor comprises an aqueous electrolyte (Shanghai McLean Biochemical Technology Co., Ltd.; CAS: 54010-75-2) and the carbon nanotube hollow fibers obtained in Examples 1 to 13 and Comparative Examples 1 to 4, and the carbon nanotube solid fibers obtained in Comparative Example 5. The preparation method of the supercapacitor comprises:

[0111] It consists of two CNT / rGO hollow fiber electrodes and PVA / H3PO4 gel electrolyte. Specifically, the two electrodes are immersed in the electrolyte for about 1 hour, and then placed side by side in parallel with a spacing of about 0.2 cm. They are cured for about 5 hours, and the electrodes are coated with electrolyte again and dried at room temperature. The assembled linear device with a length of 1 cm is directly used for CV and GCD tests. The preparation method of the electrolyte is as follows: 1g of PVA is dissolved in 10mL of deionized water, heated at 90°C for 2h under continuous stirring, and when the mixture becomes clear, 1g of H3PO4 is added dropwise at a dropping speed of 1 drop / s, and stirred for 30min to obtain the electrolyte.

[0112] Performance Testing

[0113] The following performance tests were performed on the carbon nanotube hollow fibers obtained in Examples 1 to 13, Comparative Examples 1 to 4, and the carbon nanotube solid fibers obtained in Comparative Example 5;

[0114] (1) Tensile strength: Select 3 m long continuous fiber and weigh it on a microbalance to record the mass; fiber density = mass / length; then, prepare 5 samples of the same length (1 cm long) for each sample and perform a tensile test on an instron 3365 mechanical tensile tester at a tensile speed of 0.5 mm / min. Record the load data of each sample and calculate the specific strength of each sample using the specific strength calculation formula (specific strength = strength / fiber density). Finally, average the results to obtain the specific strength data of each sample.

[0115] (2) Specific capacitance: The capacitance study was carried out on a CHI 760E electrochemical workstation using a three-electrode test apparatus. CNT / rGO (1 cm), saturated calomel electrode and Pt were used as the working electrode, reference electrode and counter electrode, respectively, and 2 M zinc trifluoromethanesulfonate solution was used as the electrolyte. The cyclic voltammetry curves of 2 to 50 mV / s were studied in the potential range of 0 to 1.1 V and the cyclic voltammetry curves of 0.3 A / cm 3 -1.5A / cm 3 Constant current charge and discharge tests were carried out within the range of ; the specific capacitance was recorded;

[0116] Among them, “ / ” means that the test cannot be performed and the test is meaningless.

[0117] The carbon nanotube hollow fiber (hollow fiber) obtained by the preparation method provided in Example 1 and the carbon nanotube fiber (solid fiber) obtained by the preparation method provided in Comparative Example 5 before and after treatment at 1500°C are used as electrodes. The cyclic voltammetry curves in the range of 2 to 50 mV / s are as follows: Figure 1 As shown;

[0118] The carbon nanotube hollow fiber (hollow fiber) obtained by the preparation method provided in Example 1 and the carbon nanotube fiber (solid fiber) obtained by the preparation method provided in Comparative Example 5 before and after treatment at 1500°C were used as electrodes. 3 -1.5A / cm 3 The constant current charge and discharge curve within the range of Figure 2 shown.

[0119] The specific test results are shown in Table 1:

[0120] Table 1

[0121]

[0122]

[0123] As can be seen from the above table, the preparation method of the carbon nanotube hollow fiber provided by the present invention adopts coaxial wet spinning, and the flow rates of the carbon nanotube spinning stock solution and the core layer spinning solution are within a specific range, so that the orientation degree of the carbon nanotube fiber can be improved, and the prepared carbon nanotube structure is controllable, has a hollow and porous structure, and can be produced continuously. The hollow fiber has excellent mechanical properties and electrical properties, and is particularly suitable for use as a capacitor material; as can be seen from Examples 1 to 4, the tensile strength of the carbon nanotube hollow fiber is 0.27 to 0.42 N / tex, and the specific capacitance is 134 to 163 F / cm 3 .

[0124] It can be seen from the comparison between Example 1 and Examples 7 to 8 that the internal coagulation bath is not of a specific composition, the fiber coagulation process is affected, the fiber strength is poor, the porosity is low, and the capacitance performance is poor.

[0125] It can be seen from the comparison between Example 1 and Examples 9 to 12 that the coagulation bath is not a specific combination or rotation speed, and the fiber strength is poor or cannot be formed into fibers or cannot be prepared continuously.

[0126] It can be seen from the comparison between Example 1 and Example 13 that the winding speed is not within the specific range, the fiber breaks during winding, and continuous winding is impossible.

[0127] By comparing Example 1 with Comparative Examples 1 to 4, it can be seen that in the coaxial spinning, the flow rates of the carbon nanotube spinning solution and the internal coagulation bath are not within a specific range, and the fibers cannot maintain a hollow structure, or are collapsed or solid; by comparing Examples 1 to 4 with Comparative Example 5, it can be seen that the mechanical properties and electrical properties of the carbon nanotube hollow fibers obtained by the preparation method provided by the present invention are better than those of the solid fibers obtained by uniaxial wet spinning.

[0128] In summary, the preparation method of the carbon nanotube fiber provided by the present invention adopts coaxial wet spinning and adopts specific process parameters to make the carbon nanotube fiber highly oriented, so that the carbon nanotube fiber has a hollow, porous structure and a controllable structure, and can be prepared continuously. The hollow fiber structure provides a higher specific surface area and reduces the diffusion distance, so that the supercapacitor including the carbon nanotube fiber has excellent high specific capacitance and mechanical properties.

[0129] The specific embodiments described above further illustrate the objectives, technical solutions and beneficial effects of the present invention in detail. It should be understood that the above description is only a specific embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. A method for continuously preparing carbon nanotube hollow fibers, characterized in that: The preparation method comprises: Using carbon nanotube spinning stock solution as the outer spinning solution and coaxially wet spinning with the inner coagulation bath to obtain the carbon nanotube hollow fiber; The specific steps of the coaxial wet spinning include: Extruding and coagulating the carbon nanotube spinning solution and the internal coagulation bath to obtain the carbon nanotube hollow fiber; The extrusion equipment includes a coaxial syringe pump; The internal coagulation bath is a combination of water and an organic solvent in a volume ratio of (0.1-0.9):1; The flow rate of the carbon nanotube spinning solution is 5 to 32 mL / h; The flow rate of the internal coagulation bath is 3 to 32 mL / h; The ratio of the flow rate of the carbon nanotube spinning solution to the flow rate of the internal coagulation bath is (1.2-5):

1.

2. The preparation method according to claim 1, characterized in that: The method for preparing the carbon nanotube spinning stock solution comprises: mixing and dispersing the carbon nanotubes and a solvent to obtain the carbon nanotube spinning stock solution.

3. The preparation method according to claim 2, characterized in that: The mass percentage of carbon nanotubes in the carbon nanotube spinning stock solution is 0.4-1.5%.

4. The preparation method according to claim 2, characterized in that: The mixed material also includes a dispersant.

5. The preparation method according to claim 4, characterized in that: The dispersant includes at least one of sodium cholate, sodium dodecyl sulfate or polyvinyl pyrrolidone.

6. The preparation method according to claim 2, characterized in that: The mixing and dispersing method includes at least one of ultrasonic dispersion, cell crushing or high-pressure homogenization.

7. The preparation method according to claim 2, characterized in that: The method further comprises the step of adding graphene oxide after the mixing and dispersing.

8. The preparation method according to claim 7, characterized in that: The mass percentage of graphene oxide in the carbon nanotube spinning solution is 0.01-1%.

9. The preparation method according to claim 7, characterized in that: The sheet diameter of the graphene oxide is 0.1 to 10 μm.

10. The preparation method according to claim 1, characterized in that: The organic solvent includes at least one of methanol, ethanol, isopropanol or acetone.

11. The preparation method according to claim 1, characterized in that: The coagulation bath for coagulation includes at least one of water, an organic solvent or a salt solution.

12. The preparation method according to claim 11, characterized in that: In the coagulation bath, the organic solvent includes at least one of methanol, ethanol, isopropanol or acetone.

13. The preparation method according to claim 11, characterized in that: In the coagulation bath, the salt solution includes calcium chloride solution and / or magnesium chloride solution.

14. The preparation method according to claim 11, characterized in that: The coagulation bath includes a combination of water and an organic solvent.

15. The preparation method according to claim 14, characterized in that: In the coagulation bath, the volume ratio of water to organic solvent is (0.1-0.9):

1.

16. The preparation method according to claim 11, characterized in that: The coagulation bath includes a rotating coagulation bath.

17. The preparation method according to claim 11, characterized in that: The rotation speed of the coagulation bath is 800-1200 m / h.

18. The preparation method according to claim 1, characterized in that: After the solidification, the method further comprises the steps of winding and / or drying.

19. The preparation method according to claim 18, characterized in that: The winding speed is 1000-1600 m / h.

20. The preparation method according to claim 19, characterized in that: The winding speed is 1000-1500 m / h.

21. The preparation method according to claim 18, characterized in that: The drying temperature is 20-80°C.

22. The preparation method according to claim 18, characterized in that: The method further comprises a high-temperature calcination step after the drying.

23. The preparation method according to claim 22, characterized in that: The high temperature calcination temperature is 500-1500°C.

24. The preparation method according to claim 1, characterized in that: The preparation method specifically comprises the following steps: (1) mixing and dispersing carbon nanotubes with a solvent and an optional dispersant, and adding optional graphene oxide to obtain a carbon nanotube spinning solution; (2) The carbon nanotube spinning solution obtained in step (1) is used as the outer spinning solution, extruded together with the inner coagulation bath through a coaxial injection pump, coagulated in the coagulation bath to form fibers, and wound up to obtain the carbon nanotube hollow fibers; the flow rate of the carbon nanotube spinning solution is 5 to 32 mL / h; the flow rate of the inner coagulation bath is 3 to 32 mL / h; the inner coagulation bath is a combination of water and an organic solvent in a volume ratio of (0.1 to 0.9):1; the rotation speed of the coagulation bath is 800 to 1200 m / h; and the winding speed is 1000 to 1600 m / h.

25. A carbon nanotube hollow fiber, characterized in that: The carbon nanotube hollow fiber is prepared by the preparation method according to any one of claims 1 to 24.

26. A supercapacitor, characterized in that: The supercapacitor comprises an electrolyte and the carbon nanotube hollow fiber as claimed in claim 25 .

27. The supercapacitor according to claim 26, characterized in that The supercapacitor includes a fiber-shaped supercapacitor.