Application of conjugated olefin compounds as collectors in coal slime flotation and flotation method

By using conjugated olefin compounds as collectors in coal sludge flotation, the unique chemical structure is used to improve the adhesion ability of coal particles, the problem of insufficient harvesting capacity of medium and low-order raw coal in the existing technology is solved, and efficient precision is achieved Coal yield and combustible body recovery have economical and practical advantages.

CN115814953BActive Publication Date: 2024-11-05CHONGQING KOOPPER CHEM IND
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211558280.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-12-06
Publication Date
2024-11-05
Estimated Expiration
2042-12-06

AI Technical Summary

Technical Problem

In the existing coal slime flotation technology, fuel oil is low as a collector, and has weak collection capacity for low-order raw coal. The development of coal washing collectors is mainly focused on the modification and reuse of fuel oil, and there is a lack of effective Chemical structures as alternatives lead to obstacles to the efficient use of low-order coal.

Method used

The conjugated olefin compound is used as the collector, and the double bonds in its structure are combined with olefins, aromatic rings, and ketone groups to improve the ability of coal particles to adhere to the bubbles, thereby improving the yield of low-order raw coal. Specific process It includes grinding the dried coal slurry into an ore slurry, adding conjugated olefin compounds and foaming agents, and flotation treatment.

Benefits of technology

The yield of refined coal and combustible body recovery rate has been significantly improved. Compared with traditional fuel oil collectors, the yield of refined coal can be increased by 37.79%, and the combustible body recovery rate can be increased by 28.64%, which is low in cost and economical and practical.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115814953B_ABST
    Figure CN115814953B_ABST
Patent Text Reader

Abstract

The present invention belongs to the technical field of flotation reagents, and specifically relates to an application of a conjugated olefin compound as a collector in coal slime flotation and a flotation method. The structure of the conjugated olefin compound is #imgabs0#; wherein R and R' are alkyl, alkenyl, aromatic hydrocarbon or hydrogen atoms; X is CH 2 The flotation method comprises the following steps: grinding the dried coal slime into particles to prepare a slurry, adding the conjugated olefin compound, adding a frother after stirring, and obtaining a product after roughing and concentrating. The present invention can improve the capture capacity of low-rank raw coal, thereby improving the yield of clean coal. Compared with No. 3 aviation kerosene, the yield of clean coal of the present invention can be increased by 37.79%.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of flotation reagents, and in particular relates to an application of a conjugated olefin compound as a collector in coal slime flotation and a flotation method. Background Art

[0002] my country's fossil energy reserves are rich in coal, poor in oil and low in gas. Long-term dependence on imported crude oil and natural gas is a major hidden danger to national energy security. However, most of my country's coal is low-grade coal with high ash content and many impurities. Therefore, how to use low-grade raw coal efficiently and cleanly is a long-term issue. Coal washing is one of the indispensable processes in coal deep processing. It removes dust and waste rock through water washing, reduces ash and sulfur content, sorts raw coal grades, and improves coal utilization. In the coal washing process, the amount of pulverized coal generally accounts for 10% to 30% of the raw coal, so a lot of coal slime will be formed. Coal slime flotation is currently recognized as one of the most economical and effective sorting technologies for coal slime desulfurization and ash reduction.

[0003] At present, fuel oil (mineral oil, neutral oil) and the like are widely used as collectors in coal slime flotation, and fuel oil includes kerosene, diesel, etc. There are many fuel oil suppliers, but the safety is low, and the collection capacity for low-grade raw coal is weak. In addition, because the price of coal per ton is much lower than that of non-ferrous metals, the development of coal washing collectors has long been stuck in the selection, compounding and modification of fuel oil products, or in the research on the reuse of waste mineral oils, such as retired transformer oil and retired engine lubricating oil, and has not been expanded. However, because of the developed petrochemical industry in foreign countries, petrochemical products are high-quality and low-cost, and more importantly, the coal resources are good, most of the coal is high-grade coal, and the demand for washing is small. Therefore, only a very small number of foreign companies develop and provide coal washing collectors, and the price of foreign coal washing collectors is high and the cost performance is not strong. In summary, it is of great significance and application value to find effective chemical structures as coal washing collectors in a wider range. Summary of the invention

[0004] The present invention aims to provide an application of a conjugated olefin compound as a collector in coal slime flotation and a flotation method, in order to provide a new coal washing collector and improve the collection capacity of low-rank raw coal.

[0005] In order to achieve the above object, the scheme of the present invention is: use of a conjugated olefin compound as a collector in coal slime flotation, wherein the structure of the conjugated olefin compound is as shown in formula (I) or formula (II);

[0006]

[0007] Wherein, R and R' are alkyl, alkenyl, aromatic hydrocarbon groups or hydrogen atoms; X is a CH2 group, CH-R" or an oxygen atom, and R" in CH-R" is an alkyl, alkenyl or aromatic hydrocarbon group.

[0008] The present invention also provides a flotation method, comprising the following steps: grinding dried coal slime into particles to prepare ore pulp, adding the conjugated olefin compound, adding a frother after stirring, and obtaining a product after roughing and concentrating.

[0009] Optionally, the carbon chain length of the alkyl group is C2-C6.

[0010] Optionally, the carbon chain length of the alkenyl group is C2-C12, preferably C4-C10, and more preferably C6-C8.

[0011] Optionally, the conjugated olefin compound is 1,3-octadiene, benzophenone, α-propylstyrene or divinylbenzene.

[0012] Optionally, the conjugated olefin compound is used in an amount of 800 to 3000 g / t dry coal slime.

[0013] Optionally, the foaming agent is octanol.

[0014] Optionally, the dosage of the secondary octanol is 80-120 g / t dry coal slime.

[0015] Optionally, the concentration of the slurry is 60-100 g / L.

[0016] The working principle and beneficial effects of this scheme are as follows: the above-mentioned conjugated olefin compound contains two double bonds, one of which is selected from one of olefins and aromatic rings, and the other double bond is selected from one of olefins, aromatic rings, ketone groups and aldehyde groups. Compared with traditional fuel oil as a collector, the conjugated olefin compound in this scheme can better make the hydrophobic coal particles adhere to the bubbles when used as a collector, thereby improving the capture ability of low-rank raw coal and further increasing the yield of clean coal.

[0017] This scheme uses the above conjugated olefin compound as a collector, has good flotation effect, low cost, and is economical and practical. Moreover, compared with using No. 3 aviation kerosene as a collector, the clean coal yield of this scheme can be increased by 37.79%, and the combustible recovery rate can be increased by 28.64%. BRIEF DESCRIPTION OF THE DRAWINGS

[0018] Figure 1 The present invention provides a coal slime flotation process of a flotation method in Embodiment 1. DETAILED DESCRIPTION

[0019] The following is further described in detail through specific implementation methods:

[0020] Example 1

[0021] This embodiment provides an application of a conjugated olefin compound as a collector in coal slime flotation, wherein the conjugated olefin compound contains two double bonds, wherein one double bond is selected from one of an olefin and an aromatic ring, and the other double bond is selected from one of an olefin, an aromatic ring, and a carbonyl group in a ketone group and an aldehyde group. Specifically, the structural formula of the conjugated olefin compound is shown in formula (I) or formula (II);

[0022]

[0023] Wherein, R and R' are alkyl, alkenyl, aromatic hydrocarbon groups or hydrogen atoms; X is a CH2 group, CH-R" or an oxygen atom, and R" in CH-R" is an alkyl, alkenyl or aromatic hydrocarbon group.

[0024] The structure of the conjugated olefin compound in this embodiment is shown in formula (I), wherein R is a hydrogen atom; R' is a C4H9 group; and X is a CH2 group. That is, the conjugated olefin compound in this embodiment is 1,3-octadiene, and the structure is shown in formula (a):

[0025]

[0026] This embodiment also provides a flotation method, which uses the above conjugated olefin compound as a collector to float low-rank coal slime. The process flow is as follows: Figure 1 As shown, the specific process is as follows.

[0027] A low-rank coal slime, the total ash content and the ash content of each particle size of the low-rank coal slime are shown in Table 1, that is, the low-rank coal slime is already in powder form and no further grinding is required. If the coal slime is in a lumpy state, it is necessary to grind it by a rod mill or a grinder until there are no lumps in the powder and the particle size is less than 40 meshes. Use tap water to prepare the low-rank coal slime into a slurry, and the concentration of the slurry is 60-100g / L. In this embodiment, the concentration of the slurry is 100g / L. Add a collector (1,3-octadiene) to the slurry, and the amount of the collector is 800-3000g / t dry coal slime. In this embodiment, the amount of the collector is 1200g / t dry coal slime. After stirring for 2min, add a foaming agent, the amount of the foaming agent is 80-120g / t dry coal slime, and the foaming agent in this embodiment is 2-octanol, and the amount of 2-octanol is 100g / t dry coal slime. In addition, the flotation steps not completed in this embodiment are carried out in accordance with the steps of "GB-T 36167-2018 Coal Preparation Laboratory Step-by-Step Release Flotation Test Method".

[0028] Table 1 Particle size analysis of a low-rank coal slime

[0029] Particle size / mesh Yield / % Ash / % -40+60 16.24 27.32 -60+80 25.41 24.36 -80+120 9.61 24.14 -120+200 8.74 24.16 -200+300 4.47 27.39 -300 35.53 34.13 total 100.00 28.41

[0030] Example 2

[0031] The difference between this embodiment and embodiment 1 is that the conjugated olefin compound in this embodiment is different from the conjugated olefin compound in embodiment 1. Specifically, the structure of the conjugated olefin compound in this embodiment is shown in formula (II), wherein R is a C3H7 group; R' is a hydrogen atom; and X is a CH2 group. That is, the conjugated olefin compound in this embodiment is α-propylstyrene, and the structure is shown in formula (b):

[0032]

[0033] Example 3

[0034] The difference between this embodiment and embodiment 1 is that the conjugated olefin compound in this embodiment is different from the conjugated olefin compound in embodiment 1. Specifically, the structure of the conjugated olefin compound in this embodiment is shown in formula (II), wherein R is a hydrogen atom; R' is a C2H3 group; and X is a CH2 group. That is, the conjugated olefin compound in this embodiment is divinylbenzene, and the structure is shown in formula (c):

[0035]

[0036] Example 4

[0037] The difference between this embodiment and embodiment 1 is that the conjugated olefin compound in this embodiment is different from the conjugated olefin compound in embodiment 1. Specifically, the structure of the conjugated olefin compound in this embodiment is shown in formula (II), wherein R is a phenyl group; R' is an H atom; and X is an oxygen atom in a ketone group. That is, the conjugated olefin compound in this embodiment is benzophenone, and the structure is shown in formula (d):

[0038]

[0039] Comparative Example 1

[0040] In this comparative example, No. 3 aviation kerosene was used as the collector, and the flotation method was the same as that in Example 1.

[0041] Comparative Example 2

[0042] In this comparative example, No. 0 diesel was used as the collector, and the flotation method was the same as that in Example 1.

[0043] Test results

[0044] According to GB-T 36167-2018 Coal Preparation Laboratory Step-by-Step Release Flotation Test Method, the ash content and yield of Examples 1 to 4 and Comparative Examples 1 and 2 were calculated, and the results are shown in Table 2. As can be seen from Table 2, when the ash content is 10%, when 1,3-octadiene is used as a collector, the clean coal yield and combustible body recovery rate are higher than those when No. 3 aviation kerosene and No. 0 diesel are used as collectors, and the clean coal yield is increased by 17.0% and 12.5%, and the combustible body recovery rate is increased by 17.9% and 12.2%.

[0045] In addition, when α-propylstyrene, divinylbenzene and benzophenone are used as collectors, at various ash contents (10%, 10.5%, 11%, 11.5%, 12%), their clean coal yield and combustible recovery rate are higher than those when No. 3 aviation kerosene and No. 0 diesel are used as collectors.

[0046] The clean coal yield and combustible body recovery rate of α-propylstyrene are as high as 65.99% and 77.37% (ash content is 12%) respectively. Compared with No. 3 aviation kerosene, the clean coal yield and combustible body recovery rate can be increased by up to 22.48% and 23.41% (ash content is 10%) respectively; compared with No. 0 diesel, the clean coal yield and combustible body recovery rate can be increased by up to 23.41% and 17.45% (ash content is 10%) respectively.

[0047] The clean coal yield and combustible body recovery rate of divinylbenzene are as high as 67.45% and 78.91% (ash content is 12%) respectively. Compared with No. 3 aviation kerosene, the clean coal yield and combustible body recovery rate can be increased by up to 34.44% and 27.51% (ash content is 10%) respectively; compared with No. 0 diesel, the clean coal yield and combustible body recovery rate can be increased by up to 29.06% and 21.36% (ash content is 10%) respectively.

[0048] The clean coal yield and combustible body recovery rate of benzophenone are as high as 68.99% and 79.53% (ash content is 12%), respectively. Compared with No. 3 aviation kerosene, the clean coal yield and combustible body recovery rate can be increased by up to 37.79% and 28.64% (ash content is 10%), respectively; compared with No. 0 diesel, the clean coal yield and combustible body recovery rate can be increased by up to 32.27% and 22.43% (ash content is 10%), respectively.

[0049] In summary, the conjugated olefin compound provided by the present invention can be used as a collector in coal slime flotation, and improves the clean coal yield and combustible recovery rate of coal slime flotation. It is economical and practical, and has important significance and application value in the field of coal washing collectors.

[0050] Table 2 Floatability results of low-rank coal slime using various collectors

[0051]

[0052]

[0053] The above are only embodiments of the present invention. The invention is not limited to the fields involved in this implementation case. The common sense such as the known specific structures and characteristics in the scheme is not described in detail here. The ordinary technicians in the relevant field know all the common technical knowledge in the technical field to which the invention belongs before the application date or priority date, can obtain all the existing technologies in the field, and have the ability to apply the conventional experimental means before that date. The ordinary technicians in the relevant field can improve and implement this scheme in combination with their own abilities under the enlightenment given by this application. Some typical known structures or known methods should not become obstacles for ordinary technicians in the relevant field to implement this application. It should be pointed out that for those skilled in the art, without departing from the structure of the present invention, several deformations and improvements can be made, which should also be regarded as the protection scope of the present invention, which will not affect the effect of the implementation of the present invention and the practicality of the present invention. The protection scope required by this application shall be based on the content of its claims, and the specific implementation methods and other records in the specification can be used to explain the content of the claims.

Claims

1. Application of conjugated olefin compounds as collectors in coal slime flotation, Features: The conjugated olefin compound contains a conjugated double bond, and the conjugated olefin compound is 1,3-octadiene, benzophenone, α-propylstyrene or divinylbenzene.

2. A flotation method, Features: The following steps are involved: The dried coal sludge is ground into particles to prepare ore slurry, the conjugated olefin compound as claimed in claim 1 is added, a foaming agent is added after stirring, and a product is obtained after roughing and concentrating.

3. The flotation method according to claim 2, Features: The usage of the conjugated olefin compound is 800-3000 g / t dry coal slime.

4. The flotation method according to claim 2, Features: The foaming agent is octanol.

5. The flotation method according to claim 4, Features: The dosage of the secondary octanol is 80-120 g / t dry coal slime.