A low surface energy change cover glass protective film and preparation method thereof
By introducing a non-ionic fluorine surfactant into the cover glass protective film, a spatial network layer is formed, which solves the problem of surface energy decrease during processing, ensures high adhesion and stability, and satisfies the ink surface bonding requirement. demand, and reduces the peel strength of the protective film.
Patent Information
- Application Number
- CN202211270924.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-10-17
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2042-10-17
AI Technical Summary
During the processing of the cover glass, especially after frame printing, the surface energy of the ink area and window area drops below 34 dynes, which affects the adhesion and overall waterproof performance of subsequent processes.
A low surface energy change cover glass protective film including a PE base material layer and an acrylic pressure-sensitive adhesive layer is used. Non-ionic fluorine surfactants FC-4430 and FC-4434 are introduced into the acrylic pressure-sensitive adhesive to form a spatial network. It blocks the precipitation of residual monomers or other small molecules from glue synthesis, ensuring that the surface energy of the protective film is stable above 36 dynes after the protective film is attached.
It effectively improves the surface energy of the glass surface after the protective film is attached to meet the adhesion of the ink surface for subsequent lamination. It also ensures full cross-linking within the glue through fully automatic constant tension adjustment and thermal aging, reduces the peeling strength, and prevents additive transfer.
Smart Images

Figure BDA0003892696710000061 
Figure BDA0003892696710000071 
Figure HDA0003892696720000011
Abstract
Description
Technical Field
[0001] The present invention relates to the field of C09J7 / 38, and in particular to a low surface energy change cover glass protective film and a preparation method thereof. Background Art
[0002] Cover glass is mainly used for the outermost layer of the touch screen. The main raw material of the product is ultra-thin flat glass, which has the functions of anti-impact, scratch resistance, oil resistance, anti-fingerprint, and enhanced light transmittance. It is currently widely used in a variety of electronic consumer products with touch and display functions. Compared with cover plates made of other materials, cover glass has obvious advantages in important parameters and properties such as surface finish, thickness, high hardness, pressure resistance, and scratch resistance, so it has gradually become the mainstream protection solution for various touch technologies. With the increasing popularity of 5G networks, in order to solve the problem that metal materials easily weaken 5G signal transmission, more and more mobile phones’ back covers are also made of non-metallic materials such as glass with excellent signal transmission. The rise of large-screen tablet devices that support 5G networks on the market has led to a rapid increase in demand for cover glass.
[0003] From the perspective of structural breakdown, the current mobile phone screen is mainly composed of three major parts: window protection glass, touch module, and display module, and the display module structure also includes two substrate glasses. The window protection glass has the characteristics of high strength, high light transmittance, good toughness, and scratch resistance. Its inner surface must be able to fit tightly with the touch module and display screen, and the outer surface must have sufficient strength to achieve the protection function of the flat screen, touch module, etc.
[0004] The production and processing flow of cover glass: engineering design → cutting and opening → fine carving → grinding → cleaning → hot bending → polishing → testing → tempering → UV transfer → coating (PVD) → frame printing (screen printing, spraying) ink → laminating → laminating → packaging, etc. Chinese patent CN108864977B discloses a PET protective film and preparation method for cover glass processing or shipment. Specifically, polyurethane acrylate and acrylate monomers are used as raw materials to prepare an anti-static pressure-sensitive adhesive layer, so that the provided protective film solves the problems of poor scratch resistance, easy powdering, and poor die-cutting resistance of traditional acrylic products. However, a protective film must be attached at each stage of the cover glass processing flow to protect the surface from scratches, especially after the frame printing (screen printing, spraying) ink process. The protective film attached cannot significantly reduce the surface energy of the ink area and the window area. The surface energy of the ink area and the window area is generally required to reach 34 dynes or above. If it is lower than 34 dynes, it will reduce the adhesion of the subsequent process and affect the overall waterproof performance of the assembled product. Summary of the invention
[0005] In order to solve the problem that the surface energy of the ink area and the window area of the glass frame drops below 34 dynes after the cover glass is attached, the present invention provides a low surface energy change cover glass protective film and a preparation method thereof, which effectively improves the problem of surface energy drop after the protective film is attached to the cover glass, so that the surface energy of the glass cover is stabilized at more than 36 dynes, meeting the subsequent bonding adhesion of the ink surface.
[0006] On the one hand, the present invention provides a low surface energy change cover glass protective film, comprising a PE substrate layer and an acrylic pressure-sensitive adhesive layer; in parts by weight, the raw materials for preparing the acrylic pressure-sensitive adhesive layer at least include: 80-120 parts of acrylic adhesive, 280-350 parts of diluent, 2-5 parts of isocyanate curing agent, and 0.2-1 part of surfactant.
[0007] As a preferred technical solution, the thickness of the PE substrate layer is 48-68 μm; the thickness of the acrylic pressure-sensitive adhesive layer is 1-3 μm;
[0008] As a preferred technical solution, the raw materials for preparing the acrylic adhesive include at least 50-120 parts by weight of soft monomer, 3-8 parts of hard monomer, 3-8 parts of hydroxyl-containing acrylate monomer, and 0.01-0.1 parts of initiator.
[0009] Preferably, the soft monomer is selected from at least one of isooctyl acrylate, methyl acrylate, butyl acrylate and ethyl acrylate; preferably, the soft monomer is isooctyl acrylate, methyl acrylate and ethyl acrylate; the mass ratio of isooctyl acrylate, methyl acrylate and ethyl acrylate is (40-75):(10-20):(8-15).
[0010] Preferably, the hard monomer is at least one of methyl methacrylate, butyl methacrylate, and isooctyl methacrylate;
[0011] Preferably, the hydroxyl-containing acrylate monomer is at least one of hydroxyethyl acrylate, trimethylolpropane diacrylate, trimethylolpropane triacrylate, and pentaerythritol triacrylate; preferably, the hydroxyl-containing acrylate monomer is hydroxyethyl acrylate.
[0012] Preferably, the initiator is azobisisobutyronitrile.
[0013] Preferably, the preparation process of the acrylic adhesive is as follows: adding soft monomer, hard monomer, hydroxyl-containing acrylate monomer and initiator in parts by weight, stirring and dispersing, and vacuum degassing to obtain the acrylic adhesive.
[0014] As a preferred technical solution, the diluent is at least one of ethyl acetate, butyl acetate and toluene; preferably, the diluent is a combination of ethyl acetate, butyl acetate and toluene; the mass ratio of ethyl acetate, butyl acetate and toluene is (180-220):(90-110):(15-25).
[0015] As a preferred technical solution, the isocyanate curing agent is at least one of toluene diisocyanate (TDI), isophorone diisocyanate (IPDI), diphenylmethane diisocyanate (MDI), dicyclohexylmethane diisocyanate (HMDI), and hexamethylene diisocyanate (HDI); preferably, the isocyanate curing agent is hexamethylene diisocyanate. Preferably, the hexamethylene diisocyanate contains a biuret structure; the model of the hexamethylene diisocyanate is HB-100, from Wanhua Chemical.
[0016] As a preferred technical solution, the surfactant is at least one of a fluorine surfactant and a hydrocarbon surfactant; preferably, the surfactant is a fluorine surfactant; the fluorine surfactant is a non-ionic fluorine surfactant; preferably, the non-ionic fluorine surfactant is FC-4430 and / or FC-4434. Preferably, the non-ionic fluorine surfactants are FC-4430 and FC-4434; the mass ratio of FC-4430 and FC-4434 is (0.8-1.2): (1-1.5); based on the system of the present invention, by introducing 0.2-1 parts of surfactant into the system, especially the introduced surfactants are FC-4430 and FC-4434 non-ionic fluorine surfactants with a mass ratio of (0.8-1.2): (1-1.5), which interact with the acrylate polymer in the system to form a spatial network layer, blocking the precipitation of residual monomers or other small molecules synthesized by the glue, and can effectively improve the problem of surface energy decrease after the protective film is attached to the cover glass, so that the surface energy of the glass cover can be stabilized at a value of more than 36 dynes, meeting the subsequent bonding adhesion of the ink surface.
[0017] The non-ionic fluorine surfactants FC-4430 and FC-4434 are both from Kunshan Libaodi Electronic Materials Co., Ltd.
[0018] Another aspect of the present invention provides a method for preparing a low surface energy change cover glass protective film, comprising at least the following steps:
[0019] (1) In a Class 10,000 dust-free workshop, a three-layer co-extruded dust removal system and a five-layer high-density special steel filter are used to blow the PE substrate;
[0020] (2) adding an acrylic adhesive to a diluent by weight, stirring and dispersing, then adding an isocyanate curing agent and a surfactant, and stirring for 20 minutes to obtain an acrylic pressure-sensitive adhesive;
[0021] (3) Ensure that the coating workshop is a Class 1000 cleanroom, use the gravure coating method to coat the acrylic pressure-sensitive adhesive, and put it into the oven for curing and winding after leveling with a mirror scraper. The wound finished product is then placed in a constant temperature aging room at 48-55°C for 96-120 hours.
[0022] Based on the system of the present invention, by controlling the blowing conditions of the PE substrate, it is ensured that the fisheye diameter of the substrate quality appearance cannot exceed 0.1mm, the fisheyes and impurity points do not exceed 5PCS / 1 square meter, there are no scratch lines with a length exceeding 2mm, and the light transmittance of the PE substrate reaches more than 88%.
[0023] Based on the system of the present invention, the entire coating production line of acrylic pressure-sensitive adhesive is fully automatic with constant tension adjustment to ensure that the finished product is rolled up flat and without creases. By controlling the finished product after rolling up to be aged again at 48-55°C for 96-120 hours, it is ensured that the glue is fully cross-linked internally, so that the prepared protective film has a lower peel strength, which is helpful for the removal of the protective film. At the same time, it has excellent polymer stability, which can prevent the problem of the additives being transferred to the adherend due to the additives.
[0024] Beneficial Effects
[0025] 1. Based on the system of the present invention, by introducing 0.2-1 parts of surfactant into the system, especially the surfactant introduced is FC-4430 and FC-4434 non-ionic fluorine surfactants with a mass ratio of (0.8-1.2): (1-1.5), which interact with the acrylate polymer in the system to form a spatial network layer, blocking the precipitation of residual monomers or other small molecules synthesized by the glue, the problem of surface energy reduction after the protective film is attached to the cover glass can be effectively improved, so that the surface energy of the glass cover can be stabilized at more than 36 dynes, which meets the subsequent bonding adhesion of the ink surface.
[0026] 2. Based on the system of the present invention, the entire coating production line of acrylic pressure-sensitive adhesive is fully automatic with constant tension adjustment to ensure that the finished product is rolled up flat and without creases. By controlling the finished product after rolling up to be aged again at 48-55°C for 96-120 hours, it is ensured that the glue is fully cross-linked internally, so that the prepared protective film has a lower peel strength, which is helpful for the removal of the protective film. At the same time, it has excellent polymer stability, which can prevent the problem of the additives being transferred to the adherend due to the additives. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] Figure 1This is a schematic diagram of the structure of the low surface energy change cover glass protective film prepared in Example 1 of the present invention, wherein: 1. acrylic pressure-sensitive adhesive layer; 2. PE substrate layer. DETAILED DESCRIPTION
[0028] Example 1
[0029] See also Figure 1 Embodiment 1 of the present invention provides a low surface energy change cover glass protective film, including a PE substrate layer and an acrylic pressure-sensitive adhesive layer; in parts by weight, the raw materials for preparing the acrylic pressure-sensitive adhesive layer include: 100 parts of acrylic adhesive, 320 parts of diluent, 3 parts of isocyanate curing agent, and 0.5 parts of surfactant.
[0030] The thickness of the PE substrate layer is 50 μm; the thickness of the acrylic pressure-sensitive adhesive layer is 1.5 μm;
[0031] The raw materials for preparing the acrylic adhesive include at least 90 parts by weight of soft monomer, 5 parts of hard monomer, 5 parts of hydroxyl-containing acrylate monomer and 0.01 parts of initiator.
[0032] The soft monomers are isooctyl acrylate, methyl acrylate and ethyl acrylate; the mass ratio of isooctyl acrylate, methyl acrylate and ethyl acrylate is 6:2:1.
[0033] The hard monomer is methyl methacrylate;
[0034] The hydroxyl-containing acrylic ester monomer is hydroxyethyl acrylate.
[0035] The initiator is azobisisobutyronitrile.
[0036] The preparation process of the acrylic adhesive is as follows: adding soft monomer, hard monomer, hydroxyl-containing acrylate monomer and initiator in parts by weight, stirring and dispersing, and vacuum degassing to obtain the acrylic adhesive.
[0037] The diluent is a combination of ethyl acetate, butyl acetate and toluene; the mass ratio of the ethyl acetate, butyl acetate and toluene is 10:5:1.
[0038] The isocyanate curing agent is hexamethylene diisocyanate. The model of the hexamethylene diisocyanate is HB-100, from Wanhua Chemical.
[0039] The surfactant is a fluorine surfactant; the fluorine surfactant is a non-ionic fluorine surfactant; the non-ionic fluorine surfactant is FC-4430 and FC-4434; the mass ratio of FC-4430 to FC-4434 is 1:1. The non-ionic fluorine surfactants FC-4430 and FC-4434 are both from Kunshan Libaodi Electronic Materials Co., Ltd.
[0040] Embodiment 1 of the present invention provides, on the other hand, a method for preparing a low surface energy change cover glass protective film, comprising the following steps:
[0041] (1) In a Class 10,000 dust-free workshop, a three-layer co-extruded dust removal system and a five-layer high-density special steel filter are used to blow the PE substrate;
[0042] (2) adding an acrylic adhesive to a diluent by weight, stirring and dispersing, then adding an isocyanate curing agent and a surfactant, and stirring for 20 minutes to obtain an acrylic pressure-sensitive adhesive;
[0043] (3) Ensure that the coating workshop is a Class 1000 cleanroom, use the gravure coating method to coat the acrylic pressure-sensitive adhesive, and after leveling with a mirror scraper, put it into an oven for curing and winding. The wound product is then placed in a constant temperature aging room at 50°C for 120 hours.
[0044] Example 2
[0045] Example 2 of the present invention provides a low surface energy change cover glass protective film and a preparation method thereof. Its specific implementation method is the same as that of Example 1, except that, in parts by weight, the raw materials for preparing the acrylic pressure-sensitive adhesive layer include: 120 parts of acrylic adhesive, 300 parts of diluent, 3 parts of isocyanate curing agent, and 0.5 parts of surfactant.
[0046] Example 3
[0047] Example 3 of the present invention provides a low surface energy change cover glass protective film and a preparation method thereof. Its specific implementation method is the same as that of Example 1. In parts by weight, the raw materials for preparing the acrylic pressure-sensitive adhesive layer include: 90 parts of acrylic adhesive, 330 parts of diluent, 3 parts of isocyanate curing agent, and 0.5 parts of surfactant.
[0048] Comparative Example 1
[0049] Comparative Example 1 of the present invention provides a low surface energy change cover glass protective film and a preparation method thereof. Its specific implementation method is the same as that of Example 1, except that, in parts by weight, the raw materials for preparing the acrylic pressure-sensitive adhesive layer include: 120 parts of acrylic adhesive, 300 parts of diluent, and 3 parts of isocyanate curing agent.
[0050] Comparative Example 2
[0051] Comparative Example 2 of the present invention provides a low surface energy change cover glass protective film and a preparation method thereof, and its specific implementation manner is the same as that of Example 1, except that the diluent is ethyl acetate.
[0052] Comparative Example 3
[0053] Comparative Example 3 of the present invention provides a low surface energy change cover glass protective film and a preparation method thereof, and its specific implementation manner is the same as that of Example 1, except that the surfactant is sodium dodecylbenzene sulfonate.
[0054] Performance Testing Methods
[0055] 1. The low surface energy change cover glass protective film prepared in the examples and comparative examples was attached to a clean glass cover (including the ink area and the window area), and its dyne value was tested using a dyne pen. It was left to stand for 30 days under 25°C and 60% humidity conditions. After the protective film was removed, the dyne value of the cover glass surface was tested using a dyne pen. The results are shown in Table 1.
[0056] 2. Referring to the national standard GB 2792-2014, the peeling force of the protective films prepared in the examples and comparative examples was tested. The results are shown in Table 1.
[0057] Table 1: Performance test results of protective film products of embodiments and comparative examples
[0058]
[0059]
Claims
1. A low surface energy variable cover glass protective film, It is characterized in that It includes a PE substrate layer and an acrylic pressure-sensitive adhesive layer; The raw materials for preparing the acrylic pressure-sensitive adhesive layer include at least 80-120 parts of acrylic adhesive, 280-350 parts of diluent, 2-5 parts of isocyanate curing agent, and 0.2-1 parts of surfactant by weight; the raw materials for preparing the acrylic adhesive include at least 50-120 parts of soft monomer, 3-8 parts of hard monomer, 3-8 parts of hydroxyl-containing acrylate monomer, and 0.01-0.1 parts of initiator by weight; the soft monomer is isooctyl acrylate, methyl acrylate, and ethyl acrylate; the mass ratio of isooctyl acrylate, methyl acrylate, and ethyl acrylate is (40-75): (10-20): (8-15); the hard monomer is at least one of methyl methacrylate, butyl methacrylate, and isooctyl methacrylate; the initiator is azobisisobutyronitrile; the hydroxyl-containing The acrylate monomer is hydroxyethyl acrylate; the isocyanate curing agent is hexamethylene diisocyanate; the diluent is a combination of ethyl acetate, butyl acetate and toluene; the mass ratio of ethyl acetate, butyl acetate and toluene is (180-220): (90-110): (15-25); the preparation process of the acrylic adhesive is: adding soft monomer, hard monomer, hydroxyl acrylate monomer and initiator by weight, stirring and dispersing, and vacuum degassing to obtain the acrylic adhesive; the surfactant is a fluorine surfactant; the fluorine surfactant is a non-ionic fluorine surfactant; the non-ionic fluorine surfactant is FC-4430 and FC-4434; the mass ratio of FC-4430 and FC-4434 is (0.8-1.2): (1-1.5); The method for preparing the low surface energy change cover glass protective film is characterized by comprising at least the following steps: (1) In a Class 10,000 dust-free workshop, a three-layer co-extruded dust removal system and a five-layer high-density special steel filter are used to blow the PE substrate; (2) adding an acrylic adhesive to a diluent by weight, stirring and dispersing the adhesive, then adding an isocyanate curing agent and a surfactant, and stirring the mixture for 20 minutes to obtain an acrylic pressure-sensitive adhesive; (3) Ensure that the coating workshop is a Class 1000 cleanroom, use the gravure coating method to coat the acrylic pressure-sensitive adhesive, and put it into the oven for curing and winding after leveling with a mirror scraper. The wound finished product is then placed in a constant temperature aging room at 48-55°C for 96-120 hours.
Citation Information
Patent Citations
A PET protective film for cover glass manufacturing or shipping and its preparation method
CN108864977B
Preparation method of acrylic pressure-sensitive adhesive tape bonded with low-surface-energy material
CN111394008A
Pressure-sensitive adhesive composition and surface protective film
CN113993964A