Zirconia sintered bodies for dental applications
By using a multi-layered zirconia preburning body in zirconia dental patches, using monoclinic crystal system and yttrium oxide distribution with different content rates, the light transmittance, tone and intensity after short-term firing is solved. Problem, a dental patch is achieved that matches natural teeth.
Patent Information
- Application Number
- CN202180047202.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2020-07-01
- Filing Date
- 2021-07-01
- Publication Date
- 2024-11-05
- Estimated Expiration
- 2041-07-01
AI Technical Summary
The existing zirconia dental patches cannot take into account the requirements of light transmittance, tone and intensity when firing for a short time, and the different contents of multiple yttrium oxides make it impossible to adapt to the requirements of various natural teeth.
The zirconia preburned body with at least three layers of laminated structure is adopted, wherein the main crystal system is a monoclinic crystal system, the content of the stabilizer is different from each other and contains colored components. By adjusting the content of the yttrium oxide and the distribution of the stabilizer, sintering is ensured. The body has suitable tone, light transmittance and intensity after a short period of time.
After a short time of firing, the zirconia sintered body has the same light transmittance and tone gradient as the natural teeth, and reduces the poor sintering shrinkage rate, ensuring that the dental patches are free from deformation and cracks.
Smart Images

Figure CN115802980B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a zirconia calcined body suitable for dental use, a method for producing the same, and a method for producing a dental product.
[0002] Zirconia is a compound that undergoes phase transitions between multiple crystal systems. Therefore, partially stabilized zirconia (PSZ; Partially-Stabilized Zirconia) and fully stabilized zirconia, which suppress phase transitions by dissolving stabilizers such as yttria (yttrium oxide; Y2O3) in zirconia, are used in various fields.
[0003] In the dental field, zirconium oxide materials are used as framework materials due to their high strength. In addition, in recent years, as the light transmittance of zirconium oxide materials has increased, the number of dental restorations made of only zirconium oxide has increased. Patent Document 1 discloses a zirconium oxide sintered body having different yttria contents in each layer, which exhibits appropriate light transmittance as a dental restoration by reducing the yttria content from the cutting end to the tooth neck. Patent Document 2 discloses a zirconium oxide sintered body containing a pigment having different yttria contents in each layer, which exhibits appropriate light transmittance as a dental restoration by reducing the yttria content from the cutting end to the tooth neck.
[0004] In addition, the production of dental prostheses made of only zirconium oxide is often carried out in dental laboratories, but in recent years, the production of dental prostheses in dental hospitals has also increased, and with this, the demand for zirconium oxide fired in a short time has increased. Patent document 3 discloses a zirconium oxide calcined body that has high light transmittance even after firing in a short time and is suitable for dental use.
[0005] Prior art literature
[0006] Patent Literature
[0007] Patent Document 1: U.S. Patent Application Publication No. 2013 / 0221554
[0008] Patent Document 2: U.S. Patent Application Publication No. 2016 / 0120765
[0009] Patent Document 3: International Publication No. 2018 / 056330 Summary of the invention
[0010] Problems to be solved by the invention
[0011] As described above, in recent years, the use of zirconia dental prostheses for easy production in dental clinics has increased, and it is necessary to maintain strength using only zirconia while showing excellent aesthetics. In addition, in order to cope with one-day treatments in dental clinics, it is necessary to be able to fire in a short time.
[0012] The zirconia described in Patent Documents 1 and 2 is considered to have layers with different yttrium oxide contents, and has appropriate light transmittance and strength as a dental prosthesis, but there is a problem that the holding time at the maximum firing temperature is 2 hours during firing, and it is not possible to fire in a short time. In addition, dental prostheses need to be prepared in multiple varieties to fit various natural teeth, but the yttrium oxide contents of the various layers of the zirconia described in Patent Documents 1 and 2 are completely different, and there is a problem that it is not possible to fully cope with the various light transmittances, colors, and strengths required for dental prostheses.
[0013] In the zirconia calcined body described in Patent Document 3, at least a portion of yttrium oxide is not dissolved in zirconia, and even if sintered for a short time (e.g., 30 minutes of holding time at the maximum sintering temperature), a sintered body having the same light transmittance as that under the existing sintering conditions (holding time at the maximum sintering temperature = 2 hours) can be produced. However, the yttrium oxide content of the sintered body is constant from the tooth neck to the cutting end, and there is a problem that the light transmittance and color tone required at the cutting end and the strength and color tone required at the tooth neck cannot be achieved at the same time.
[0014] Therefore, there is a demand for a zirconia calcined body which has a color tone, light transmittance, and strength suitable for use in dentistry (particularly, use in dental clinics) even if the sintered body is sintered in a short time.
[0015] Means for solving problems
[0016] As a result of intensive studies to solve the above problems, the present inventors have found that the above problems can be solved by preparing a calcined zirconium oxide body whose main crystal system is monoclinic and preparing a calcined zirconium oxide body in which the contents of stabilizers and coloring components in each layer are appropriately adjusted. Based on this finding, the present inventors have conducted further studies and completed the present invention.
[0017] That is, the present invention includes the following inventions.
[0018] [1] A calcined zirconium oxide body having a laminated structure of at least three layers containing zirconium oxide and a stabilizer capable of suppressing phase transformation of zirconium oxide,
[0019] The main crystal system of zirconium oxide is monoclinic system.
[0020] The laminated structure has at least two layers having different contents of the stabilizer relative to the total molar content of zirconium oxide and the stabilizer.
[0021] The laminated structure has at least two layers having substantially the same content ratio of the stabilizer relative to the total molar content of zirconium oxide and the stabilizer.
[0022] All the layers having substantially the same content of the stabilizer contain a coloring component, and the compositions of the coloring components in the layers are different from each other.
[0023] [2] The zirconia calcined body according to [1], wherein layers having substantially the same content of the stabilizer are adjacent to each other.
[0024] [3] The zirconium oxide calcined body according to [1] or [2], wherein the coloring component comprises an oxide of at least one element selected from the group consisting of Ti, V, Cr, Mn, Fe, Co, Ni, Pr, Tb and Er, or (Zr, V)O2.
[0025] [4] The calcined zirconium oxide according to any one of [1] to [3], wherein 55% or more of the zirconium oxide is monoclinic.
[0026] [5] The calcined zirconium oxide according to any one of [1] to [4], wherein 75% or more of the zirconium oxide is monoclinic.
[0027] [6] The zirconia calcined body according to any one of [1] to [5], wherein the layers having different contents of the stabilizer have different monoclinic crystal ratios.
[0028] [7] The zirconia calcined body according to any one of [1] to [6], wherein the layered structure includes only one layer having the highest content of the stabilizer.
[0029] [8] The zirconia calcined body according to any one of [1] to [7], wherein the layer having the highest content of the stabilizer does not contain a coloring component.
[0030] [9] The zirconia calcined body according to any one of [1] to [7], wherein the layer having the highest content of the stabilizer contains a coloring component.
[0031]
[10] The zirconia calcined body according to [9], wherein the composition of the coloring component contained in the layer having the highest content of the stabilizer is different from the composition of the coloring component in the other layers.
[0032]
[11] The zirconia calcined body according to any one of [1] to
[10] , wherein at least a part of the stabilizer is not dissolved in the zirconia.
[0033]
[12] The zirconia calcined body according to any one of [1] to
[11] , wherein on a straight line extending in a first direction from one end to the other end of the zirconia calcined body,
[0034] In the layers having different contents of the stabilizer, the increasing and decreasing tendency of the content of the stabilizer relative to the total molar amount of zirconium oxide and the stabilizer does not change from one end to the other end.
[0035]
[13] The zirconium oxide calcined body according to any one of [1] to
[12] , wherein the stabilizer is yttrium oxide.
[0036]
[14] The zirconia calcined body according to
[13] , wherein on a straight line extending in a first direction from one end to the other end of the zirconia calcined body,
[0037] For the layers having different yttrium oxide contents, the increasing and decreasing tendency of the content of the stabilizer relative to the total molar amount of zirconium oxide and the stabilizer does not change from one end to the other end.
[0038] With respect to the total mol of the aforementioned zirconium oxide and the aforementioned yttrium oxide,
[0039] The yttrium oxide content of the layer including the one end is 3.5 mol% or more and 6.5 mol% or less,
[0040] The yttrium oxide content of the layer including the other end is 2.5 mol % or more and less than 4.5 mol %.
[0041]
[15] The zirconia calcined body according to
[14] , wherein on a straight line extending in the first direction from one end to the other end of the zirconia calcined body,
[0042] For the layers having different yttrium oxide contents, the increasing and decreasing tendency of the content of the stabilizer relative to the total molar amount of zirconium oxide and the stabilizer does not change from one end to the other end.
[0043] With respect to the total mol of the aforementioned zirconium oxide and the aforementioned yttrium oxide,
[0044] The difference in yttrium oxide content between the layer including the one end and the layer including the other end is 3.0 mol % or less.
[0045]
[16] The zirconium oxide calcined body according to any one of
[13] to
[15] , wherein a peak of yttrium oxide exists in the X-ray diffraction pattern.
[0046]
[17] The zirconia calcined body according to any one of
[13] to
[16] , wherein f calculated based on the following formula (1) y Greater than 0%,
[0047] [Number 1]
[0048]
[0049] (Among them, I y (111) represents the peak intensity of the (111) plane of yttrium oxide at around 2θ=29° in the X-ray diffraction pattern using CuKα line,
[0050] Im (111) and I m (11-1) represents the peak intensity of the (111) plane and the (11-1) plane of the monoclinic system of zirconium oxide in the above X-ray diffraction pattern,
[0051] I t (111) represents the peak intensity of the (111) plane of the tetragonal zirconium oxide in the above X-ray diffraction pattern,
[0052] I c (111) represents the peak intensity of the (111) plane of the cubic crystal system of zirconium oxide in the above X-ray diffraction pattern).
[0053]
[18] The zirconia calcined body according to
[17] , wherein the f y It is less than 13%.
[0054]
[19] The zirconia calcined body according to
[17] or
[18] , wherein on a straight line extending in the first direction from one end to the other end of the zirconia calcined body,
[0055] For the layers having different yttrium oxide contents, the tendency of increase or decrease of the yttrium oxide content relative to the total molar content of zirconium oxide and yttrium oxide does not change from one end to the other end.
[0056] In the layer including the aforementioned end,
[0057] The aforementioned y More than 1%.
[0058]
[20] The zirconia calcined body according to any one of
[17] to
[19] , wherein on a straight line extending in a first direction from one end to the other end of the zirconia calcined body,
[0059] For the layers having different yttrium oxide contents, the tendency of increase or decrease of the yttrium oxide content relative to the total molar content of zirconium oxide and yttrium oxide does not change from one end to the other end.
[0060] In the layer including the aforementioned other end,
[0061] The aforementioned y It is more than 0.5%.
[0062]
[21] The zirconia calcined body according to any one of [1] to
[20] , wherein the color tone (L1 * 、a1 * 、b1 * ), and the color tone (L2* 、a2 * 、b2 * )hour,
[0063] In all layers, the color difference ΔE represented by the following formula (3) * is below 2.7,
[0064] ΔE * ={(L2 * -L1 * ) 2 +(a2 * -a1 * ) 2 +(b2 * -b1 * ) 2} 1 / 2 (3).
[0065]
[22] The zirconia calcined body according to any one of [1] to
[21] , wherein, regarding the two layers having substantially the same content of the stabilizer in a sintered body produced by sintering the zirconia calcined body at an appropriate sintering temperature for 15 minutes, when comparing the color tone (L3 * 、a3 * 、b3 * ) and the hue of layer 2 (L4 * 、a4 * 、b4 * )hour,
[0066] The color difference ΔE2 between the hue of the first layer and the hue of the second layer is expressed by the following formula (4): * is 0.3 or more and 6.0 or less,
[0067] ΔE2 * ={(L4 * -L3 * ) 2 +(a4 * -a3 * ) 2 +(b4 * -b3 * ) 2} 1 / 2 (4)
[0068] (Wherein, hue (L3 * 、a3 * 、b3 * ) represents the color tone of the first layer with approximately the same content of the stabilizer, and the color tone (L4 * 、a4 * 、b4 * ) represents the color tone of the second layer having approximately the same content of the stabilizer).
[0069]
[23] A method for producing a calcined zirconium oxide body according to any one of [1] to
[22] , wherein the calcined zirconium oxide formed from a raw material powder comprising zirconium oxide particles whose main crystal system of zirconium oxide is monoclinic and a stabilizer is calcined at 800°C to 1200°C.
[0070]
[24] A method for producing a zirconia sintered body, comprising sintering the zirconia calcined body according to any one of [1] to
[22] at a maximum sintering temperature of 1400°C to 1650°C.
[0071]
[25] The method for producing a zirconia sintered body according to
[24] , wherein the holding time at the maximum sintering temperature is less than 120 minutes.
[0072]
[26] A method for producing a dental product, comprising cutting the zirconium oxide calcined body according to any one of [1] to
[22] and then sintering it.
[0073]
[27] The method for manufacturing a dental product according to
[26] , wherein the cutting process is cutting process using a CAD / CAM system.
[0074] Effects of the Invention
[0075] According to the present invention, it is possible to provide a zirconia calcined body which has a color tone, light transmittance and strength suitable for dental use (especially use in dental hospitals) even if it is calcined for a short time. According to the present invention, it is particularly possible to provide a zirconia calcined body which can be visually identified as having the same light transmittance and color tone as natural teeth and has a gradual decrease in light transmittance even if it is calcined for a short time. In addition, according to the present invention, it is possible to provide a zirconia calcined body which has a small difference in calcination shrinkage even if it is calcined for a short time, and can produce a dental prosthesis without deformation and cracks. It should be noted that in this specification, "difference in calcination shrinkage" refers to the difference in shrinkage between layers after calcination as described in the examples described later. "Short-time calcination" means that the holding time at an appropriate calcination temperature is less than 30 minutes, and may also be less than 25 minutes, less than 20 minutes, or less than 15 minutes. BRIEF DESCRIPTION OF THE DRAWINGS
[0076] Figure 1 is a schematic diagram of a zirconia sintered body.
[0077] Figure 2 This is a photograph of the appearance of a zirconia sintered body, which is related to the determination of an appropriate sintering temperature.
[0078] Figure 3A This is a schematic diagram of a sample for measuring firing shrinkage.
[0079] Figure 3B is a schematic diagram of a zirconia sintered body.
[0080] Figure 4 This is an X-ray diffraction diagram of the calcined body produced in the first layer of Example 1.
[0081] Figure 5 This is an X-ray diffraction pattern of the calcined body produced in the first layer of Comparative Example 3. DETAILED DESCRIPTION
[0082] The zirconia calcined body of the present invention is characterized in that it has a stacked structure of at least three layers containing zirconium oxide and a stabilizer capable of inhibiting phase transformation of zirconium oxide, the main crystal system of zirconium oxide is a monoclinic system, the stacked structure has at least two layers with different mol contents of the stabilizer relative to the total mol of zirconium oxide and the stabilizer (hereinafter also referred to as "layers with different mol contents of the stabilizer"), the stacked structure has at least two layers with approximately the same mol content of the stabilizer relative to the total mol of the zirconium oxide and the stabilizer (hereinafter also referred to as "layers with approximately the same content of the stabilizer"), and all layers with approximately the same content of the stabilizer contain a coloring component, and the compositions of the coloring components in the layers are different from each other.
[0083] The zirconia calcined body of the present invention is described. The zirconia calcined body can be a precursor (intermediate product) of a zirconia sintered body. In the present invention, the zirconia calcined body may refer to a substance obtained by agglomerating zirconia particles (powder) in an incompletely sintered state. The density of the zirconia calcined body is preferably 2.7 g / cm 3 In addition, the density of the calcined zirconium oxide is preferably 4.0 g / cm 3 Below, more preferably 3.8 g / cm 3 Below, more preferably 3.6 g / cm 3 If it is within this density range, processing can be easily performed. It should be noted that in this specification, the upper limit and lower limit of the numerical range (the content of each component, the value calculated by each component, and each physical property, etc.) can be appropriately combined.
[0084] The calcined zirconium oxide of the present invention has a laminated structure of at least three layers, each layer containing zirconium oxide and a stabilizer capable of inhibiting the phase transformation of zirconium oxide. The stabilizer is preferably capable of forming partially stabilized zirconium oxide. Examples of the stabilizer include calcium oxide (CaO), magnesium oxide (MgO), yttrium oxide, cerium oxide (CeO2), scandium oxide (Sc2O3), niobium oxide (Nb2O5), lanthanum oxide (La2O3), erbium oxide (Er2O3), praseodymium oxide (Pr6O3), and tantalum oxide (T). 11), samarium oxide (Sm2O3), europium oxide (Eu2O3) and thulium oxide (Tm2O3), preferably yttrium oxide. The content of the stabilizer in the zirconium oxide calcined body and its sintered body of the present invention can be measured by, for example, inductively coupled plasma (ICP; Inductively Coupled Plasma) emission spectrometry, fluorescent X-ray analysis, etc. In the zirconium oxide calcined body and its sintered body of the present invention, the content of the stabilizer is preferably 0.1 to 18 mol%, more preferably 1 to 15 mol%, and further preferably 1.5 to 10 mol% relative to the total mol of zirconium oxide and the stabilizer.
[0085] From the viewpoint of achieving a color tone, light transmittance and strength suitable for dental use (especially use in dental hospitals) by firing in a short time, and reducing the difference in firing shrinkage, the main crystal system of zirconium oxide in the zirconium oxide calcined body of the present invention needs to be a monoclinic system. In addition, from the viewpoint of obtaining suitable light transmittance, the main crystal system of zirconium oxide in the zirconium oxide calcined body of the present invention is also preferably a monoclinic system. In the present invention, "the main crystal system is a monoclinic system" means that the proportion of the monoclinic system in zirconium oxide calculated by the following formula (2) relative to the total amount of all crystal systems (monoclinic system, tetragonal system and cubic system) in zirconium oxide is f m In the calcined zirconium oxide of the present invention, the ratio of the monoclinic system in the zirconium oxide calculated by the following formula (2) is: m The total amount of monoclinic, tetragonal and cubic crystals is preferably 55% or more. From the viewpoint of showing a more suitable color tone and excellent strength for dental use (especially use in dental hospitals), it is more preferably 60% or more, further preferably 70% or more, further preferably 75% or more, particularly preferably 80% or more, further particularly preferably 85% or more, and most preferably 90% or more. If it is the ratio of these monoclinic crystals, suitable light transmittance can also be obtained. In addition, from the viewpoint of obtaining a suitable color tone, etc., layers with different contents of stabilizers preferably have different ratios of monoclinic crystals. The ratio of monoclinic crystals f m It can be calculated from the following formula (2) based on the peak of the X-ray diffraction (XRD) pattern using CuKα line: It is considered that the main crystal system in the calcined zirconium oxide body contributes to the increase of the shrinkage temperature and the shortening of the sintering time.
[0086] In the calcined zirconium oxide of the present invention, the peaks of the tetragonal system and the cubic system may not be substantially detected. m Set to 100%.
[0087] [Number 2]
[0088]
[0089] In equation (2), I m (111) and I m (11-1) respectively represent the peak intensities of the (111) plane and the (11-1) plane of the monoclinic system of zirconium oxide. t (111) represents the peak intensity of the (111) plane of the tetragonal system of zirconium oxide. c (111) represents the peak intensity of the (111) plane of the cubic crystal system of zirconium oxide.
[0090] In the zirconia calcined body of the present invention, from the viewpoint of achieving a color tone, light transmittance and strength suitable for dental use (especially use in dental hospitals) by sintering in a short time, and reducing the difference in sintering shrinkage, the aforementioned stabilizer is preferably present in a manner that makes at least a portion of the crystals of zirconia monoclinic. From the viewpoint of achieving a color tone, light transmittance and strength suitable for dental use (especially use in dental hospitals) by sintering in a short time, and reducing the difference in sintering shrinkage, at least a portion of the stabilizer is preferably not dissolved in zirconia. The fact that a portion of the stabilizer is not dissolved in zirconia can be confirmed by, for example, an XRD diagram. In the XRD diagram of the zirconia calcined body, when a peak derived from the stabilizer is confirmed, there is a stabilizer that is not dissolved in zirconia in the zirconia calcined body. When the entire amount of the stabilizer is dissolved, the peak derived from the stabilizer is basically not confirmed in the XRD diagram. However, depending on conditions such as the crystal state of the stabilizer, even if there is no peak of the stabilizer in the XRD diagram, the stabilizer may not be dissolved in zirconia. When the main crystal system of zirconium oxide is tetragonal and / or cubic and there is no peak of the stabilizer in the XRD diagram, it can be considered that most of the stabilizer, or substantially all of it, is solid-dissolved in the zirconium oxide. In the zirconium oxide calcined body of the present invention, the stabilizer may not be solid-dissolved in the zirconium oxide. It should be noted that in the present invention, "solid-dissolved stabilizer" means, for example, that the elements (atoms) contained in the stabilizer are solid-dissolved in the zirconium oxide.
[0091] From the viewpoint of achieving a color tone and strength suitable for dental use (particularly use in dental clinics) in the calcined zirconium oxide of the present invention, it is preferred that, on a straight line extending in a first direction from one end to the other end of the calcined zirconium oxide, for layers having different stabilizer contents, the ratio f of the monoclinic system in the zirconium oxide calculated by the above-mentioned formula (2) from the one end to the other end is m In other words, the proportion of monoclinic crystals in zirconium oxide is m Preferably, the ratio f of the monoclinic system is monotonically increased or decreased. m The increase or decrease tendency of is preferably unchanged. Figure 1 For explanation. Figure 1 On a straight line extending in the first direction Y from one end P to the other end Q of the zirconia calcined body 10, for layers with different stabilizer contents, the ratio of monoclinic crystals in zirconia is f m The increasing or decreasing tendency of zirconium oxide preferably does not change in the opposite direction. That is, the proportion of monoclinic crystals in zirconium oxide on the straight line from one end P to the other end Q is f m In order to reduce the tendency, it is preferable that the ratio f of monoclinic crystal in zirconium oxide does not exist in the layers with different contents of the stabilizer. m In a certain embodiment, in terms of the relationship with the content of the stabilizer, from the viewpoint of achieving a color tone and strength suitable for dental use (especially use in dental clinics), when the content of the stabilizer tends to decrease on a straight line from one end P to the other end Q, the ratio of the monoclinic system in the zirconium oxide on the straight line from one end P to the other end Q is m In addition, from the viewpoint of obtaining suitable light transmittance, when the content of the stabilizer on the straight line from one end P to the other end Q tends to decrease, the ratio of the monoclinic system in the zirconium oxide on the straight line from one end P to the other end Q is preferably m An increasing tendency is also preferred.
[0092] The zirconia calcined body of the present invention contains a coloring component. The coloring component is not particularly limited as long as it can color the zirconia sintered body, and examples thereof include pigments, composite pigments, and fluorescent agents.
[0093] Examples of the aforementioned pigment include oxides of at least one element selected from the group consisting of Ti, V, Cr, Mn, Fe, Co, Ni, Zn, Y, Zr, Sn, Sb, Bi, Ce, Pr, Sm, Eu, Gd, Tb and Er, preferably oxides containing at least one element selected from the group consisting of Ti, V, Cr, Mn, Fe, Co, Ni, Pr, Tb and Er. Examples of the aforementioned composite pigment include (Zr, V) O2, Fe(Fe, Cr) 2 O4, (Ni, Co, Fe)(Fe, Cr) 2 O4·ZrSiO4, (Co, Zn) Al2 O4, etc., preferably containing (Zr, V) O2. Examples of the aforementioned fluorescent agent include Y2SiO5:Ce, Y2SiO5:Tb, (Y, Gd, Eu) BO3, Y2O3:Eu, YAG:Ce, ZnGa2O4:Zn, BaMgAl 10 O 17 :Eu et al.
[0094] The calcined zirconium oxide of the present invention has at least two layers in which the content of the stabilizer relative to the total mol of the zirconium oxide and the stabilizer is different from each other. The number of layers in which the content of the stabilizer is different from each other is not particularly limited as long as it is 2 layers or more, and may be 3 layers, 4 layers, or 5 layers or more. In this specification, the content of the stabilizer (for example, the content of yttrium oxide) is "different from each other" means that the difference in the content of the stabilizer is 0.1 mol% or more, preferably 0.3 mol% or more, and more preferably 0.5 mol% or more. In addition, the difference in the content of the stabilizer is preferably 3.0 mol% or less, more preferably 2.5 mol% or less, further preferably 2.0 mol% or less, particularly preferably 1.5 mol% or less, and most preferably 1.0 mol% or less. Further, the calcined zirconium oxide of the present invention has at least two layers in which the content of the stabilizer relative to the total mol of the zirconium oxide and the stabilizer is approximately the same. The number of layers in which the content of the stabilizer is approximately the same is not particularly limited as long as it is 2 layers or more, and may be 3 layers, 4 layers, or 5 layers or more. Furthermore, all layers having approximately the same content of stabilizer contain coloring components, and the compositions of the coloring components in the layers are different from each other. The zirconia calcined body of the present invention has layers having different contents of stabilizers, and at the same time has layers having approximately the same content of stabilizers. Further, all layers having approximately the same content of stabilizers contain coloring components, and the compositions of the coloring components in the layers are different from each other, thereby reproducing the light transmittance and hue changes in the tooth neck area to be the same as those of natural teeth, and at the same time, the light transmittance changes in stages from the tooth neck to the cutting end, and the gradual change of light transmittance can also be reproduced, the light transmittance and hue of the cutting end can be reproduced, and it has appropriate strength and excellent aesthetics. From the viewpoint of excellent aesthetics, layers having different compositions of coloring components and approximately the same content of stabilizers are preferably adjacent to each other.
[0095] In this specification, the content of the stabilizer (for example, the content of yttrium oxide) is "substantially the same" means that the difference in the content of the stabilizer is less than 0.1%, preferably less than 0.05%, and more preferably less than 0.03%. In addition, "the composition of the coloring component is different" includes the case where only the type of coloring component contained in each layer is different, and also includes the case where only the content of the coloring component in each layer is different. For example, as described later, for two layers containing substantially the same content of the stabilizer in a sintered body produced by sintering a zirconium oxide pre-sintered body at an appropriate sintering temperature for 15 minutes, the color difference ΔE2 between the color tone of the first layer and the color tone of the second layer can be *The type and content of the coloring component contained in each layer are changed in a manner to achieve the desired range. It should be noted that the coloring component only needs to be contained in at least one layer of the zirconia calcined body. For example, in the suitable embodiment (X-1) described later, only one of the second layer or the third layer may contain the coloring component. The zirconia calcined body has layers with different stabilizer contents and layers with the same stabilizer content and different amounts of coloring components. For the obtained zirconia sintered body, the light transmittance, color tone, and strength required for different parts (layers) can be appropriately set with one material. The thickness of each layer is not particularly limited and can be about 0.5 mm to 3 cm.
[0096] In the zirconia calcined body of the present invention, layers with different stabilizer contents and layers with approximately the same stabilizer contents may overlap in some layers. Specific examples are given below. As a suitable embodiment (X-1), a zirconia calcined body can be cited, which has a stacked structure of 3 layers containing zirconium oxide and a stabilizer capable of inhibiting the phase transition of zirconium oxide, the main crystal system of zirconium oxide is a monoclinic system, the contents of the stabilizer in the first layer and the second layer are different from each other, and the contents of the stabilizer in the second layer and the third layer are approximately the same. As another suitable embodiment (X-2), a zirconia calcined body can be cited, which has a stacked structure of 4 layers containing zirconium oxide and a stabilizer capable of inhibiting the phase transition of zirconium oxide, the main crystal system of zirconium oxide is a monoclinic system, the contents of the stabilizer in the first layer, the second layer and the third layer are different from each other, and the contents of the stabilizer in the third layer and the fourth layer are approximately the same. In addition, as another suitable embodiment (X-3), there can be mentioned a zirconia calcined body having a 4-layer stacked structure containing zirconia and a stabilizer capable of inhibiting the phase transformation of zirconia, wherein the main crystal system of the zirconia is a monoclinic system, the contents of the stabilizer in the first layer and the second layer are different from each other, and the contents of the stabilizer in the second layer, the third layer, and the fourth layer are substantially the same. In addition, in the zirconia calcined body of the present invention, the layer having the highest content of the stabilizer is preferably a layer existing at the end surface. For example, in Figure 1On a straight line extending in the first direction Y from one end P to the other end Q of the zirconia calcined body 10, the layer including the one end P may be the layer with the highest content of the stabilizer. In a suitable embodiment, from the point of view of obtaining a color tone suitable for dental use, a zirconia calcined body can be cited, wherein the laminated structure only includes one layer with the highest content of the stabilizer. In the zirconia calcined body of the present invention, the layer with the highest content of the stabilizer may contain a coloring component. In the case where the layer with the highest content of the stabilizer contains a coloring component, the composition of the coloring component contained in the layer is preferably different from the composition of the coloring component contained in other layers. As a zirconia calcined body in which the composition of the coloring component contained in the layer with the highest content of the stabilizer is different from the composition of the coloring component contained in other layers, for example, a zirconia calcined body in which the composition of the coloring component is different from that of the coloring component contained in the layer with the highest content of the stabilizer is equivalent to a layer containing a cut end portion, and a zirconia calcined body having a different composition of the coloring component by reducing the content of the coloring component, changing the type of the coloring component, etc. compared with a layer with approximately the same content of the stabilizer can be cited. In one embodiment, when the stabilizer is yttrium oxide, the content of the stabilizer in the layer having the highest content of the stabilizer may be the content of yttrium oxide in the layer including the one end P of the zirconia calcined body 10 described later. In another embodiment, when the stabilizer is yttrium oxide, the content of the stabilizer in the layers having substantially the same content of the stabilizer may be the content of yttrium oxide in the layer including the other end Q of the zirconia calcined body 10 described later.
[0097] From the viewpoint of achieving a color tone and strength suitable for dental use, the zirconium oxide calcined body of the present invention is preferably such that, on a straight line extending in the first direction Y from one end P to the other end Q of the aforementioned zirconium oxide calcined body, while including a plurality of layers having approximately the same content of the stabilizer (suitably yttrium oxide) relative to the total mol of zirconium oxide and the stabilizer from the aforementioned one end to the other end, the overall increase or decrease tendency does not change. In other words, it is preferred that the content of the stabilizer (suitably yttrium oxide) increases or decreases monotonically. Furthermore, from the viewpoint of obtaining suitable light transmittance, it is also preferred that, on a straight line extending in the first direction Y from one end P to the other end Q of the aforementioned zirconium oxide calcined body, while including a plurality of layers having approximately the same content of the stabilizer (suitably yttrium oxide) from the aforementioned one end to the other end, the overall increase or decrease tendency does not change. Below, as a schematic diagram of a zirconium oxide calcined body, use Figure 1 For explanation. Figure 1 The increasing tendency or decreasing tendency of the content of the stabilizer preferably does not change in the opposite direction on a straight line extending in the first direction Y from one end P to the other end Q of the zirconia calcined body 10. That is, when the content of the stabilizer tends to decrease on the straight line from the one end P to the other end Q, it is preferred that there is no interval in which the content of the stabilizer substantially increases while including a plurality of layers having substantially the same content of the stabilizer (preferably yttrium oxide).
[0098] From the viewpoint of the strength and light transmittance of the zirconium oxide sintered body produced from the zirconium oxide calcined body of the present invention, the stabilizer is preferably yttrium oxide. Figure 1 The content of yttrium oxide in the layer including one end P of the zirconium oxide calcined body 10 is preferably 3.5 mol% or more, more preferably 3.7 mol% or more, further preferably 3.8 mol% or more, particularly preferably 4.0 mol% or more, and preferably 6.5 mol% or less, more preferably 6.0 mol% or less, further preferably 5.8 mol% or less, particularly preferably 5.5 mol% or less, relative to the total mol of zirconium oxide and yttrium oxide. When the content of yttrium oxide in the layer is 3.5 mol% or more and 6.5 mol% or less, the light transmittance of the zirconium oxide sintered body can be improved, and light transmittance suitable for the cutting end portion of a dental prosthesis can be obtained. In addition, the content of yttrium oxide in the layer including the other end Q of the zirconium oxide calcined body 10 is preferably 2.5 mol% or more, more preferably 3.0 mol% or more, further preferably 3.3 mol% or more, particularly preferably 3.5 mol% or more, relative to the total mol of zirconium oxide and yttrium oxide, and is preferably less than 4.5 mol%, more preferably 4.2 mol% or less, further preferably 4.1 mol% or less, and particularly preferably 4.0 mol% or less. When the content of yttrium oxide in the above-mentioned layer is 2.5 mol% or more and less than 4.5 mol%, the strength of the zirconium oxide sintered body can be improved, and the strength suitable for the tooth neck portion as a dental prosthesis can be obtained. Furthermore, when the content of yttrium oxide is 2.5 mol% or more and less than 4.5 mol%, the light transmittance is not too high, and the light transmittance suitable for the tooth neck portion as a dental prosthesis can be obtained. It should be noted that the zirconia calcined body of the present invention includes at least one layer having a yttrium oxide content different from that of the layer having one end P or the layer having the other end q as an intermediate layer between the layer having one end P and the layer having the other end Q. As a result, the light transmittance changes in stages between the tooth neck and the cutting end, and the same light transmittance as that of a natural tooth can be obtained. In addition, the zirconia calcined body of the present invention is preferably such that, on a straight line extending in the first direction from one end to the other end of the zirconia calcined body, for the layers having different yttrium oxide contents, the tendency of the increase or decrease of the yttrium oxide content relative to the total mol of zirconium oxide and yttrium oxide does not change from the one end to the other end, and the yttrium oxide content of each of the layers is within the respective specified ranges.
[0099] The difference in the content of yttrium oxide between the layer including one end P and the layer including the other end Q of the zirconia calcined body 10 is preferably 3.0 mol% or less, more preferably 2.5 mol% or less, and further preferably 2.0 mol% or less, relative to the total mol of zirconium oxide and yttrium oxide. In addition, the difference in the content of yttrium oxide is preferably 0.3 mol% or more, more preferably 0.5 mol% or more, and further preferably 1.0 mol% or more. When the difference in the content of yttrium oxide between the layer including one end P and the layer including the other end Q of the zirconia calcined body 10 is 3.0 mol% or less, the difference in light transmittance between the cutting end portion and the tooth neck portion of the dental prosthesis produced from the zirconia calcined body 10 will not be too large, and light transmittance suitable for the dental prosthesis can be obtained. Furthermore, when the difference in the content of yttrium oxide is 3.0 mol% or less, the difference in the firing shrinkage between the layer containing one end P and the layer containing the other end Q can be set to within 0.3%, and when a dental prosthesis is made from the zirconia calcined body 10, the occurrence of cracks and deformation can be prevented. In one embodiment, the zirconia calcined body of the present invention includes at least one layer having a different content of yttrium oxide from the content of either the layer containing one end P or the layer containing the other end Q as an intermediate layer between the layer containing one end P and the layer containing the other end Q. The difference in the content of yttrium oxide between the intermediate layer and the layer having a different content of yttrium oxide from the intermediate layer (for example, the layer containing one end P or the layer containing the other end Q) is preferably 2.0 mol% or less, more preferably 1.5 mol% or less, and further preferably 1.0 mol% or less. In addition, the difference in the content of yttrium oxide is preferably 0.1 mol% or more, more preferably 0.3 mol% or more, and more preferably 0.5 mol% or more.
[0100] In the calcined zirconium oxide body of the present invention, the existence ratio of yttrium oxide that is not dissolved in zirconium oxide (hereinafter sometimes referred to as "undissolved yttrium oxide") is y It can be calculated based on the following formula (1).
[0101] [Number 3]
[0102]
[0103] In equation (1), I y (111) represents the peak intensity of the (111) plane of yttrium oxide at around 2θ=29° in the XRD pattern using CuKα line. m (111) and I m (11-1) represents the peak intensity of the (111) plane and the (11-1) plane of the monoclinic system of zirconium oxide. t (111) represents the peak intensity of the (111) plane of the tetragonal system of zirconium oxide. c(111) represents the peak intensity of the (111) plane of the cubic crystal system of zirconium oxide.
[0104] The existence ratio of undissolved yttrium oxide in the calcined zirconium oxide of the present invention is f y From the viewpoint of showing a color tone, light transmittance, and excellent strength that are more suitable for dental use (especially use in dental hospitals) by firing in a short time, it is preferably greater than 0%, more preferably 1% or more, and further preferably 2% or more. y The upper limit of γ may be, for example, 13% or less, and preferably depends on the content of yttria in the zirconia calcined body. Figure 1 In the layer containing P at one end of the zirconia calcined body 10, that is, the layer having an yttria content of 3.5 mol% or more and 6.5 mol% or less, f y It can be set to 13% or less. Figure 1 In the layer including the other end Q of the zirconia calcined body 10, that is, the layer having an yttrium oxide content of 2.5 mol% or more and less than 4.5 mol%, f y It can be set to 7% or less. Figure 1 In the layer containing P at one end of the zirconia calcined body 10, that is, the layer having an yttria content of 3.5 mol% or more and 6.5 mol% or less, f y It is preferably 1% or more, more preferably 2% or more, and even more preferably 3% or more. Figure 1 In the layer including the other end Q of the zirconia calcined body 10, that is, the layer having an yttrium oxide content of 2.5 mol% or more and less than 4.5 mol%, f y It is preferably 0.5% or more, more preferably 1% or more, and even more preferably 2% or more.
[0105] It should be noted that the above formula (1) can be obtained by replacing I y (111) Substituting other peaks can be applied to calculate the non-solid solution existence rate of stabilizers other than yttrium oxide.
[0106] From the viewpoint of achieving a color tone, light transmittance and strength suitable for dental use (particularly use in dental clinics) by sintering in a short time, the zirconia calcined body of the present invention preferably has a ratio f of undissolved yttrium oxide in the zirconia calcined body calculated by the above formula (1) from one end to the other end for layers having different yttrium oxide contents on a straight line extending in a first direction from one end to the other end of the zirconia calcined body. y In other words, for layers with different yttrium oxide contents, it is preferred that the yttrium oxide content increases or decreases monotonically, and the existence rate of undissolved yttrium oxide in the zirconia calcined body is f y The following is a schematic diagram of a zirconia calcined body using Figure 1For explanation. Figure 1 On a straight line extending in the first direction Y from one end P to the other end Q of the zirconia calcined body 10, for layers having different yttrium oxide contents, the existence rate f of undissolved yttrium oxide in the zirconia calcined body is y The increasing tendency or decreasing tendency of yttrium oxide in the calcined zirconium oxide preferably does not change in the opposite direction. That is, on the straight line from one end P to the other end Q, for layers with different yttrium oxide contents, as the yttrium oxide content increases or decreases monotonically, the existence rate f of undissolved yttrium oxide in the calcined zirconium oxide is y In order to reduce the tendency, it is preferred that the existence ratio f of the undissolved yttrium oxide in the calcined zirconium oxide is not y In one embodiment, in terms of the relationship with the content of the stabilizer, from the viewpoint of achieving a color tone, light transmittance and strength suitable for dental use (especially use in dental clinics) by sintering in a short time, the existence rate of undissolved yttrium oxide in the zirconia calcined body is f , with respect to layers having different yttrium oxide contents on a straight line from one end P to the other end Q. y In order to reduce the tendency, it is preferred that the ratio of the monoclinic system in zirconium oxide on the straight line from one end P to the other end Q is m To increase the tendency.
[0107] Above, use Figure 1 , but in the present invention, for example, when the zirconia calcined body and its sintered body have a crown shape, the above-mentioned "one end" and "the other end" preferably refer to a point on the end of the cutting end side and a point on the end of the root side (tooth neck side). This point may be a point on the end surface or a point on the cross section.
[0108] When the zirconia calcined body has a disk shape or a hexahedral shape such as a rectangular parallelepiped, the above-mentioned "one end" and "the other end" preferably refer to a point on the upper and lower surfaces (bottom surfaces). The point may be a point on the end surface or a point on the cross section.
[0109] It should be noted that in the present invention, "the first direction from one end to the other end" refers to the direction in which the content of yttrium oxide changes. For example, the first direction preferably refers to the direction in which the powder is stacked in the manufacturing method described later. For example, when the zirconia calcined body has a crown shape, the first direction is preferably a direction connecting the cutting end side and the tooth neck side.
[0110] The zirconia calcined body of the present invention preferably has a bending strength of 15 MPa or more to ensure strength for machining. In addition, the zirconia calcined body preferably has a bending strength of 70 MPa or less, more preferably 60 MPa or less, to facilitate machining.
[0111] The bending strength can be measured in accordance with ISO 6872:2015, and only the size of the test piece is changed, and a test piece of 5mm×10mm×50mm is used for measurement. The surface and C surface of the test piece are surface-finished in the length direction with 600# sandpaper. The test piece is arranged in a manner that the widest surface faces the vertical direction (load direction). In the bending test measurement, the span is set to 30mm and the crosshead speed is set to 0.5mm / min.
[0112] The calcined zirconium oxide of the present invention may contain additives other than zirconium oxide, stabilizers and coloring components as long as the effects of the present invention are achieved. In addition, the layer with the highest content of the stabilizer may contain a coloring component or may not contain it. Examples of such additives include aluminum oxide (Al2O3), titanium oxide (TiO2), silicon dioxide (SiO2), and the like.
[0113] The zirconia calcined body of the present invention can be made by sintering (i.e., calcining) a zirconia molded body formed by a raw powder containing zirconia particles, a stabilizer, and a coloring component at a temperature at which the zirconia particles do not reach sintering (pre-calcining step). The layer with the highest content of the stabilizer may contain a coloring component or may not contain it. The zirconia molded body is not particularly limited, and can be manufactured using a raw powder containing zirconia particles and a stabilizer using a known method (such as press molding, etc.). As the zirconia particles contained in the aforementioned raw powder, zirconia particles (powder) whose main crystal system of zirconia is a monoclinic system can be used. Zirconia particles whose main crystal system of zirconia is a monoclinic system can use commercial products. The manufacturing method of the aforementioned raw powder is not particularly limited, and the method described in, for example, International Publication No. 2018 / 056330 can be used. Specifically, monoclinic zirconia and yttrium oxide are combined to make a mixture. It should be noted that the monoclinic zirconia and yttrium oxide are made in separate steps. Next, the mixture is added to water to prepare a slurry, and the mixture is wet-milled and mixed with a ball mill to a predetermined average particle size (e.g., an average particle size of 0.13 μm) (primary milling step). Next, the milled slurry is dried with a spray dryer, and the resulting powder is calcined at 950°C for 2 hours (calcining step). Next, the calcined powder is added to water to prepare a slurry, and the mixture is wet-milled with a ball mill to a predetermined average particle size (e.g., an average particle size of 0.13 μm) or less (secondary milling step). After adding a binder to the milled slurry, the raw material powder as a composition can be prepared by drying it with a spray dryer. The calcination temperature (calcination temperature) in the calcination step is preferably 800°C or more, more preferably 900°C or more, and further preferably 950°C or more in order to ensure agglomeration. In addition, the calcination temperature is preferably 1200°C or less, more preferably 1150°C or less, and further preferably 1100°C or less in order to improve dimensional accuracy. That is, the method for producing the zirconia calcined body of the present invention is preferably 800° C. to 1200° C. At such a sintering temperature, it is considered that the solid solution of the stabilizer does not proceed in the sintering step.
[0114] The zirconia calcined body of the present invention may be a molded body having a predetermined shape. For example, the zirconia calcined body may have a disk (circular plate) shape, a rectangular parallelepiped shape, or a dental product shape (e.g., a crown shape). Dental products (e.g., crown-shaped prostheses) obtained by processing the calcined zirconia disk using a CAD / CAM (Computer-Aided Design / Computer-Aided Manufacturing) system are also included in the calcined body.
[0115] Regarding color tone, the zirconia calcined body of the present invention can produce a sintered body having a suitable color tone even if it is sintered for a short time. The sintered body produced by sintering the zirconia calcined body of the present invention at an appropriate sintering temperature for a certain time is recorded as the first sintered body. In addition, the sintered body produced by sintering the zirconia calcined body of the present invention at an appropriate sintering temperature for 120 minutes is recorded as the second sintered body. The sintering time of the first sintered body is set to 15 minutes, and the color tone (L1 * 、a1 * 、b1 * ) and the color tone of the second sintered body (L2 * 、a2 * 、b2 * ), in all layers, the color difference ΔE shown in the following formula (3) * It is preferably 2.7 or less, more preferably 2.0 or less, further preferably 1.6 or less, and particularly preferably 0.8 or less.
[0116] ΔE * ={(L2 * -L1 * ) 2 +(a2 * -a1 * ) 2 +(b2 * -b1 * ) 2} 1 / 2 (3).
[0117] In addition, the details of the appropriate firing temperature, color tone, and color tone difference in the present invention, such as an evaluation method, will be described in the examples described later.
[0118] As described above, in the zirconia calcined body of the present invention, the laminated structure has at least two layers having substantially the same content of the stabilizer. In other words, the laminated structure has at least the first layer and the second layer having substantially the same content of the stabilizer. In one embodiment, the color tone (L3) of the first layer is compared with the color tone (L4) of the second layer, which is included in the two layers having substantially the same content of the stabilizer in the sintered body produced by calcining the zirconia calcined body at an appropriate calcination temperature for 15 minutes. * 、a3 * 、b3 * ) and the hue of layer 2 (L4 * 、a4 * 、b4 * ), the color difference ΔE2 between the hue of the first layer and the hue of the second layer is shown in the following formula (4): * From the viewpoint of reproducing the color tone change of the tooth neck region of a natural tooth in a sintered body, it is preferably 0.3 or more, more preferably 0.4 or more, and even more preferably 0.5 or more.* It is preferably 6.0 or less, more preferably 5.0 or less, further preferably 4.5 or less, and particularly preferably 4.0 or less.
[0119] ΔE2 * ={(L4 * -L3 * ) 2 +(a4 * -a3 * ) 2 +(b4 * -b3 * ) 2} 1 / 2 (4)
[0120] (Wherein, hue (L3 * 、a3 * 、b3 * ) represents the color tone of the first layer with approximately the same content of the stabilizer, and the color tone (L4 * 、a4 * 、b4 * ) represents the color tone of the second layer having approximately the same content of the stabilizer).
[0121] In another embodiment, from the viewpoint of reproducing the color change of the neck region of a natural tooth in the sintered body, for all layers having substantially the same content of the stabilizer, the color difference ΔE2 between adjacent layers is preferably * In the aforementioned range.
[0122] In the calcined zirconium oxide of the present invention, the laminated structure has at least two layers having substantially the same content of the stabilizer relative to the total molar content of the zirconium oxide and the stabilizer, all the layers having substantially the same content of the stabilizer contain a coloring component, and the compositions of the coloring components in the layers are different from each other, and in addition, the main crystal system of the zirconium oxide contained in each layer is a monoclinic system, thereby, even though there are layers having substantially the same content of the stabilizer, the color difference ΔE2 between the layers having substantially the same content of the stabilizer in the sintered zirconium oxide can be reduced by calcining in a short time. * Set to the aforementioned range. Since there are at least two layers with different stabilizer contents, in addition, since there is a color difference in the sintered body required to reproduce the color tone change of the neck area of the natural tooth, the obtained zirconium oxide sintered body has the same light transmittance and color tone as natural teeth as a whole, and can form a gradient in which the light transmittance gradually decreases. In the prior art such as Patent Documents 1 and 2, the yttrium oxide content of each layer in the block or blank is completely different. In addition, for example, in the embodiment (paragraph 0123) of Patent Document 1, it is recorded that it is distinguished from the monoclinic zirconium oxide on the market, but it is not taught that the main crystal system of the zirconium oxide contained in each layer is the monoclinic system, and it is not used, so such an effect cannot be achieved.
[0123] The zirconia sintered body of the present invention is described. In the present invention, the zirconia sintered body refers to a substance in which, for example, zirconia particles (powder) are sintered. In particular, the zirconia sintered body of the present invention refers to a substance made from the zirconia calcined body of the present invention. The relative density of the zirconia sintered body is preferably 99.5% or more. The relative density can be calculated as a ratio of the measured density measured by the Archimedean method to the theoretical density.
[0124] The zirconia sintered body of the present invention includes not only a sintered body obtained by sintering molded zirconia particles under normal pressure or without pressure, but also a sintered body densified by a high temperature pressurization treatment such as HIP (Hot Isostatic Pressing) treatment.
[0125] The content of zirconium oxide and stabilizer in the zirconium oxide sintered body of the present invention is the same as that in the pre-sintered body before the sintered body is produced. Regarding the crystal system of zirconium oxide in the zirconium oxide sintered body, the proportion of monoclinic system is m It is preferably 10% or less, more preferably 5% or less, and even more preferably substantially free (0%). The crystal system other than the monoclinic system is a tetragonal system and / or a cubic system.
[0126] Regarding the proportion of the stabilizer dissolved in the zirconia sintered body of the present invention, preferably 95% or more of the stabilizer is dissolved in the zirconia, and more preferably substantially all of the stabilizer is dissolved. y It is preferably 5% or less, more preferably 1% or less, and even more preferably substantially all dissolved (0%). It is to be noted that the stabilizer (eg, yttrium oxide) is considered to be dissolved in zirconium oxide in the sintering step described later.
[0127] The method for producing a zirconia sintered body of the present invention is described as follows. The zirconia sintered body of the present invention can be produced by sintering a zirconia calcined body at a temperature at which the zirconia particles reach sintering (sintering step). The sintering temperature in the sintering step is, for example, preferably above 1400°C, and more preferably above 1450°C. In addition, the sintering temperature is, for example, preferably below 1650°C, and more preferably below 1600°C. The heating rate and the cooling rate are preferably below 300°C / minute. That is, as a method for producing a zirconia sintered body of the present invention, it is preferred that the zirconia calcined body be sintered at a maximum sintering temperature of 1400°C to 1650°C. The appropriate sintering temperature of the zirconia calcined body can be set to the aforementioned maximum sintering temperature.
[0128] In the sintering step, the holding time at the sinterable temperature (e.g., the maximum sintering temperature) is preferably less than 120 minutes, more preferably less than 90 minutes, further preferably less than 75 minutes, further preferably less than 60 minutes, particularly preferably less than 45 minutes, and most preferably less than 30 minutes. Further, it can also be set to less than 25 minutes, less than 20 minutes, or less than 15 minutes. In addition, the holding time is preferably more than 1 minute, more preferably more than 5 minutes, and more preferably more than 10 minutes. According to the zirconia calcined body of the present invention, even with such a short sintering time, the change in the color tone of the produced zirconia sintered body can be suppressed. In addition, by shortening the sintering time, while improving production efficiency, energy costs can be reduced.
[0129] The heating rate and cooling rate in the sintering step are preferably set to shorten the time required for the sintering step. For example, the heating rate can be set to reach the maximum sintering temperature in the shortest time according to the performance of the sintering furnace. The heating rate to the maximum sintering temperature can be set, for example, at least 10°C / minute, at least 50°C / minute, at least 100°C / minute, at least 120°C / minute, at least 150°C / minute, or at least 200°C / minute. The cooling rate is preferably set to a rate that does not cause defects such as cracks in the sintered body. For example, after the heating is completed, the sintered body can be left to cool at room temperature. The maximum sintering temperature refers to the highest temperature reached in the sintering step.
[0130] The zirconium oxide sintered body obtained by sintering the zirconium oxide calcined body of the present invention can be suitable for dental products. As dental products, for example, inner crowns (copings), frameworks (frameworks), crowns (crowns), crown bridges (crown bridges), abutments (abutments), implants (implants), implant screws (implantscrews), implant fixtures (implant fixtures), implant bridges (implant bridges), implant bars (implant bars), braces (brackets), denture beds (denture bases), inlays (inlays), onlays (onlays), correction wires (orthodontic wires), veneers (laminate veneers) etc. can be cited. In addition, as its manufacturing method, appropriate method can be selected according to each purpose, for example, by sintering after the zirconium oxide calcined body of the present invention is cut, dental products can be obtained. It should be noted that CAD / CAM system is preferably used in this cutting process.
[0131] The present invention includes various combinations of the above-described configurations within the scope of the technical concept of the present invention as long as the effects of the present invention are achieved.
[0132] Example
[0133] The present invention is further described below with reference to examples. However, the present invention is not limited to these examples, and a person skilled in the art can make various modifications within the scope of the technical concept of the present invention.
[0134] [Production of calcined zirconia body]
[0135] The zirconia calcined bodies of the examples and comparative examples were produced by the following process.
[0136] The method for preparing the raw material powder used to prepare the calcined zirconium oxide bodies of Examples 1 to 3 and Comparative Examples 1 and 2 is described. First, a mixture is prepared using monoclinic zirconium oxide powder and yttrium oxide powder in a manner to achieve the composition described in Table 1. Next, the mixture is added to water to prepare a slurry, and the mixture is wet-ground and mixed using a ball mill until the average particle size is less than 0.13 μm. The ground slurry is dried using a spray dryer, and the resulting powder is calcined at 950° C. for 2 hours to prepare a powder (primary powder). It should be noted that the above-mentioned average particle size can be obtained by a laser diffraction scattering method. Specifically, the laser diffraction scattering method can be measured, for example, using a laser diffraction particle size distribution measuring device (SALD-2300: manufactured by Shimadzu Corporation) using a 0.2% sodium hexametaphosphate aqueous solution as a dispersion medium.
[0137] A coloring component was added to the obtained primary powder according to the composition described in Table 1. Thereafter, the powder to which the coloring component was added was added to water to prepare a slurry, and wet-milled and mixed with a ball mill until the average particle size reached 0.13 μm or less. After adding a binder to the milled slurry, the slurry was dried with a spray dryer to prepare a powder (secondary powder). The prepared secondary powder was prepared as a raw material powder and used for the production of the zirconia calcined body described later.
[0138] As raw material powders for producing the zirconia calcined body according to Comparative Example 3, Zpex (registered trademark) Smile manufactured by Tosoh Corporation was used for the first layer, and Zpex (registered trademark) manufactured by Tosoh Corporation was used for the second and third layers.
[0139] Next, the method for producing the zirconia calcined body is described. First, the raw material powders are filled in a mold with an inner size of 20 mm×25 mm in the order described in Table 1, and the mold is pressed by a uniaxial pressing machine at a surface pressure of 300 kg / cm 2 The first press molding was performed for 90 seconds. The obtained first press molded body was subjected to a pressure of 1700 kg / cm 2CIP molding was performed for 5 minutes to produce a molded body having a laminated structure. It should be noted that in Example 3 having a 4-layer laminated structure, the filling amount of each layer was 7.5 g, and in Examples 1, 2 and Comparative Examples 1 to 3 having a 3-layer laminated structure, the filling amount of each layer was 10 g. The obtained molded body was sintered at 1000° C. for 2 hours to produce a zirconia calcined body.
[0140] [Definition and determination of appropriate sintering temperature of zirconia calcined body]
[0141] In the present invention, the appropriate firing temperature of the zirconia calcined body refers to the firing temperature specified by the manufacturer when commercially available zirconia is used. On the other hand, in the absence of information on a specifically specified firing temperature, it can be specified as follows. First, the zirconia calcined body is fired at various temperatures for 120 minutes, and then both sides are ground with #600 grinding paper to obtain a sample of zirconia sintered body with a thickness of 0.5 mm. The appearance of the obtained sample is visually observed, and based on the transparency of the sample, the appropriate firing temperature of each zirconia calcined body is determined according to the following criteria. Figure 2 The state that the zirconia calcined body is high in transparency and can be seen through the background, as in the sample on the left of FIG. Figure 2 The state of low transparency or turbidity, such as the sample on the right side of the figure, can be judged as insufficient sintering. Figure 2 The lowest temperature that can be considered to be fully fired as the sample on the left side of is judged as the appropriate firing temperature of the zirconia calcined body. It should be noted that the appropriate firing temperature of the layer with the highest yttria content in the zirconia calcined body is the appropriate firing temperature of the zirconia calcined body.
[0142] As a result of the above-mentioned measurement, the appropriate firing temperature of the zirconia calcined body used in each example and comparative example was 1500°C in Example 1, and 1550°C in Examples 2 and 3 and Comparative Examples 1 and 2. On the other hand, in Comparative Example 3 using Zpex (registered trademark) and Zpex (registered trademark) Smile manufactured by Tosoh Corporation, the firing temperature specified by the manufacturer was 1450°C.
[0143] [Measurement of Difference in Firing Shrinkage]
[0144] A zirconia sintered body was produced by the following method using the zirconia calcined bodies of the examples and comparative examples, and the difference in firing shrinkage between the layer including the one end P and the layer including the other end Q was evaluated.
[0145] First, if Figure 3AAs shown in FIG. 1 , a rectangular parallelepiped zirconia calcined body 20 having a cross section of 8 mm×10 mm and being long in the stacking direction was cut out from the zirconia calcined bodies of the examples and comparative examples produced by the aforementioned method, and the lengths of the long side WP and the short side LP of the layer including one end P and the long side WQ and the short side LQ of the layer including the other end Q were measured.
[0146] Next, the cut zirconia calcined body 20 is calcined at an appropriate calcination temperature for 120 minutes or 15 minutes to produce a zirconia sintered body. The heating rate and the cooling rate are the same for both the 120-minute and 15-minute calcinations.
[0147] In the obtained sintered body, the lengths of the long side WP and the short side LP of the layer including one end P and the long side WQ and the short side LQ of the layer including the other end Q were also measured, and the difference in firing shrinkage was calculated by the following formula (n=3). The average value of the calculated values is shown in Table 1 as the evaluation result. It should be noted that the difference in firing shrinkage is expressed as an absolute value.
[0148] [Number 4]
[0149]
[0150]
[0151] (Difference in firing shrinkage) = |(Shrinkage of the layer including one end P) - (Shrinkage of the layer including the other end Q) |
[0152] (Examples 1 to 3 and Comparative Examples 1 to 3)
[0153] As shown in Table 1, the result is that the difference in firing shrinkage between Examples 1 to 3 and Comparative Examples 1 and 2 is within 0.3%, and by using this zirconia calcined body, a dental prosthesis without deformation and cracks can be produced. It should be noted that in Examples 1 and 2 and Comparative Examples 1 and 2, the difference in firing shrinkage described in Table 1 represents the value of the difference in firing shrinkage between the first layer and the third layer, and the difference in firing shrinkage between the first layer and the second layer, and the difference in firing shrinkage between the second layer and the third layer, are also within 0.3%. In addition, in Example 3, the difference in firing shrinkage described in Table 1 represents the value of the difference in firing shrinkage between the first layer and the fourth layer, and the difference in firing shrinkage between the first layer and the second layer, the difference in firing shrinkage between the second layer and the third layer, and the difference in firing shrinkage between the third layer and the fourth layer are also within 0.3%. On the other hand, the result showed that the difference in the firing shrinkage ratio at the time of firing for 15 minutes in Comparative Example 3 was much larger than 0.3%. The calcined zirconium oxide body was greatly deformed during firing and could not be used as a dental prosthesis.
[0154] [Table 1]
[0155]
[0156] [Evaluation of aesthetic properties of zirconia sintered body]
[0157] The zirconia calcined bodies of the embodiments and comparative examples were used to prepare zirconia sintered bodies by the following method, and the aesthetic properties were visually evaluated from the perspective of comparison with the appearance of natural teeth. In the evaluation, a commercially available color scale having an appearance equivalent to that of natural teeth can be used. Specifically, the commercially available color scale can include, for example, the color scale VITA Classical (trade name) manufactured by VITA Corporation.
[0158] First, the zirconia calcined body 10 of the embodiment and the comparative example produced by the aforementioned method is cut into a crown shape using a CAD / CAM system ("KATANA (registered trademark) CAD / CAM system", Kuraray Noritake Dental Inc.). The cut zirconia calcined body obtained is fired at an appropriate firing temperature for 120 minutes or 15 minutes to produce a zirconia sintered body. It should be noted that the heating rate and the cooling rate are set to the same conditions under both the 120-minute firing and the 15-minute firing conditions. In addition, the length of the zirconia sintered body in the stacking direction is about 8 mm. The obtained zirconia sintered body is visually evaluated according to the following criteria (n=1). The results are shown in Table 2.
[0159] <Evaluation Criteria>
[0160] ○: Both the 120-minute firing and the 15-minute firing had the same light transmittance and color tone as natural teeth, and a gradual decrease in light transmittance was observed.
[0161] Δ: After only 120 minutes of firing, the light transmittance and color tone are the same as those of natural teeth, and a gradual decrease in light transmittance is observed.
[0162] ×: Gradual change in which light transmittance gradually decreases was not observed in both the 120-minute firing and the 15-minute firing.
[0163] (Examples 1 to 3 and Comparative Examples 1 to 3)
[0164] In Examples 1 to 3, any of the zirconia sintered bodies is obtained from Figure 1The light transmittance of the zirconia calcined body 10 shown gradually decreases from the region corresponding to the layer including one end P to the region corresponding to the layer including the other end Q, forming a gradient with a darker color tone, and the light transmittance and color tone change in the tooth neck region and the light transmittance and color tone of the cutting end can be reproduced, showing the same appearance as a natural tooth. In addition, with respect to the holding time at the appropriate firing temperature when firing the zirconia calcined body, it was confirmed that there was no significant difference in the light transmittance and color tone of the sintered body under either the conditions of 120 minutes and 15 minutes, and a dental prosthesis with appropriate light transmittance and color tone can be produced even with a short firing time.
[0165] On the other hand, in Comparative Example 1 corresponding to Patent Document 3, Figure 1 In the zirconia calcined body 10 shown, the color tone tends to darken from the region corresponding to the layer including one end P to the region corresponding to the layer including the other end Q. However, since the content of yttrium oxide is the same in all layers, the change in light transmittance under the conditions of 120 minutes and 15 minutes is not sufficient, and it cannot be said that the appearance is the same as that of a natural tooth. Figure 1 The zirconium oxide calcined body 10 shown has a gradual change in light transmittance from the region corresponding to the layer including one end P to the region corresponding to the layer including the other end Q, but since the content of yttrium oxide and the amount of coloring components change simultaneously, the light transmittance and color change of the tooth neck region cannot be achieved at the same time under either the conditions of 120 minutes or 15 minutes, and cannot be said to be the same as natural teeth. In addition, the result of Comparative Example 3 is that the light transmittance when the holding time at the appropriate firing temperature is set to 120 minutes is significantly reduced, and the light transmittance of the case where the holding time is set to 15 minutes cannot be exhibited by firing for a short time, and a dental prosthesis having the same light transmittance as natural teeth cannot be produced.
[0166] [Evaluation of color tone of zirconia sintered body]
[0167] Regarding the color tone of each layer of the zirconia sintered body of each example and comparative example, a separate zirconia sintered body of each layer was prepared by the following method, and the color tone (L*a*b* colorimetric system (JIS Z 8781-4: 2013 Colorimetry - Part 4: CIE1976 L*a*b* color space) was measured. * , a * , b * ). In addition, the sintered bodies fired for 120 minutes and 15 minutes were calculated. * , a * , b * ) obtained by * , confirm the difference in color tone.
[0168] First, the size is adjusted in advance and compression molding is performed in such a manner that both sides of the obtained zirconia sintered body are subjected to #600 grinding processing to obtain a zirconia sintered body with a thickness of 1.2 mm, thereby producing a molded body containing raw material powder in each layer of each embodiment and comparative example. Next, the molded body is sintered at 1000°C for 2 hours to produce a zirconia pre-calcined body. Next, the zirconia pre-calcined body is sintered for 120 minutes or 15 minutes at an appropriate sintering temperature to produce a zirconia sintered body. After both sides of the obtained zirconia sintered body are subjected to #600 grinding processing to obtain a zirconia sintered body with a thickness of 1.2 mm, the color tone is measured using a spectrophotometer CM-3610A manufactured by Konica Minolta Inc. with D65 light source, measurement mode SCI, measurement diameter / illumination diameter = φ8mm / φ11mm, and white background. Color difference ΔE * The color tone of the zirconia sintered body (L2 * 、a2 * 、b2 * ), and the color tone of the zirconia sintered body when fired for 15 minutes (L1 * 、a1 * 、b1 * ), and was determined by the following formula (n=3). Table 2 shows the average value of the calculated results.
[0169] ΔE * ={(L2 * -L1 * ) 2 +(a2 * -a1 * ) 2 +(b2 * -b1 * ) 2} 1 / 2 (3).
[0170] Color difference ΔE * From the viewpoint of suitability as a dental product, it is preferably 2.7 or less, more preferably 2.0 or less, further preferably 1.6 or less, and particularly preferably 0.8 or less.
[0171] In addition, the color tone (L1 * 、a1 * 、b1 * ) were measured, and the color difference ΔE2 between the second layer and the third layer of Examples 1 and 2 and Comparative Examples 1 to 3, and between the third layer and the fourth layer of Example 3 was calculated by the following formula (4): * .
[0172] ΔE2 * ={(L4* -L3 * ) 2 +(a4 * -a3 * ) 2 +(b4 * -b3 * ) 2} 1 / 2 (4)
[0173] (Wherein, hue (L3 * 、a3 * 、b3 * ) represents the color tone of the first layer (the second layer of Examples 1 and 2 and Comparative Examples 1 to 3, and the third layer of Example 3) having substantially the same content of the stabilizer, and the color tone (L4 * 、a4 * 、b4 * ) represents the color tone of the second layer (the third layer of Examples 1 and 2 and Comparative Examples 1 to 3, and the fourth layer of Example 3) having substantially the same content of the stabilizer)
[0174] The result calculated from the color tone values shown in Table 2 is that ΔE2 * The values were 3.15, 2.85, and 3.70 in Examples 1 to 3, respectively. In Examples 1 to 3, the color tone change in the tooth neck region was reproduced, and the reason why the color tone was the same as that of natural teeth was visually confirmed even when the cutting end was fired for a short time.
[0175] According to Table 2, in each layer of the zirconia sintered bodies of Examples 1 to 3 and Comparative Examples 1 and 2, there is no significant difference in the color tone when the holding time at the appropriate sintering temperature is 120 minutes and when the holding time is 15 minutes. The color difference ΔE * On the other hand, in each layer of Comparative Example 3, the color tone when the holding time at the appropriate firing temperature was 120 minutes was significantly different from that when the holding time was 15 minutes, and the color difference ΔE * 3 or more.
[0176] [Table 2]
[0177]
[0178] [Measurement of flexural strength of zirconia sintered body]
[0179] (Example 3)
[0180] Using the raw material powder in the fourth layer of Example 3, a zirconia calcined body was prepared according to the manufacturing method of the calcined body described above, and then calcined under the conditions described below to obtain a zirconia sintered body. According to ISO6872, the bending strength was measured under the conditions of sample size 1.2mm×4.0mm×16.0mm, fulcrum distance (span length) 12mm, and crosshead speed 0.5mm / min. The result was 1170MPa when the holding time at the maximum sintering temperature was 120 minutes, and 1120MPa when the holding time at the maximum sintering temperature was 15 minutes. The holding time at the maximum sintering temperature was either 120 minutes or 15 minutes, and it was confirmed that it had the strength necessary for the tooth neck as a dental prosthesis. It should be noted that, as shown in Table 2, for the aesthetics (translucency, color tone) of Example 3, it is suitable as a dental prosthesis when the holding time at the maximum sintering temperature is either 120 minutes or 15 minutes. That is, it was confirmed that both the aesthetic properties and the strength suitable as a dental prosthesis were achieved.
[0181] (Example 1)
[0182] Using the raw material powder in the third layer of Example 1, a zirconia sintered body was obtained in the same manner as in Example 3. Using this zirconia sintered body, the bending strength was measured in the same manner as in Example 3. The result was 1310 MPa when the holding time at the maximum sintering temperature was 120 minutes, and 1298 MPa when the holding time at the maximum sintering temperature was 15 minutes.
[0183] (Example 2)
[0184] Similarly, using the raw material powder in the third layer of Example 2, a zirconia sintered body was obtained in the same manner as in Example 3. Using this zirconia sintered body, the bending strength was measured in the same manner as in Example 3. The result was 1157 MPa when the holding time at the maximum sintering temperature was 120 minutes, and 1139 MPa when the holding time at the maximum sintering temperature was 15 minutes.
[0185] [XRD measurement of calcined zirconia body]
[0186] The crystal system of zirconium oxide and the extent to which the stabilizer was not dissolved in zirconium oxide were confirmed.
[0187] (Examples 1 to 3 and Comparative Examples 1 to 3)
[0188] The zirconia calcined bodies in the respective layers of Examples 1 to 3 and Comparative Examples 1 to 3 were measured by XRD patterns using CuKα radiation, and f was calculated. y and f m The results are shown in Tables 1 and 2. Figure 4 , an XRD pattern of the zirconia calcined body of the first layer of Example 1 is shown. Figure 5 , an XRD pattern of the zirconia calcined body produced in the first layer of Comparative Example 3 is shown.
[0189] like Figure 5 As shown in FIG. 1 , in the zirconium oxide calcined body in the first layer of Comparative Example 3, no peak of monoclinic zirconium oxide was confirmed. In addition, no peak of yttrium oxide was confirmed. The second layer of Comparative Example 3 also showed the same result. On the other hand, according to Figure 4 In the zirconia calcined body of the second layer of Example 1, peaks of monoclinic, tetragonal and cubic zirconia were confirmed, and the peak of the monoclinic system was higher in intensity. The other examples also had the same results. In addition, in any of the zirconia calcined bodies of the examples, a peak of yttrium oxide was confirmed near 2θ of 29.4° ( Figure 4 Peak No. 6 in FIG. 1 ), it can be considered that in each zirconia calcined body, part of yttrium oxide was not dissolved in zirconia.
[0190] The numerical range described in the present specification should be construed as if any numerical value or range included in the range is specifically described in the present specification even if not otherwise described.
[0191] Industrial Applicability
[0192] The zirconia calcined body and the sintered body thereof of the present invention can be used for dental products such as prostheses.
[0193] Description of Reference Numerals
[0194] 10 Zirconia sintered body
[0195] P end
[0196] Q The other end
[0197] L Total length
[0198] Y 1st direction
[0199] 20 Sample for determination of firing shrinkage (zirconia calcined body)
[0200] WP is the long side of the layer containing one end P.
[0201] LP The short side of the layer containing one end P
[0202] WQ The long side of the layer containing the other end Q
[0203] LQ The short side of the layer containing the other end Q
Claims
1. A calcined zirconium oxide body having a laminated structure of at least three layers containing zirconium oxide and a stabilizer capable of inhibiting phase transformation of zirconium oxide, The main crystal system of zirconium oxide is monoclinic system. The laminated structure has at least two layers having different contents of the stabilizer relative to the total molar content of zirconium oxide and the stabilizer. The laminated structure has at least two layers having substantially the same content ratio of the stabilizer relative to the total molar content of zirconium oxide and the stabilizer. All layers having substantially the same content of the stabilizer contain a coloring component, and the compositions of the coloring components in the layers are different from each other. The different contents of the stabilizers mean that the difference in the contents of the stabilizers is 0.1 mol % or more. The term “the content of the stabilizer is substantially the same” means that the difference in the content of the stabilizer is less than 0.1 mol %.
2. The zirconium oxide calcined body according to claim 1, wherein Layers having substantially the same content of the stabilizer are adjacent to each other.
3. The zirconium oxide calcined body according to claim 1 or 2, wherein: The coloring component includes an oxide of at least one element selected from Ti, V, Cr, Mn, Fe, Co, Ni, Pr, Tb and Er, or (Zr, V)O2.
4. The zirconium oxide calcined body according to claim 1 or 2, wherein 55% or more of the zirconium oxide is monoclinic.
5. The zirconium oxide calcined body according to claim 1 or 2, wherein 75% or more of the zirconium oxide is monoclinic.
6. The zirconium oxide calcined body according to claim 1 or 2, wherein: The layers having different contents of the stabilizer have different ratios of monoclinic crystals.
7. The zirconium oxide calcined body according to claim 1 or 2, wherein: The laminated structure includes only one layer having the highest content of the stabilizer.
8. The zirconium oxide calcined body according to claim 1 or 2, wherein: The layer having the highest content of the stabilizer does not contain any coloring component.
9. The zirconium oxide calcined body according to claim 1 or 2, wherein: The layer having the highest content of the stabilizer contains a coloring component.
10. The zirconium oxide calcined body according to claim 9, wherein The composition of the coloring component contained in the layer having the highest content of the stabilizer is different from the composition of the coloring component in the other layers.
11. The zirconium oxide calcined body according to claim 1 or 2, wherein: At least a part of the stabilizer is not dissolved in zirconium oxide.
12. The zirconium oxide calcined body according to claim 1 or 2, wherein: On a straight line extending in a first direction from one end to the other end of the zirconia calcined body, In the layers having different contents of the stabilizer, the increasing and decreasing tendency of the content of the stabilizer relative to the total molar amount of zirconium oxide and the stabilizer does not change from one end to the other end.
13. The zirconium oxide calcined body according to claim 1 or 2, wherein: The aforementioned stabilizer is yttrium oxide.
14. The zirconium oxide calcined body according to claim 13, wherein On a straight line extending in a first direction from one end to the other end of the zirconia calcined body, For the layers having different yttrium oxide contents, the increasing and decreasing tendency of the content of the stabilizer relative to the total molar amount of zirconium oxide and the stabilizer does not change from one end to the other end. With respect to the total mol of the aforementioned zirconium oxide and the aforementioned yttrium oxide, The yttrium oxide content of the layer including the one end is 3.5 mol% or more and 6.5 mol% or less, The yttrium oxide content of the layer including the other end is 2.5 mol % or more and less than 4.5 mol %.
15. The zirconium oxide calcined body according to claim 14, wherein On a straight line extending in a first direction from one end to the other end of the zirconia calcined body, For the layers having different yttrium oxide contents, the increasing and decreasing tendency of the content of the stabilizer relative to the total molar amount of zirconium oxide and the stabilizer does not change from one end to the other end. With respect to the total mol of the aforementioned zirconium oxide and the aforementioned yttrium oxide, The difference in yttrium oxide content between the layer including the one end and the layer including the other end is 3.0 mol % or less.
16. The zirconium oxide calcined body according to claim 13, wherein The X-ray diffraction pattern shows a peak of yttrium oxide.
17. The zirconium oxide calcined body according to claim 13, wherein f calculated based on the following formula (1) y Greater than 0%, Among them, I y (111) represents the peak intensity of the (111) plane of yttrium oxide at around 2θ=29° in the X-ray diffraction pattern using CuKα line, I m (111) and I m (11-1) represents the peak intensity of the (111) plane and the (11-1) plane of the monoclinic system of zirconium oxide in the above X-ray diffraction pattern, I t (111) represents the peak intensity of the (111) plane of the tetragonal zirconium oxide in the above X-ray diffraction pattern, I c (111) represents the peak intensity of the (111) plane of the cubic crystal system of zirconium oxide in the above X-ray diffraction pattern.
18. The zirconium oxide calcined body according to claim 17, wherein The aforementioned y It is less than 13%.
19. The zirconium oxide calcined body according to claim 17, wherein On a straight line extending in a first direction from one end to the other end of the zirconia calcined body, For the layers having different yttrium oxide contents, the tendency of increase or decrease of the yttrium oxide content relative to the total molar content of zirconium oxide and yttrium oxide does not change from one end to the other end. In the layer including the aforementioned end, The aforementioned y More than 1%.
20. The zirconium oxide calcined body according to claim 17, wherein On a straight line extending in a first direction from one end to the other end of the zirconia calcined body, For the layers having different yttrium oxide contents, the tendency of increase or decrease of the yttrium oxide content relative to the total molar content of zirconium oxide and yttrium oxide does not change from one end to the other end. In the layer including the aforementioned other end, The aforementioned y It is more than 0.5%.
21. The zirconium oxide calcined body according to claim 1 or 2, wherein: In comparison with the color tone (L1 * 、a1 * 、b1 * ), and the color tone (L2 * 、a2 * 、b2 * )hour, In all layers, the color difference ΔE represented by the following formula (3) * is below 2.7, <h2 style=";text-align:left;direction:ltr">ΔE<h2 style=";text-align:left;direction:ltr"> * <h2 style=";text-align:left;direction:ltr"> (L2<h2 style=";text-align:left;direction:ltr"> * <h2 style=";text-align:left;direction:ltr"> -L1<h2 style=";text-align:left;direction:ltr"> * <h2 style=";text-align:left;direction:ltr"> )<h2 style=";text-align:left;direction:ltr"> 2 <h2 style=";text-align:left;direction:ltr"> +(a2<h2 style=";text-align:left;direction:ltr"> * <h2 style=";text-align:left;direction:ltr"> -a1<h2 style=";text-align:left;direction:ltr"> * <h2 style=";text-align:left;direction:ltr"> )<h2 style=";text-align:left;direction:ltr"> 2 <h2 style=";text-align:left;direction:ltr"> +(b2<h2 style=";text-align:left;direction:ltr"> * <h2 style=";text-align:left;direction:ltr"> -b1<h2 style=";text-align:left;direction:ltr"> * <h2 style=";text-align:left;direction:ltr"> )<h2 style=";text-align:left;direction:ltr"> 2 <h2 style=";text-align:left;direction:ltr">}<h2 style=";text-align:left;direction:ltr"> 1 / 2 <h2 style=";text-align:left;direction:ltr"> (3) 22. The zirconium oxide calcined body according to claim 1 or 2, wherein: Regarding the two layers having substantially the same content of the stabilizer in the sintered body produced by sintering the zirconia calcined body at an appropriate sintering temperature for 15 minutes, when comparing the color tone (L3 * 、a3 * 、b3 * ) and the hue of layer 2 (L4 * 、a4 * 、b4 * )hour, The color difference ΔE2 between the hue of the first layer and the hue of the second layer is expressed by the following formula (4): * is 0.3 or more and 6.0 or less, ΔE2 * ={(L4 * -L3 * ) 2 +(a4 * -a3 * ) 2 +(b4 * -b3 * ) 2 } 1 / 2 (4) Where, hue (L3 * 、a3 * 、b3 * ) represents the color tone of the first layer with approximately the same content of the stabilizer, and the color tone (L4 * 、a4 * 、b4 * ) represents the color tone of the second layer having approximately the same content of the stabilizer.
23. The method for producing a zirconia calcined body according to any one of claims 1 to 22, wherein A zirconia molded body formed of raw material powder containing zirconia particles whose main crystal system of zirconia is monoclinic and a stabilizer is pre-fired at 800°C to 1200°C.
24. A method for producing a zirconia sintered body, wherein: The zirconium oxide calcined body according to any one of claims 1 to 22 is calcined at a maximum calcination temperature of 1400°C to 1650°C.
25. The method for producing a zirconia sintered body according to claim 24, wherein: The holding time at the maximum firing temperature is less than 120 minutes.
26. A method for producing a dental product, wherein: The zirconium oxide calcined body according to any one of claims 1 to 22 is subjected to cutting and then sintered.
27. The method for manufacturing a dental product according to claim 26, wherein: The aforementioned cutting process is cutting process using a CAD / CAM system.