A composite material of perovskite and molecular sieve and its preparation method and application
Through the simultaneous coating method of molecular sieve etching and perovskite limited growth, the problem of poor stability of perovskite materials in humidity and atmospheric environments has been solved, efficient composite material preparation has been achieved, and the stability and spectrum of the materials have been improved. Characteristics, suitable for optoelectronic devices, simplifying the process flow and suitable for mass production.
Patent Information
- Application Number
- CN202111075210.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-09-14
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2041-09-14
AI Technical Summary
Perovskite materials have poor stability in humidity and atmospheric environments. The preparation process is complex and difficult to produce on a large scale. The existing protective layer cannot completely isolate water and oxygen, resulting in insufficient material stability.
A one-step method is adopted to achieve the preparation of perovskite and molecular sieve composite materials through a simultaneous coating method of molecular sieve etching and perovskite localized growth, and a high-temperature solid-phase synthesis method to avoid the use of organic solvents. The porous structure of the molecular sieve is used for calcium synthesis. Fixation and encapsulation of titanium.
It improves the environmental and thermal stability of perovskite composite materials, achieves efficient load capacity increase and spectrum control, is suitable for electroluminescence and photoluminescence fields, simplifies the preparation process, reduces equipment requirements, and is suitable for large-scale production.
Smart Images

Figure CN115806814B_ABST
Abstract
Description
Technical field:
[0001] The present invention belongs to the field of inorganic luminescent materials, and specifically relates to a composite material of perovskite and molecular sieve and a preparation method thereof Background technology:
[0002] Inorganic perovskite (CsPbX3) is an excellent optoelectronic material with advantages such as narrow half-width of fluorescence spectrum, high quantum efficiency, and broadband adjustable emission wavelength. In recent years, it has been widely used in optoelectronic devices such as solar cells and light-emitting diodes and has attracted more and more attention. However, perovskite materials have poor stability and are extremely sensitive to external environments such as organic solvents, humidity, air, and thermal ultraviolet. In addition, the current preparation process of perovskite materials is relatively complicated and difficult to prepare on a large scale in industrial production, which limits the development of perovskite materials.
[0003] So far, various methods have been developed to improve CsPbX3 to solve the problem of perovskite stability, including surface passivation, doping, and coating with inorganic or organic protective layers. Among them, coating is considered to be the most effective and direct method. The protective layer can isolate CsPbX3 from water and oxygen, and can also prevent ion migration and fusion between particles. Commonly used shell materials include inorganic oxides (SiO2, Al2O3, TiO2, etc.), mesoporous materials (MOF, molecular sieves, etc.), organic polymer materials (polyethylene, epoxy resin, polymethyl methacrylate, etc.), and inorganic salts (NaNO3, NH4Br). However, these protective layers can only slow down the degradation rate of CsPbX3 by external environmental factors, and cannot completely protect CsPbX3. For example, the pore structure is exposed to the outside and cannot completely isolate perovskite and water oxygen. Inorganic oxides are not dense enough at lower annealing temperatures and have higher permeability to external water and oxygen, but higher temperatures will damage and strip organic ligands, leading to agglomeration and fluorescence quenching.
[0004] Molecular sieves are a large class of inorganic porous materials that form a three-dimensional network structure through the combination of shared oxygen atoms. Due to their high porosity, large specific surface area, easy adsorption and ion exchange, they can be used as excellent carriers of luminescent materials. Chinese invention CN106701070B discloses a blue-yellow-orange light perovskite quantum dot and molecular sieve composite luminescent material and its preparation method and application. First, the molecular sieve is mixed with cesium halide for ion exchange to obtain a Cs-exchanged molecular sieve, and then octadecene, oleylamine, oleic acid, and lead halide are used as raw materials to prepare a polyhalogen lead halide solution. Octadecene is added to the Cs-exchanged molecular sieve, and after heating and stirring for a period of time under a nitrogen atmosphere, a polyhalogen lead halide solution sub-sieve is added. After washing and drying, a perovskite quantum dot and molecular sieve composite luminescent material is obtained, and its fluorescence lifetime and stability are significantly increased. Similarly, Chinese invention CN107384387B discloses a manganese-doped CsPbBr3 perovskite quantum dot and molecular sieve composite luminescent material and its preparation method and application. By introducing Y-type molecular sieve as a carrier of quantum dots, the environmental stability is significantly increased. However, the preparation methods of the above patents are all liquid phase synthesis methods, which are relatively cumbersome and require operation under N2 atmosphere, and organic ligands need to be added. Post-processing is also required to obtain the corresponding powder material, which is not conducive to large-scale application and stability improvement. Summary of the invention:
[0005] Purpose of the invention: In view of the problems existing in the prior art, the purpose of the present invention is to introduce a porous material such as molecular sieve as a substrate, to achieve the preparation and compounding of perovskite by a one-step method, to achieve a unique process and structure of molecular sieve etching, perovskite confined growth and synchronous coating, to solve the problems of poor stability and uneven size of perovskite in humidity and atmospheric environment. Another purpose of the present invention is to provide a method for preparing a composite phosphor that is simple to operate, has low equipment requirements, and can be produced in large quantities. This method avoids the use of organic solvents, is simple to operate, and has good repeatability, providing a new idea for the subsequent large-scale industrial application of optoelectronic devices.
[0006] To achieve the above object, the present invention provides the following technical solutions:
[0007] One aspect of the present invention provides a method for preparing a composite material of perovskite and molecular sieve, the preparation method comprising the following steps:
[0008] Step 1: Add lead source and cesium source into the reaction vessel.
[0009] Alternatively, a lead source, a cesium source and a first halogen source are added to a reaction vessel;
[0010] Step 2, evenly dispersing the molecular sieve in the reaction container;
[0011] Step 3, placing the crucible in a muffle furnace for high temperature treatment, with the reaction temperature being above 500° C. until the reaction is complete;
[0012] Step 4: After cooling to room temperature, a composite material of perovskite and molecular sieve can be obtained.
[0013] In some specific technical schemes of the present invention, the method for preparing the composite material of perovskite and molecular sieve also includes step five, annealing the obtained composite material of perovskite and molecular sieve with a second halogen source to obtain a composite material of perovskite and molecular sieve substituted with the halogen in the halogen source; the melting point of the second halogen source is not higher than 350°C.
[0014] The halogen in the composite material of perovskite and molecular sieve obtained in step 4 is not completely the same as the halogen type in the halogen source in step 5.
[0015] In some technical solutions of the present invention, the temperature of the annealing treatment is 150-350°C, for example, 200°C, 250°C, 300°C.
[0016] In some technical schemes of the present invention, the melting point of the second halogen source is 0-350°C, for example, 10°C, 20°C, 30°C, 40°C, 50°C, 60°C, 70°C, 80°C, 90°C, 100°C, 150°C, 200°C, 250°C, 300°C.
[0017] Another aspect of the present invention provides a composite material of perovskite and molecular sieve, wherein the composite material of perovskite and molecular sieve is prepared by the above method of the present invention.
[0018] In one aspect, the present invention provides a composite material of perovskite and molecular sieve, which has a unique structure of molecular sieve etching, perovskite confined growth and molecular sieve coated perovskite. Under certain conditions, halogen ion exchange can be further performed.
[0019] In the technical solution of the present invention, the lead source, cesium source and halogen source in step 1 are not dissolved and do not contain any solvent.
[0020] In the technical solution of the present invention, in steps 1 to 4, no solvent or solution is used.
[0021] The composite material of perovskite and molecular sieve, the amount of perovskite loaded by the molecular sieve can be regulated according to the degree of etching, and the loaded perovskite accounts for 0.1-30% of the total weight ratio, preferably 1-20%, for example 1%, 2%, 3%, 4%, 5%, 6%, 7%, 8%, 9%, 10%, 11%, 12%, 13%, 14%, 15%, 16%, 17%, 18%, 19%, 20%, 25%, 30%.
[0022] The lead source is one or more of halogen-containing lead salts, lead carbonate, lead nitrate, lead sulfate, lead acetate and organic lead salts, and the halogen-containing lead salt is selected from lead chloride, lead bromide or lead iodide.
[0023] The cesium source is one or more of cesium salts containing halogen, cesium carbonate, cesium nitrate, cesium sulfate, cesium acetate and organic cesium salts, and the cesium salt containing halogen is selected from cesium chloride, cesium bromide or cesium iodide.
[0024] The first halogen source is one or more of ammonium halide and organic halide. The ammonium halide is selected from ammonium chloride, ammonium bromide or ammonium iodide; the organic halide is selected from tetrabutylammonium bromide, tetrabutylammonium chloride, tetraethylammonium chloride, benzyltriethylammonium chloride, trioctylmethylammonium chloride, dodecyltrimethylammonium chloride, octaalkyltrimethylammonium bromide, and dodecyltrimethylammonium bromide.
[0025] In the step 1, the molar ratio of the cesium source to the lead source is 4:1-1:4, preferably 1.2:1-1:1.2, for example 1:1.
[0026] In the step 1, the molar amount of halogen in the cesium source, the lead source and the first halogen source is more than 3 times the molar amount of cesium in the cesium source or the molar amount of lead in the lead source.
[0027] In the step 1, the cesium source and the lead source are placed in a mixed manner, stacked up and down, or separately placed at both ends of the reaction container. Further preferably, the cesium source and the lead source are placed at both ends of the reaction container and do not contact each other.
[0028] In the step 2, the weight ratio of the molecular sieve to the total mass of the lead source and the cesium source, or to the total mass of the lead source, the cesium source and the first halogen source is 1:0.1 to 1:4, for example, 1:0.3, 1:0.5, 1:0.7, 1:1, 1:5, 1:2, 1:2.5, 1:3, 1:3.5, 1:4.
[0029] In the step 2, the molecular sieve and the lead source, cesium source and the first halogen source are placed in a mixed manner, stacked up and down, or separately placed at both ends of the reaction container. Preferably, the molecular sieve is placed above the lead source, cesium source and the first halogen source.
[0030] The molecular sieve is a zeolite molecular sieve, preferably selected from a silicon-aluminum molecular sieve and a titanium-silicon molecular sieve, an aluminum phosphate molecular sieve, and an aluminum silicate molecular sieve formed by substitution and compounding.
[0031] In the step three, the heating rate is 0.5°C / min to 20°C / min, for example, 1°C, 2°C, 3°C, 4°C, 5°C, 10°C, 15°C, or 20°C.
[0032] In the step three, the reaction temperature is 500°C to 1000°C, and the insulation time is 1-24h; for example, the reaction temperature is 600°C, 700°C, 800°C, 900°C, and the insulation time is 2h, 3h, 4h, 5h, 6h, 7h, 8h, 10h, 12h, 14h, 16h, 18h, 20h, 22h, 24h.
[0033] In the step 4, the temperature is cooled to room temperature at a cooling rate of 1-10°C / min, for example, 2°C, 3°C, 4°C, 5°C, 6°C, 7°C, 8°C, or 9°C.
[0034] In the step 5, the second halogen source is preferably an organic halogen source, and the organic halide is selected from tetrabutylammonium bromide, tetrabutylammonium chloride, tetraethylammonium chloride, benzyltriethylammonium chloride, trioctylmethylammonium chloride, dodecyltrimethylammonium chloride, octaalkyltrimethylammonium bromide, and dodecyltrimethylammonium bromide.
[0035] Another aspect of the present invention provides the use of the composite material of the present invention as electroluminescence, photoluminescence, and white light LED luminescent material.
[0036] The present invention unexpectedly discovered that at a relatively high temperature, the molecular thermal motion in the reaction system forms convection, and the lead source, cesium source and halogen source will form cesium halide and lead halide vapor adsorbed into the pores of the molecular sieve. Lead bromide will first react with the molecular sieve, and by reacting with Si-OH, an intermediate product Si-PbX structure will be formed. The HX generated in this process etches the molecular sieve micropores (Si-O network structure), increasing the adsorption of the perovskite raw material, and at the same time causing the pores to collapse to form encapsulation. Furthermore, the free X - , and the intermediate product then reacts with cesium halide to form perovskite, thereby achieving efficient composite of perovskite nanocrystals and molecular sieves.
[0037] As a carrier of perovskite, molecular sieve has a unique pore structure. Due to the etching effect, even if the molecular sieve structure collapses, there are still certain pores for ion exchange reactions, which facilitates other ions to enter the molecular sieve pores and synthesize related compounds. During the high-temperature reaction process, the pores of the molecular sieve are etched and enlarged, and a large amount of perovskite raw materials are fixed, which can limit the growth size of perovskite nanocrystals and block the interaction of nanocrystals at high temperatures, reduce the concentration quenching caused by agglomeration between luminescent centers, and improve the stability of perovskite in the pores.
[0038] Beneficial effects: Compared with the prior art, the present invention has the following significant features:
[0039] 1. The etching of the molecular sieve pores realizes the large-scale adsorption and fixation of the perovskite raw materials, increases the loading capacity of the perovskite, and achieves a high-efficiency composite effect of synchronous coating and confined growth, has a good water and oxygen barrier effect, and improves the environmental stability and thermal stability of the perovskite composite material;
[0040] 2. Due to the presence of etched microchannels, the composite material can also undergo halogen ion exchange under certain conditions, which can expand its spectral range. The composite material exhibits narrow-band emission in the range of 360-700nm, with an adjustable band gap and a narrow half-peak width of about 20nm, and high luminous intensity, and can be used in lighting fields such as electroluminescence and photoluminescence;
[0041] 3. The composite material adopts high-temperature solid-phase synthesis method, which avoids the use of organic solvents and does not require the introduction of organic ligands. It is simple to operate, has good repeatability, low equipment requirements, can be produced in large quantities, and is conducive to industrial application;
[0042] 4. The perovskite and molecular sieve composite material prepared by the present invention has good application prospects in the fields of lighting display, especially white light LED.
[0043] 5. The composite material prepared by the present invention has a higher loading capacity. In the prior art, lead bromide and cesium bromide are dissolved in water to prepare the composite material. However, since lead bromide is a slightly soluble raw material, the molecular sieve loading capacity is limited. Moreover, since lead bromide is easily hydrolyzed to form a basic salt, lead bromide and cesium bromide are dissolved together, so a structure of perovskite plus crystal water is formed during the drying process, so it is necessary to add an annealing process to dehydrate the crystal water. Description of the drawings:
[0044] Figure 1 This is a white light picture of the composite material prepared in Example 1 of the present invention.
[0045] Figure 2 is a scanning electron microscope image of the composite material prepared in Example 2 of the present invention.
[0046] Figure 3 is the X-ray diffraction pattern of the composite material prepared in Example 2 of the present invention.
[0047] Figure 4 It is the luminescence spectrum diagram of the composite material prepared in Example 7 of the present invention.
[0048] Figure 5 The white light LED spectra (a) and spectra under different currents (b) prepared by combining the green light and red light composite materials prepared in Examples 1 and 14 of the present invention with a blue light chip are shown.
[0049] Figure 6The water stability (a), 80°C-80% humidity environment aging stability (b) and ultraviolet radiation stability (c) of the blue light, green light and red light composite materials in the embodiments of the present invention are shown.
[0050] Figure 7 It is the thermal stability of the blue light (a), green light (b) and red light (c) composite materials in the embodiment of the present invention.
[0051] Figure 8 This is a characterization of the reaction mechanism in the present invention, that is, when bromine and lead exist simultaneously, the binding energies of Si 2p (a) and O1s (b) orbitals in the binding energy spectrum shift greatly toward the low binding energy direction, indicating the formation of a new structure. Specific implementation method:
[0052] The present invention is further described below in conjunction with the examples, but the protection scope of the present invention should not be limited thereto. In the following examples, the raw materials are directly purchased.
[0053] Example 1 Preparation of composite materials of perovskite and molecular sieve
[0054] The following steps are involved:
[0055] Step 1, weigh 1.47 g (4 mmol) of lead bromide and 0.851 g (4 mmol) of cesium bromide respectively and add them into an alumina crucible;
[0056] Step 2, covering the raw material with 2 g of molecular sieve as a substrate;
[0057] Step 3, placing the alumina crucible containing the raw materials into a muffle furnace, heating to 650° C. for 100 min, and keeping the temperature for 5 h;
[0058] Step 4: After cooling to room temperature at 5°C / min, the perovskite and molecular sieve composite material can be obtained.
[0059] The yield of the composite luminescent material prepared in this embodiment is relatively high, the perovskite loading is about 20%, and the powder white light picture is as follows: Figure 1 As shown, it can be observed that the perovskite is uniformly embedded in the pores of the molecular sieve, forming a structure of confined growth and synchronous coating.
[0060] Example 2 Preparation of composite materials of perovskite and molecular sieve
[0061] The following steps are involved:
[0062] Step 1, weigh 1.764 g (4.8 mmol) of lead bromide and 0.851 g (4 mmol) of cesium bromide respectively, and add them into an alumina crucible;
[0063] Step 2, covering the raw material with 2.25 g of molecular sieve as a substrate;
[0064] Step 3, placing the alumina crucible containing the raw materials into a muffle furnace, heating to 650° C. at a heating rate of 75 min, and keeping the temperature for 24 h;
[0065] Step 4: After cooling to room temperature at 3°C / min, the perovskite and molecular sieve composite material can be obtained.
[0066] This example can also obtain green phosphor with high quality and yield, with a perovskite loading of about 18%. Figure 2 As shown, the XRD results of perovskite composite powder are as follows Figure 3 shown.
[0067] Example 3 Preparation of composite materials of perovskite and molecular sieve
[0068] The following steps are involved:
[0069] Step 1, weigh 5.86 g (16 mmol) of lead bromide and 0.851 g (4 mmol) of cesium bromide, respectively, and add them into an alumina crucible;
[0070] Step 2, covering the raw material with 10 g of molecular sieve as a substrate;
[0071] Step 3, placing the alumina crucible containing the raw materials into a muffle furnace, heating to 650° C. at a heating rate of 100 min, and keeping the temperature for 1 h;
[0072] Step 4: After cooling to room temperature at 10°C / min, the perovskite and molecular sieve composite material can be obtained.
[0073] In this example, the amount of lead bromide added is relatively large, and the overall output of the composite phosphor is slightly lower.
[0074] Example 4 Preparation of composite materials of perovskite and molecular sieve
[0075] The following steps are involved:
[0076] Step 1, weigh 1.47 g (4 mmol) of lead bromide and 0.6734 g (4 mmol) of cesium chloride respectively, and add them into an alumina crucible;
[0077] Step 2, covering the raw material with 2 g of molecular sieve as a substrate;
[0078] Step 3, placing the alumina crucible containing the raw materials into a muffle furnace, heating to 670° C. for 75 min, and keeping the temperature for 5 h;
[0079] Step 4: After cooling to room temperature at 8°C / min, the perovskite and molecular sieve composite material can be obtained.
[0080] This example can synthesize blue phosphor with a high yield.
[0081] Example 5 Preparation of composite materials of perovskite and molecular sieve
[0082] The following steps are involved:
[0083] Step 1: Weigh 1.112 g (4 mmol) of lead chloride, 0.6734 g (4 mmol) of cesium chloride, and 0.053 g (1 mmol) of ammonium chloride, respectively, and add them into an alumina crucible;
[0084] Step 2, covering the raw material with 2 g of molecular sieve as a substrate;
[0085] Step 3, placing the alumina crucible containing the raw materials into a muffle furnace, heating to 670° C. for 75 min, and keeping the temperature for 5 h;
[0086] Step 4: After cooling to room temperature at 2°C / min, the perovskite and molecular sieve composite material can be obtained.
[0087] This example can synthesize purple fluorescent powder with a high yield.
[0088] Example 6 Preparation of composite materials of perovskite and molecular sieve
[0089] The following steps are involved:
[0090] Step 1, weigh 1.47 g (4 mmol) of lead bromide and 0.851 g (4 mmol) of cesium bromide respectively, and add them into an alumina crucible;
[0091] Step 2, covering the raw material with 5 g of molecular sieve as a substrate;
[0092] Step 3, placing the alumina crucible containing the raw materials into a muffle furnace, heating to 500° C. for 100 min, and keeping the temperature for 5 h;
[0093] Step 4: After cooling to room temperature at 1°C / min, the perovskite and molecular sieve composite material can be obtained.
[0094] In this example, green phosphor can be synthesized, but part of the molecular sieve is not reacted and the perovskite loading is about 3%.
[0095] Example 7 Preparation of composite materials of perovskite and molecular sieve
[0096] The following steps are involved:
[0097] Step 1, weigh 1.764 g (4.8 mmol) of lead bromide and 0.851 g (4 mmol) of cesium bromide respectively, and add them into an alumina crucible;
[0098] Step 2, covering the raw material with 2.5 g of molecular sieve as a substrate;
[0099] Step 3, placing the alumina crucible containing the raw materials into a muffle furnace, heating to 650° C. for 30 min, and keeping the temperature for 5 h;
[0100] Step 4: After cooling to room temperature at 5°C / min, the perovskite and molecular sieve composite material can be obtained.
[0101] In this example, green phosphor can be synthesized. The perovskite loading is about 15%. The fluorescence emission spectrum is as follows: Figure 4 As shown, the half-peak width of the visible material is very narrow, only about 20nm, and the size is uniform.
[0102] Example 8 Preparation of composite materials of perovskite and molecular sieve
[0103] The following steps are involved:
[0104] Step 1: Weigh 1.764 g (4.8 mmol) of lead bromide, 0.851 g (4 mmol) of cesium bromide, and 0.098 g (1 mmol) of ammonium bromide, respectively, and add them into an alumina crucible;
[0105] Step 2, covering the raw material with 2.5 g of molecular sieve as a substrate;
[0106] Step 3, placing the alumina crucible containing the raw materials into a muffle furnace, heating to 670° C. for 1300 min, and keeping the temperature for 5 h;
[0107] Step 4: After cooling to room temperature at 5°C / min, the perovskite and molecular sieve composite material can be obtained.
[0108] This example can synthesize green phosphor, but there are lumps at the bottom and the yield is reduced.
[0109] Example 9 Preparation of composite materials of perovskite and molecular sieve
[0110] The following steps are involved:
[0111] Step 1, weigh 1.764 g (4.8 mmol) of lead bromide and 0.851 g (4 mmol) of cesium bromide respectively, and add them into an alumina crucible;
[0112] Step 2, covering the raw material with 2.5 g of molecular sieve as a substrate;
[0113] Step 3, placing the alumina crucible containing the raw materials into a muffle furnace, heating to 1000° C. for 300 min, and keeping the temperature for 5 h;
[0114] Step 4: After cooling to room temperature at 5°C / min, the perovskite and molecular sieve composite material can be obtained.
[0115] This example can synthesize green phosphor, and excessive perovskite loading will cause agglomeration.
[0116] Example 10 Preparation of composite materials of perovskite and molecular sieve
[0117] The following steps are involved:
[0118] Step 1, weigh 1.47 g (4 mmol) of lead bromide and 0.851 g (4 mmol) of cesium bromide respectively and add them into an alumina crucible;
[0119] Step 2, covering the raw material with 10 g of molecular sieve as a substrate;
[0120] Step 3, placing the alumina crucible containing the raw materials into a muffle furnace, heating to 650° C. for 100 min, and keeping the temperature for 15 h;
[0121] Step 4: After cooling to room temperature at 5°C / min, the perovskite and molecular sieve composite material can be obtained.
[0122] In this example, green phosphor can be synthesized, but part of the molecular sieve is not reacted and the perovskite loading is about 1%.
[0123] Example 11 Preparation of composite materials of perovskite and molecular sieve
[0124] The following steps are involved:
[0125] Step 1, weigh 1.47 g (4 mmol) of lead bromide and 0.851 g (4 mmol) of cesium bromide respectively and add them into an alumina crucible;
[0126] Step 2, covering the raw material with 1 g of molecular sieve as a substrate;
[0127] Step 3, placing the alumina crucible containing the raw materials into a muffle furnace, heating to 650° C. for 100 min, and keeping the temperature for 10 h;
[0128] Step 4: After cooling to room temperature at 5°C / min, the perovskite and molecular sieve composite material can be obtained.
[0129] This example can synthesize green phosphor, but due to the small amount of molecular sieve added, the perovskite is overloaded and agglomerates are produced.
[0130] Example 12 Preparation of composite materials of perovskite and molecular sieve
[0131] The following steps are involved:
[0132] Step 1: Weigh 1.068 g (4 mmol) of lead carbonate, 0.851 g (4 mmol) of cesium bromide, and 0.79 g (8 mmol) of ammonium bromide into an alumina crucible;
[0133] Step 2, covering the raw material with 2 g of molecular sieve as a substrate;
[0134] Step 3, placing the alumina crucible containing the raw materials into a muffle furnace, heating to 650° C. for 100 min, and keeping the temperature for 5 h;
[0135] Step 4: After cooling to room temperature at 5°C / min, the perovskite and molecular sieve composite material can be obtained.
[0136] This example can synthesize green phosphor.
[0137] Example 13 Preparation of composite materials of perovskite and molecular sieve
[0138] The following steps are involved:
[0139] Step 1: Weigh 1.5 g (4.6 mmol) of lead acetate, 0.8 g (4.2 mmol) of cesium acetate, and 3.2 g (9.9 mmol) of tetrabutylammonium bromide into an alumina crucible;
[0140] Step 2, covering the raw material with 2 g of molecular sieve as a substrate;
[0141] Step 3, placing the alumina crucible containing the raw materials into a muffle furnace, heating to 650° C. for 100 min, and keeping the temperature for 5 h;
[0142] Step 4: After cooling to room temperature at 5°C / min, the perovskite and molecular sieve composite material can be obtained.
[0143] This example can synthesize green phosphor.
[0144] Example 14 Experimental substitution of halogen species in composite materials of perovskite and molecular sieve
[0145] A mixture of excess tetrabutylammonium iodide and the composite material powder in Example 1 is added to a crucible and annealed at 300° C. to complete the substitution of iodine for bromine in the composite material, thereby changing the fluorescence of the composite material from green to red.
[0146] A mixture of excess tetraethylammonium chloride and the composite material powder of Example 1 is added to a crucible and annealed at 250° C. to complete the substitution of chlorine for bromine in the composite material, thereby changing the fluorescence of the composite material from green to blue-purple.
[0147] It can be seen from the above embodiments that the molecular sieve composite material loaded with perovskite can be prepared by a one-step method through the method of the present invention. Different lead sources, different cesium sources, and different ratios can all prepare composite materials. And by adjusting the type of halogen in the lead source, composite materials of different colors can also be obtained. And by adjusting the ratio of each component and the reaction temperature and time, a composite material loaded with more perovskite and more complete reaction can be obtained. In addition, more colorful perovskite composite materials can be formed by further ion exchange.
[0148] Embodiment 15
[0149] The spectra of the white light LED prepared by combining the green light and red light composite materials prepared in Examples 1 and 14 with the blue light chip and the spectra under different currents are respectively detected. The experimental results are shown in Figure 5 .
[0150] The water stability, aging stability in an 80°C-80% humidity environment, and UV radiation stability of the blue, green, and red light composite materials in the examples were tested respectively, as well as the thermal stability of the blue, green, and red light composite materials. Figure 6-7 , indicating that the material prepared by the present invention has high stability.
[0151] Figure 8 The binding energy spectrum of the material of the present invention is shown, which illustrates the reaction mechanism characterization of the present invention, that is, when bromine and lead exist at the same time, the binding energy of Si 2p (a) and O1s (b) orbitals in the binding energy spectrum shifts greatly toward the low binding energy direction, indicating the formation of a new structure.
[0152] The method of the present invention completely avoids the use of organic solvents and does not require the introduction of organic ligands. It is also unnecessary to add liquid solvents such as water, and the preparation is achieved under all-solid phase conditions, so the entire preparation process has only one step, the reaction method and the equipment used are very simple, and the reaction time is very short. More importantly, the pores of the molecular sieve are further etched during the preparation process of the present invention to form a coating structure, thereby improving the stability of the perovskite loaded thereon.
[0153] The above embodiments are partial implementation methods of the present invention, but the implementation methods of the present invention are not limited to the above embodiments. Any other changes, modifications, substitutions, combinations, and simplifications that do not deviate from the spirit and principles of the present invention should be equivalent replacement methods and are included in the protection scope of the present invention.
Claims
1. A method for preparing a composite material of perovskite and molecular sieve, characterized in that: The preparation method comprises the following steps: Step 1: Add lead source and cesium source into the reaction vessel. Alternatively, a lead source, a cesium source and a first halogen source are added to a reaction vessel; Step 2, evenly dispersing the molecular sieve in the reaction container; Step 3, high temperature treatment, the reaction temperature is above 500 ° C until the reaction is complete; Step 4: After cooling to room temperature, a composite material of perovskite and molecular sieve can be obtained; In steps 1 to 4, no solvent or solution is used; The lead source, cesium source and halogen source described in step 1 are not dissolved and do not contain any solvent; The method for preparing the composite material of perovskite and molecular sieve further comprises step five: Step 5, annealing the obtained composite material of perovskite and molecular sieve with a second halogen source to obtain a composite material of perovskite and molecular sieve substituted with the halogen in the halogen source; the melting point of the second halogen source is not higher than 350 ° C; wherein the halogen in the composite material of perovskite and molecular sieve obtained in step 4 is not completely the same as the halogen in the halogen source in step 5; The second halogen source is selected from at least one of tetrabutylammonium bromide, tetrabutylammonium chloride, tetraethylammonium chloride, benzyltriethylammonium chloride, trioctylmethylammonium chloride, dodecyltrimethylammonium chloride, octaalkyltrimethylammonium bromide and dodecyltrimethylammonium bromide.
2. The preparation method according to claim 1, characterized in that: The temperature of the annealing treatment in step five is 150-350°C.
3. The preparation method according to claim 1, characterized in that: The lead source is one or more of halogen-containing lead salts, lead carbonate, lead nitrate, lead sulfate, lead acetate and organic lead salts; The cesium source is one or more of cesium salts containing halogen, cesium carbonate, cesium nitrate, cesium sulfate, cesium acetate and organic cesium salts; The first halogen source is one or more of ammonium halide and organic halide.
4. The preparation method according to claim 3, characterized in that: The halogen-containing lead salt is selected from lead chloride, lead bromide or lead iodide; the halogen-containing cesium salt is selected from cesium chloride, cesium bromide or cesium iodide; the ammonium halide is selected from ammonium chloride, ammonium bromide or ammonium iodide; the organic halide is selected from tetrabutylammonium bromide, tetrabutylammonium chloride, tetraethylammonium chloride, benzyltriethylammonium chloride, trioctylmethylammonium chloride, dodecyltrimethylammonium chloride, octaalkyltrimethylammonium bromide or dodecyltrimethylammonium bromide.
5. The preparation method according to claim 1, characterized in that: In the step 1, the molar ratio of the cesium source to the lead source is 4:1-1:
4.
6. The preparation method according to claim 5, characterized in that: In the step 1, the molar ratio of the cesium source to the lead source is 1.2:1-1:1.
2.
7. The preparation method according to claim 1, characterized in that: In the step 1, the molar amount of halogen in the cesium source, the lead source and the first halogen source is more than 3 times the molar amount of cesium in the cesium source or the molar amount of lead in the lead source.
8. The preparation method according to claim 1, characterized in that: The weight ratio of the mass of the molecular sieve to the total mass of the lead source and the cesium source, or to the total mass of the lead source, the cesium source and the first halogen source is 1:0.1 to 1:
4.
9. The preparation method according to claim 1, characterized in that: The molecular sieve is a zeolite molecular sieve.
10. The preparation method according to claim 9, characterized in that: The molecular sieve is selected from silicon-aluminum molecular sieve and titanium silicon molecular sieve, aluminum phosphate molecular sieve and aluminum silicate molecular sieve formed by substitution and compounding.
11. The preparation method according to claim 1, characterized in that: In the step 3, the reaction temperature is 500°C to 1000°C, the heating rate is 0.5°C / min to 20°C / min, and the holding time is 1-24h; In the step 4, the temperature is cooled to room temperature at a cooling rate of 1-10°C / min.
Citation Information
Patent Citations
A blue-yellow-orange luminescent perovskite quantum dot and molecular sieve composite luminescent material, its preparation method and application
CN106701070B
A manganese-doped CsPbBr3 perovskite quantum dot-molecular sieve composite luminescent material, its preparation method and application
CN107384387B
Preparation method and application of cesium-lead halide perovskite quantum dot
CN110628428A