A method for preparing micro-nano flaky nickel material

Through liquid phase chemical reduction method, using polyvinylpyrrolidone and sodium citrate as structural guides, a micro-nanoflake nickel material with controllable morphology was successfully prepared, solving the existing technology The problem of complex preparation process and high cost is achieved, and high performance materials suitable for printing electronics are achieved.

CN115815613BActive Publication Date: 2024-11-15NORTHWEST INSTITUTE FOR NONFERROUS METAL RESEARCH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211492676.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-11-25
Publication Date
2024-11-15
Estimated Expiration
2042-11-25

AI Technical Summary

Technical Problem

The prior art is difficult to control the morphology when preparing two-dimensional micro-nano nickel materials, and it is cost-effective and has a complex preparation process, making it not suitable for large-scale production.

Method used

The liquid phase chemical reduction method is used to mix nickel raw materials for reaction without hard templates and no external magnetic field. Polyvinylpyrrolidone and sodium citrate are used as structural guides to generate complexes by controlling the reaction conditions to promote the orientation of nickel atoms. Growth, achieve anisotropic growth, and prepare micro-nanoflake nickel materials with controllable morphology.

Benefits of technology

The process is simplicity, controllability and low cost, and a micro-nano sheet-shaped nickel material with high mechanical flexibility and excellent conductivity is prepared, suitable for printing electronic conductive inks and for large-scale production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115815613B_ABST
    Figure CN115815613B_ABST
Patent Text Reader

Abstract

The invention discloses a method for preparing a micro-nano flaky nickel material, which comprises: 1. mixing a nickel source, polyvinyl pyrrolidone, sodium citrate, sodium hydroxide, hydrazine hydrate, ethylene glycol and H2O, and then stirring the mixture with magnetic force to obtain a blue transparent solution; 2. transferring the blue transparent solution to an electric constant temperature water bath for reaction; 3. separating the reaction product with a magnet, and obtaining the micro-nano flaky nickel material after washing and drying. The invention reduces the raw materials by mixing them in a "one-pot method" without a hard template and an external magnetic field, and promotes the anisotropic growth of nickel atoms and controls the morphology of the micro-nano flaky nickel material by selecting polyvinyl pyrrolidone PVP and sodium citrate as structure directing agents. The process is simple, easy to control, low in cost, and easy to produce on a large scale. The micro-nano flaky nickel material has a high sheet diameter ratio, good mechanical flexibility and excellent electrical conductivity, and is suitable for various flexible electronic devices.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of flexible printed electronic material processing, and in particular relates to a method for preparing a micro-nano flaky nickel material. Background Art

[0002] With the rapid development of wearable smart devices, the market demand for flexible electronic devices is increasing, but the traditional preparation process of flexible electronic devices is not suitable for large-area manufacturing. In contrast, printed electronics technology can achieve fast, low-cost, and large-area manufacturing of flexible electronic devices. Printed electronics use conductive ink instead of ordinary ink and use printing to additively manufacture on flexible substrates. Therefore, the performance of conductive ink not only restricts the printability, but also affects the performance and application scenarios of the prepared flexible electronic devices.

[0003] Conductive ink in printed electronics is a suspension composed of conductive fillers, connectors, solvents, additives, etc. Among them, conductive fillers are materials with conductive, dielectric or semiconductor properties, which are mainly divided into three categories: carbon-based materials, polymer materials and nano-metal materials. Carbon-based materials are low-cost, easy to prepare, light in weight and have good mechanical properties, but their conductivity is lower than that of metal materials, and the adhesion of carbon-based conductive ink to the substrate is poor, which reduces the flexibility and practicality in flexible electronic devices; polymer materials have more sources, lower costs, better compatibility with the substrate, and good application prospects, but compared with metal materials, polymer materials have poor conductivity, which limits their application scenarios. Metal materials have good conductivity and a relatively simple preparation process, and are most widely used in conductive inks.

[0004] The most commonly used nanometal materials in conductive inks are: gold, copper, silver, nickel, etc. Nanogold and nanosilver have excellent conductivity and working stability, but the preparation cost is high, which seriously restricts their large-scale production and application. Nanocopper materials are low in cost and have good conductivity, but they easily react with oxygen in the air, and their poor stability limits their scope of application. Nanonickel has slightly worse conductivity than precious metals, but it is low in cost and has better stability in the air. In addition, its unique ferromagnetism can be developed and applied to high-density magnetic recording, magnetic sensors, etc. It can be used as a candidate material for nanometals and functional electronic devices in some civil or industrial production.

[0005] Due to their special morphology, two-dimensional nickel nanomaterials can increase the contact area between nanomaterials and enhance the mechanical flexibility of the materials in practical applications, thereby enhancing the conductivity and flexibility of the materials. However, the preparation of two-dimensional nickel nanomaterials still faces huge challenges. Because under mild reaction conditions, the crystal morphology of two-dimensional nickel nanomaterials is easy to control, and the standard potential of nickel ions is relatively low, strong reducing agents are usually required in the preparation of two-dimensional micro-nano nickel materials. However, strong reducing agents will increase the reduction rate, making it more difficult to control the morphology of two-dimensional micro-nano nickel materials.

[0006] At present, low-dimensional nickel nanomaterials are mostly prepared by using an external magnetic field or a hard template method. In the process of using the hard template method to prepare low-dimensional materials, Al2O3, Si and other materials are usually used as hard templates to deposit nickel atoms at specific positions of the template. After the reaction is completed, the product and the template are peeled off by chemical etching to obtain a sample that retains the template morphology. However, during the product and template peeling process, template etching will also damage the product, and the customization of templates with specific morphology will also increase the cost. In order to reduce the cost of template preparation and solve the peeling problem, the magnetism of nickel atoms themselves can be used to select an external magnetic field assisted method to promote the directional deposition of nickel atoms along the direction of magnetic flux lines and control their morphology. However, the preparation process requires the addition of equipment with a magnetic field, which increases the production cost and is not suitable for large-scale production. Therefore, how to prepare low-dimensional micro-nano nickel materials with controllable morphology in a simple way without an external magnetic field and without the assistance of a hard template is still a difficult problem. Summary of the invention

[0007] The technical problem to be solved by the present invention is to provide a method for preparing a micro-nano flaky nickel material in view of the deficiencies of the above-mentioned prior art. The method prepares a two-dimensional micro-nano flaky nickel material by mixing the raw materials in a "one-pot method" and then reducing them through reaction without a hard template and an external magnetic field. The method promotes the directional growth of nickel atoms by selecting polyvinyl pyrrolidone PVP and sodium citrate as structure-directing agents, and at the same time generates a complex to effectively control the reduction rate of nickel ions, so that they are converted into nickel atoms and deposited at specific positions for anisotropic growth, thereby controlling the morphology of the two-dimensional micro-nano flaky nickel material. The method has a simple process, is easy to control, has low cost, and is easy to produce on a large scale.

[0008] In order to solve the above technical problems, the technical solution adopted by the present invention is: a method for preparing a micro-nano flaky nickel material, characterized in that the raw materials are mixed simultaneously by a liquid phase chemical reduction method without a hard template and an external magnetic field to prepare a micro-nano flaky nickel material with a sheet diameter of 50 μm to 400 μm and a thickness of 0.5 μm to 2 μm, and the method comprises the following steps:

[0009] Step 1: Mix the nickel source, polyvinyl pyrrolidone, sodium citrate, sodium hydroxide, hydrazine hydrate, ethylene glycol and H2O in proportion and stir them magnetically for more than 3 hours to obtain a blue transparent solution;

[0010] Step 2: Transfer the blue transparent solution obtained in step 1 to an electric constant temperature water bath for reaction; the electric constant temperature water bath is a non-magnetic pot;

[0011] Step 3: Separate the product of the reaction in step 2 with a magnet, then wash with H2O and anhydrous ethanol respectively, and obtain micro-nano flaky nickel material after vacuum drying.

[0012] The invention adopts a liquid phase chemical reduction method, under the condition of no hard template and no external magnetic field, the raw materials are mixed and stirred in a "one-pot method" and then reacted, and hydrazine hydrate is used for reduction in an alkaline environment, and polyvinyl pyrrolidone PVP and sodium citrate are selected as structure directing agents to promote the reduction of nickel ions into nickel atoms for directional growth, and generate complexes, thereby effectively controlling the reduction speed of nickel ions, reducing the activity of the crystal surface of nickel particles, and converting them into nickel atoms for deposition at specific positions; at the same time, ethylene glycol is added to the reaction system to increase the system density, thereby reducing the probability of mutual collision between nickel atomic particles, and combining the addition of sodium citrate and Ni in the reaction system. 2+ After complexation, its surface is passivated, which promotes the generation of hemispherical particles in the initial stage of the reaction, and then grows laterally after directional arrangement, thus realizing the anisotropic growth of nickel materials, thereby controlling their morphology and obtaining micro-nano flaky nickel materials.

[0013] The method for preparing the micro-nano flaky nickel material is characterized in that the nickel source in step 1 is nickel sulfate hexahydrate or nickel chloride hexahydrate. The present invention controls the type of nickel source to ensure the smooth progress of the reduction reaction to obtain a magnetic product, which is easy for the subsequent separation process.

[0014] The above-mentioned method for preparing a micro-nano flaky nickel material is characterized in that the molar ratio of the nickel source, polyvinyl pyrrolidone, and sodium citrate in step one is 1:0-1.8:0.96-3.36. The research process of the present invention confirms that sodium citrate is the key to the anisotropic growth of micro-nano flaky nickel materials. By limiting the above-mentioned molar ratio, the anisotropic growth process of the micro-nano flaky nickel material is adjusted to avoid excessive PVP causing excessive steric hindrance effect, inhibiting the anisotropic growth of the product and obtaining a chain product, and the problem that too little sodium citrate is used and cannot be completely adsorbed to a specific crystal plane, resulting in unclear anisotropic growth, a large number of particles in the product and serious particle agglomeration, and too much sodium citrate is used and the adsorption amount is large, passivating Ni 2+ On the other hand, this leads to the problem of a large number of chain products in the product.

[0015] The above-mentioned method for preparing a micro-nano flaky nickel material is characterized in that the molar ratio of the nickel source, sodium hydroxide, and hydrazine hydrate in step 1 is 1:4.8-14.4:14.4-43.2. The reduction potential of hydrazine hydrate is greatly affected by the acidity and alkalinity of the solution. In an acidic and neutral environment, the reduction potential of hydrazine hydrate is higher than that of Ni 2+ , it cannot be reduced. Therefore, the present invention adds sodium hydroxide to the reaction system to provide an alkaline environment, so that the reduction potential and potential of hydrazine hydrate are both reduced, which is conducive to the reduction reaction, avoiding too little sodium hydroxide to generate nickel hydrazine complex and adsorb on the surface of hemispherical particles to inhibit the reduction reaction, the generated particles are only partially arranged in a directional manner, and the nickel hydrazine complex falls off after cleaning due to insufficient adhesion, and the sheet structure disappears in the product to form a large number of particles. The problem, and excessive sodium hydroxide causes a large amount of nickel hydroxide with strong adhesion to be deposited on the particle surface before it can be reduced, so that the sheet structure of the product is coated by a large number of intermediate products; at the same time, since the reduction performance in the reaction system is determined by the amount of hydrazine hydrate, by controlling the above-mentioned molar ratio, it is avoided that insufficient amount of reducing agent causes some intermediate products to be unable to be reduced, and the sheet structure of the product is surrounded by a large number of intermediate products. The problem, and excessive amount of reducing agent, strong reducibility, and accelerated reduction reaction, the generated particles have not yet been arranged, that is, the reaction ends, resulting in a large number of spherical and chain products in the product.

[0016] The above-mentioned method for preparing a micro-nano flaky nickel material is characterized in that the mass ratio of the nickel source, ethylene glycol, and H2O in step 1 is 1:2.74-41.03:53.27-95.89. The present invention adds ethylene glycol as a solvent in the reaction system, and controls the density of the reaction system by controlling the mass ratio of the above-mentioned raw materials to achieve anisotropic growth of the nickel material, thereby avoiding the problem that too little ethylene glycol leads to a low density of the reaction system, an increased probability of collision between particles and a faster reaction rate, and an increased difficulty in controlling the product morphology, as well as excessive ethylene glycol leading to a high density of the reaction system and partial adsorption of ethylene glycol on the Ni 2+ The surface inhibits the reduction reaction and generates a large number of intermediate products. At the same time, it avoids the problem that too little H2O leads to too high ion density in the reaction system, accelerated reaction rate and serious particle agglomeration in the product, and too much H2O leads to too low ion density in the reaction system, incomplete reduction reaction and coexistence of magnetic products and intermediate products in the product.

[0017] The above-mentioned method for preparing a micro-nano flaky nickel material is characterized in that the temperature of the reaction in step 2 is 60°C to 80°C and the time is 5h to 19h. The present invention controls the temperature of the reaction to ensure the smooth progress of the reduction reaction, avoiding the problem that the temperature is too low, resulting in insufficient reducibility of hydrazine hydrate and the inability to undergo a reduction reaction, and the problem that the movement rate of the particles in the reaction system is accelerated due to the high temperature, the reduction reaction is accelerated, and mild conditions cannot be provided for the growth process of the particles, thereby obtaining a chain product rather than a micro-nano flaky structure product, and at the same time avoiding the problem that the reaction time is too short, resulting in an incomplete reduction reaction and poor product morphology, and the reaction time is too long, resulting in excessive lateral elongation of the particles in the product and connecting into large pieces and being unable to be separated.

[0018] The above-mentioned method for preparing a micro-nano flaky nickel material is characterized in that the vacuum drying temperature in step three is 40°C to 90°C.

[0019] Compared with the prior art, the present invention has the following advantages:

[0020] 1. The present invention adopts a liquid phase chemical reduction method. Under the condition of no hard template and no external magnetic field, the raw materials are mixed and stirred in a "one-pot method" and then reacted. Hydrazine hydrate is used for reduction in an alkaline environment. Polyvinyl pyrrolidone PVP and sodium citrate are selected as structure-directing agents to promote the directional growth of nickel atoms. At the same time, the complex is generated to effectively control the reduction rate of nickel ions, reduce the activity of the crystal surface of nickel particles, and convert them into nickel atoms to deposit at specific positions for anisotropic growth, thereby controlling their morphology and preparing a two-dimensional micro-nano flaky nickel material.

[0021] 2. The preparation method and equipment of the present invention are simple, the process parameters are controllable, the repeatability is high, the raw material sources are abundant, the cost is low, and it is easy to scale up production.

[0022] 3. The two-dimensional micro-nano flaky nickel material prepared by the present invention has a high sheet diameter ratio (diameter / thickness ratio), good mechanical flexibility and excellent conductivity. It is an ideal printed electronic conductive ink filler and is widely used in various flexible electronic devices.

[0023] The technical solution of the present invention is further described in detail below through the accompanying drawings and embodiments. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1a This is a high-magnification SEM image of the micro-nano flaky nickel material prepared in Example 1 of the present invention.

[0025] Figure 1b This is a low-magnification SEM image of the micro-nano flaky nickel material prepared in Example 1 of the present invention.

[0026] Figure 2aThis is a low-magnification SEM image of the micro-nano flaky nickel material prepared in Example 2 of the present invention.

[0027] Figure 2b This is a high-magnification SEM image of the micro-nano flaky nickel material prepared in Example 2 of the present invention.

[0028] Figure 3 This is the XRD pattern of the micro-nano flaky nickel material prepared in Example 2 of the present invention.

[0029] Figure 4 This is a physical picture of the micro-nano flaky nickel material after tableting prepared in Example 2 of the present invention.

[0030] Figure 5a This is a high-magnification SEM image of the micro-nano flaky nickel material prepared in Example 3 of the present invention.

[0031] Figure 5b This is a low-magnification SEM image of the micro-nano flaky nickel material prepared in Example 3 of the present invention. DETAILED DESCRIPTION

[0032] Example 1

[0033] In this embodiment, a liquid phase chemical reduction method is used to prepare a micro-nano flaky nickel material with a sheet diameter of 50 μm and a thickness of 0.6 μm by mixing the raw materials simultaneously without a hard template and an external magnetic field. The method comprises the following steps:

[0034] Step 1: 0.3 g nickel chloride hexahydrate, 0.54 g PVP (M w =24000, K29), 1.0 g sodium citrate, 4.32 g sodium hydroxide, 12.96 g hydrazine hydrate, 13.7 ml ethylene glycol and 28.8 mL water were mixed and magnetically stirred for 3 h to obtain a blue transparent solution;

[0035] Step 2: Transfer the blue transparent solution obtained in step 1 to a non-magnetic electric constant temperature water bath and react at 60° C. for 19 h;

[0036] Step 3: Separate the product of the reaction in step 2 with a magnet, then wash with H2O and anhydrous ethanol respectively, and obtain a micro-nano flaky nickel material after vacuum drying at 40°C.

[0037] Figure 1a This is a high-magnification SEM image of the micro-nano flaky nickel material prepared in this example. Figure 1b This is a low-magnification SEM image of the micro-nano flaky nickel material prepared in this example. Figure 1a and Figure 1b It can be seen that the nickel material is a micro-nano flake structure, and the flake diameter is about 50 μm and the thickness is about 0.6 μm.

[0038] Example 2

[0039] In this embodiment, a liquid phase chemical reduction method is used to prepare a micro-nano flaky nickel material with a sheet diameter of 100 μm and a thickness of 0.9 μm by mixing the raw materials simultaneously without a hard template and an external magnetic field. The method comprises the following steps:

[0040] Step 1: 1g nickel sulfate hexahydrate, 1.5g PVP (M w =24000, K29), 2.5 g sodium citrate, 7.5 g sodium hydroxide, 28.5 g hydrazine hydrate, 22.8 mL ethylene glycol and 76.1 mL water were mixed and magnetically stirred for 3 h to obtain a blue transparent solution;

[0041] Step 2: Transfer the blue transparent solution obtained in step 1 to a non-magnetic electric constant temperature water bath and react at 80° C. for 5 h;

[0042] Step 3: Separate the product of the reaction in step 2 with a magnet, then wash with H2O and anhydrous ethanol respectively, and obtain a micro-nano flaky nickel material after vacuum drying at 90°C.

[0043] Figure 2a This is a low-magnification SEM image of the micro-nano flaky nickel material prepared in this example. Figure 2b This is a high-magnification SEM image of the micro-nano flaky nickel material prepared in this example. Figure 2a and Figure 2b It can be seen that the nickel material is a micro-nano flake structure, and the flake diameter is about 100 μm and the thickness is about 0.9 μm.

[0044] Figure 3 The XRD pattern of the micro-nano flaky nickel material prepared in this example is shown in FIG. Figure 3 It can be seen that the positions of the diffraction peaks of the nickel material at 2θ=44.5°, 51.8° and 76.3° correspond to the (111) crystal plane, (200) crystal plane and (220) crystal plane of nickel respectively. The positions of all diffraction peaks are consistent with the JCPDS standard card 04-0850, and the standardized index is face-centered cubic Ni.

[0045] The micro-nano nickel flake material prepared in this embodiment is pressed into thin sheets using a tablet press. Figure 4 As shown, the resistance of the thin film was then measured using a four-probe tester for a total of 5 times, and the results are shown in Table 1.

[0046] Table 1

[0047] Measurement process 1st time 2nd 3rd 4th 5th Resistance value (Ω / cm) 0.099 0.102 0.105 0.100 0.097

[0048] The average value of the resistance values ​​measured 5 times in Table 1 is 0.101Ω·cm -1, indicating that the micro-nano flaky nickel material prepared in this embodiment has good electrical conductivity.

[0049] Example 3

[0050] In this embodiment, a liquid phase chemical reduction method is used to prepare a micro-nano flaky nickel material with a sheet diameter of 400 μm and a thickness of 2 μm by mixing the raw materials simultaneously without a hard template and an external magnetic field. The method comprises the following steps:

[0051] Step 1: 3 g of nickel sulfate hexahydrate, 2.88 g of sodium citrate, 14.4 g of sodium hydroxide, 43.2 g of hydrazine hydrate, 9.1 mL of ethylene glycol and 159.8 mL of water were mixed and magnetically stirred for 3 h to obtain a blue transparent solution;

[0052] Step 2: Transfer the blue transparent solution obtained in step 1 to a non-magnetic electric constant temperature water bath and react at 80° C. for 5 h;

[0053] Step 3: Separate the product of the reaction in step 2 with a magnet, then wash with H2O and anhydrous ethanol respectively, and obtain a micro-nano flaky nickel material after vacuum drying at 90°C.

[0054] Figure 5a This is a high-magnification SEM image of the micro-nano flaky nickel material prepared in this example. Figure 5b This is a low-magnification SEM image of the micro-nano flaky nickel material prepared in this example. Figure 5a and Figure 5b It can be seen that the nickel material contains about 50% of micro-nano flake structures, and the flake diameter is about 400 μm and the thickness is about 2 μm.

[0055] The above is only a preferred embodiment of the present invention and does not limit the present invention in any way. Any simple modification, change and equivalent change made to the above embodiment according to the technical essence of the invention still falls within the protection scope of the technical solution of the present invention.

Claims

1. A method for preparing micro-nano flaky nickel material, It is characterized in that A liquid phase chemical reduction method is used to prepare a micro-nano flaky nickel material with a sheet diameter of 50 μm to 400 μm and a thickness of 0.5 μm to 2 μm by mixing the raw materials simultaneously without a hard template and an external magnetic field. The method comprises the following steps: Step 1: nickel source, polyvinyl pyrrolidone, sodium citrate, sodium hydroxide, hydrazine hydrate, ethylene glycol, H 2 O were mixed in proportion and magnetically stirred for more than 3 h to obtain a blue transparent solution; Step 2: Transfer the blue transparent solution obtained in step 1 to an electric constant temperature water bath for reaction; the electric constant temperature water bath is a non-magnetic pot; Step 3: Separate the products of the reaction in step 2 using a magnet, and then use H 2 O and anhydrous ethanol and then vacuum dried to obtain micro-nano flaky nickel material.

2. A method for preparing a micro-nano flaky nickel material according to claim 1, It is characterized in that The nickel source in step 1 is nickel sulfate hexahydrate or nickel chloride hexahydrate.

3. The method for preparing a micro-nano flaky nickel material according to claim 1, It is characterized in that The molar ratio of the nickel source, polyvinyl pyrrolidone and sodium citrate in step 1 is 1:0-1.8:0.96-3.

36.

4. The method for preparing a micro-nano flaky nickel material according to claim 1, It is characterized in that The molar ratio of the nickel source, sodium hydroxide and hydrazine hydrate in step 1 is 1:4.8-14.4:14.4-43.

2.

5. The method for preparing a micro-nano flaky nickel material according to claim 1, It is characterized in that The nickel source, ethylene glycol, H 2 The mass ratio of O is 1:2.74~41.03:53.27~95.

89.

6. The method for preparing a micro-nano flaky nickel material according to claim 1, It is characterized in that The reaction temperature in step 2 is 60° C. to 80° C., and the reaction time is 5 h to 19 h.

7. The method for preparing a micro-nano flaky nickel material according to claim 1, It is characterized in that The vacuum drying temperature in step 3 is 40°C to 90°C.