A solvent extraction system for efficient lithium extraction
By using a synergistic solvent extraction system of carbonyl enol and organophosphorus in the lithium extraction process, combined with polar hydrophobic additives, efficient separation and purification of lithium, sodium, and potassium are achieved, solving the problem of low lithium extraction efficiency and poor stability in the existing technology. solve the problem and achieve efficient and low-energy lithium recovery.
Patent Information
- Application Number
- CN202211585047.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-12-09
- Publication Date
- 2024-10-08
- Estimated Expiration
- 2042-12-09
AI Technical Summary
The existing separation methods of lithium, sodium and potassium have low efficiency and poor stability of the solvent extraction system, resulting in low lithium extraction efficiency, high alkali consumption and unstable extraction process.
A synergistic solvent extraction system based on carbonyl enols and organophosphorus is used, combined with polar hydrophobic additives, to achieve efficient extraction and purification of lithium through countercurrent extraction, washing and back-extraction steps.
It achieves efficient extraction and purity improvement of lithium, reduces alkali consumption and energy consumption, solves the emulsification problem, and the extraction agent can be recycled for a long time. The lithium recovery rate can reach more than 99%, and the purity can reach more than 99.5%.
Smart Images

Figure CN115821040B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of chemical separation, and in particular relates to a solvent extraction system for efficiently extracting lithium. Background Art
[0002] Lithium is the metal with the highest energy density and an important component of lithium-ion batteries. It plays an important role in the field of new energy. With the gradual popularization of electric vehicles, the market demand for lithium salts is growing rapidly. However, lithium is associated with a variety of alkali metals, which results in low yield of lithium extraction and low purity of lithium salts. Especially for low-grade lithium resources, the current lithium extraction efficiency is extremely low.
[0003] At present, the main sources of lithium salts are ores (such as spodumene and lepidolite), salt lake brine and battery recycling. The extraction of lithium from these three resources involves the separation of lithium from other alkali metals (sodium and potassium), such as: (1) salt lake brine after magnesium removal is a mixed solution containing lithium, sodium and potassium; (2) the solution after the battery leaching solution extracts divalent and trivalent metals is a mixed solution containing lithium and sodium; (3) lithium-containing wastewater generated during battery recycling is a mixed solution containing lithium and sodium; (4) lithium precipitation mother liquor is a mixed solution containing lithium and sodium; (5) oil field brine after calcium and magnesium removal is a mixed solution containing lithium, sodium and potassium; (6) pharmaceutical wastewater of some synthetic drugs is a mixed solution containing lithium and sodium, etc.
[0004] The existing methods for separating lithium, sodium and potassium mainly include: (1) concentrating lithium by repeatedly evaporating and continuously precipitating sodium sulfate and potassium sulfate. This method is cumbersome, energy-intensive, and has a low lithium recovery rate. (2) selectively extracting lithium from a mixed solution by solvent extraction, and then purifying and concentrating lithium by washing and stripping. A typical solvent extraction system is a solvent extraction system based on β-diketone and neutral organophosphorus. However, β-diketone is an unstable compound that converts into multiple isomers; at the same time, β-diketone has low acidity (pKa≈10) and has very low activity in reacting with lithium, resulting in low lithium extraction efficiency and very high alkali consumption. In addition, β-diketone is easily decomposed in an alkaline environment, resulting in a series of problems such as loss of the extractant and emulsification, making it difficult for the extraction process to operate stably.
[0005] In view of the problems of the prior art, the present invention provides a solvent extraction system based on carbonyl enol and organic phosphorus for efficiently extracting lithium from a lithium-containing solution. The solvent extraction system has high reaction activity and high extraction selectivity, low alkali consumption and low energy consumption during the extraction process, and the extractant has a stable structure and can be repeatedly recycled without problems such as emulsification. Summary of the invention
[0006] The object of the present invention is to provide a synergistic solvent extraction system based on carbonyl enol and organophosphorus, which can efficiently extract lithium from a lithium-containing solution, and separate lithium from impurities such as sodium and potassium while efficiently recovering lithium.
[0007] A solvent extraction system for efficiently extracting lithium comprises a carbonyl enol having a structure represented by formula (IA or IB), an organic phosphorus having a structure represented by formula (IIA, IIB, IIC or IID), and an optional polar hydrophobic additive.
[0008]
[0009] In formula (IA) and (IB), R1, R2, and R3 may be the same or different and are H or C1-C 15 or an alkyl or aryl group, such as methyl, butyl, hexyl, octyl, dodecyl, phenyl, benzyl, phenylbutyl, etc.; or an alkoxy group, such as octyloxy; or an amino group, such as N,N-dibutylamino; or, R1 and R3, or R2 and R3 can be connected to form a ring, and any other groups can be connected to the ring.
[0010] The carbonyl enol can be, for example, (Z)-1-hydroxy-1-phenyl-1-dodecene-3-one, (Z)-3-hydroxy-1-phenyl-3-decene-1-one, (Z)-3-hydroxy-1-phenyl-2-decene-1-one, 1-(5-hydroxy-3-methyl-1-phenyl-4-pyrazolyl)-1-benzophenone, 4-(1-hydroxyphenylmethylene)-5-methyl-2-benzyl-2,4-dihydro-3-pyrazolone, (Z)-3-hydroxy-1-phenyl-3-dodecene-1-one, 2-hydroxybenzoic acid octyl ester, N,N-dibutyl-2-hydroxybenzamide, etc.
[0011]
[0012] In formulae (IIA) to (IID), R1, R2, and R3 may be the same or different, and are each independently C1-C 15 alkyl or aryl groups, such as methyl, butyl, hexyl, octyl, dodecyl, phenyl, benzyl, phenylbutyl and the like.
[0013] The organic phosphorus may be selected from one or a mixture of two or more of phosphine oxide (IIA), phosphinate (IIB), phosphonate (IIC) and phosphoric acid ester (IID).
[0014] The molar ratio of the carbonyl enol to the organic phosphorus is 10:1-1:10, preferably 1:1-1:4.
[0015] The polar hydrophobic additive refers to a hydrophobic solvent with a certain polarity, which can be one or two or a mixture of alcohol, ketone, ether, ester, etc. The alcohol can be selected from octanol, decanol, dodecanol, etc.; the ketone is, for example, 4-methyl-2-pentanone (MIBK), diisobutyl ketone (DIBK), etc.; the ether is, for example, diamyl ether, dihexyl ether, etc.; the ester is, for example, heptyl acetate, butyl benzoate, etc. The additive content is 0 vol%-30 vol%, based on the total volume of carbonyl enol, organic phosphorus and additive. The polar hydrophobic additive helps to improve the solubility and phase separation effect of organic matter.
[0016] The present invention further relates to a method for efficiently extracting lithium from a lithium-containing solution using the solvent extraction system of the present invention, comprising the following steps:
[0017] (1) dissolving the solvent extraction system according to the present invention in a diluent to prepare an organic phase, wherein the volume concentration of the extraction system is 3 vol% to 95 vol%, based on the total volume of the organic phase;
[0018] (2) measuring the concentration of lithium in the lithium-containing solution to be tested, adding an appropriate amount of alkali thereto to improve the activity of the extraction system in extracting lithium, and obtaining an aqueous phase to be extracted;
[0019] (3) introducing the organic phase prepared in step (1) and the aqueous phase obtained in step (2) into an extraction device to perform a countercurrent extraction reaction to obtain an organic phase loaded with lithium;
[0020] (4) countercurrently washing the lithium-loaded organic phase of step (3) with a washing liquid to obtain a washed organic phase;
[0021] (5) subjecting the organic phase washed in step (4) to countercurrent stripping to obtain a stripped organic phase and a high-purity lithium salt solution;
[0022] (6) The organic phase after stripping is returned to the organic phase storage tank and recycled for countercurrent extraction of lithium.
[0023] In step (1), the diluent is an alkane (such as kerosene, D70 solvent oil, etc.), an aromatic hydrocarbon (such as toluene, S150 solvent oil, etc.), or a mixed solvent thereof.
[0024] In step (2), the alkali is selected from sodium hydroxide, potassium hydroxide, ammonia, sodium carbonate, potassium carbonate or any mixture thereof. The amount of alkali added to the solution is controlled so that the concentration of the alkali is 0.5-3.0 times the molar concentration of lithium, based on the molar concentration of lithium in the lithium-containing solution to be measured.
[0025] In step (3), the extraction equipment may be an extraction clarification tank, an extraction tower or a centrifugal extractor, the extraction stages are 1-20, and the volume ratio of the organic phase to the aqueous phase is 1:50-50:1.
[0026] In step (4), the washing liquid is water, dilute hydrochloric acid or dilute sulfuric acid, and the concentration of the hydrochloric acid or sulfuric acid solution is 0.01-3.0 mol / L; the volume ratio of the organic phase to the washing liquid is 1:50-50:1, and the washing stage is 1-20.
[0027] In step (5), hydrochloric acid solution or sulfuric acid solution is used as the stripping solution, and its concentration is 0.1-12.0 mol / L; the volume ratio of the organic phase to the stripping solution is 1:50-50:1, and the stripping stage is 1-20.
[0028] The lithium recovery rate of the solvent extraction system for efficient lithium extraction of the present invention can reach more than 99%, and the lithium purity can reach more than 99.5%.
[0029] The solvent extraction system for efficiently extracting lithium of the present invention can be advantageously used to extract lithium from a variety of lithium-containing solutions such as salt lake brine, oilfield brine, battery leaching solution, ore leaching solution, lithium precipitation mother liquor, and lithium-containing wastewater.
[0030] Beneficial Effects
[0031] Compared with the prior art, the solvent extraction system of the present invention is a synergistic extraction system based on the mixture of carbonyl enol and organic phosphorus, which has significantly improved stability, eliminates emulsification, and can be recycled for a long time; the total organic matter content (i.e., COD) in the raffinate is low, and the raffinate treatment is simple. The solvent extraction system of the present invention has high reaction activity, can make full use of the alkali in the solution, greatly reduces the alkali consumption in the lithium extraction process, and thus reduces the production cost of lithium salts. The solvent extraction system of the present invention can be advantageously applied to the extraction of lithium from a variety of lithium-containing solutions, and its advantages are particularly significant for the extraction of lithium from low-grade lithium-containing solutions and weakly alkaline lithium-containing solutions. The method of extracting lithium from a lithium-containing solution (for example: a mixed solution of lithium, sodium, potassium (rubidium, cesium)) using the solvent extraction system of the present invention can simultaneously achieve lithium purification and concentration, shorten the process flow, and improve the lithium recovery rate. The solvent extraction system of the present invention is of great significance for making full use of low-grade lithium resources. BRIEF DESCRIPTION OF THE DRAWINGS
[0032] Figure 1 The present invention is a schematic flow diagram of the process of using the solvent extraction system of the present invention to extract, wash and strip from a lithium-containing solution. DETAILED DESCRIPTION
[0033] The following embodiments are provided to illustrate the present invention in more detail, but the present invention is not limited by these embodiments. Within the technical concept of the present invention, those skilled in the art can make various modifications.
[0034] Example 1
[0035] The lithium-containing solution to be treated is salt lake brine. After magnesium is removed by nanofiltration, the resulting solution contains 0.2 g / L lithium, 85 g / L sodium, 8.6 g / L potassium, and trace amounts of magnesium, calcium, rubidium and cesium.
[0036] The organic phase was prepared with 6 vol% (Z)-1-hydroxy-1-phenyl-1-dodecene-3-one, 6 vol% Cyanex 923 (a mixture of alkyl phosphine oxides, in which the alkyl groups are hexyl and octyl) and 88 vol% kerosene. NaOH was added to the lithium-containing solution to make the NaOH concentration 0.04 mol / L to prepare the aqueous phase. The organic phase and the aqueous phase were subjected to 4-stage continuous countercurrent extraction in an extraction and clarification tank at a volume ratio of 1:5 to obtain an organic phase loaded with lithium, and the lithium extraction rate was measured to be >98%. The organic phase loaded with lithium is further washed with 0.3 mol / L hydrochloric acid at a volume ratio of 20:1 in the extraction clarification tank to extract the co-extracted sodium and potassium, washed twice, and the washing liquid is returned to the entrance of the water phase; the washed organic phase is further stripped with 4 mol / L hydrochloric acid at a volume ratio of 20:1 in the extraction clarification tank, stripped twice, to obtain a high-purity lithium chloride solution with a lithium concentration of 18-20 g / L, and its lithium purity is measured to be >99.8%. The organic phase after stripping is returned to the extraction section for recycling. The lithium chloride solution is precipitated with sodium carbonate at 80°C with a stoichiometric ratio of 0.8 times that of lithium to obtain battery-grade lithium carbonate with a purity of >99.8%.
[0037] Example 2
[0038] The lithium-containing solution to be treated is taken from the recycled lithium batteries and is obtained by disassembling, crushing, leaching and removing divalent and trivalent metals. The solution contains 2.7 g / L lithium, 50 g / L sodium, and trace amounts of cobalt, nickel, magnesium, etc.
[0039] 18vol% (Z)-3-hydroxy-1-phenyl-3-decen-1-one, 30vol% TRPO (a mixture of alkyl phosphine oxides, in which the alkyl groups are heptyl and octyl) and 5vol% octanol are dissolved in 47vol% kerosene to form an organic phase. NaOH is added to the lithium-containing solution to make the NaOH concentration 0.45mol / L to form an aqueous phase. The organic phase and the aqueous phase are subjected to three-stage continuous countercurrent extraction in an extraction clarification tank at a volume ratio of 1:1, and the extraction rate of lithium is >99%. The loaded organic phase continues to be washed with 0.2mol / L sulfuric acid in a volume ratio of 10:1 in the extraction clarification tank to extract the co-extracted sodium and potassium, washing for 2 stages, and the washing liquid is returned to the inlet of the aqueous phase; the washed organic phase continues to be stripped with 2mol / L sulfuric acid in a volume ratio of 10:1 in the extraction clarification tank, stripping for 2 stages, and a high-purity Li2SO4 solution with a lithium concentration of 25-27g / L is obtained, and its lithium purity is >99.8%. The organic phase after stripping is returned to the extraction section for recycling. The lithium sulfate solution is precipitated with sodium carbonate at a stoichiometric ratio of 0.8 times the lithium at 80°C to obtain battery-grade lithium carbonate with a purity of 99.8%.
[0040] Example 3
[0041] The solution to be treated is lithium-containing wastewater generated during the battery recycling process, with a lithium concentration of 0.5g / L and a sodium concentration of 48g / L.
[0042] 15vol% (Z)-3-hydroxy-1-phenyl-2-decene-1-one and 20vol% Cyanex 925 (alkyl phosphine oxide containing branched alkyl) are dissolved in 65vol% kerosene to form an organic phase. NaOH is added to the lithium-containing solution to make the NaOH concentration 0.10mol / L to form an aqueous phase. The organic phase and the aqueous phase are subjected to three-stage continuous countercurrent extraction in an extraction clarification tank at a volume ratio of 1:5, and the lithium extraction rate is measured to be >99%. The loaded organic phase continues to be washed with 1.0mol / L hydrochloric acid in a volume ratio of 20:1 in the extraction clarification tank to extract the co-extracted sodium, wash for 2 stages, and the washing liquid is returned to the inlet of the aqueous phase; the washed organic phase continues to be stripped with 8.0mol / L hydrochloric acid in a volume ratio of 20:1 in the extraction clarification tank, stripped for 2 stages, and a LiCl solution with a lithium concentration of 45-50g / L is obtained. The stripped organic phase is returned to the extraction section for recycling. The lithium chloride solution is precipitated with sodium carbonate at 80°C with a stoichiometric ratio of 0.7 times the lithium to obtain battery-grade lithium carbonate with a purity of >99.6%.
[0043] Example 4
[0044] The solution to be treated is a lithium precipitation mother liquor obtained by adding sodium carbonate to a lithium sulfate solution to precipitate lithium carbonate, and contains 3.4 g / L lithium and 46 g / L sodium.
[0045] 18vol% 1-(5-hydroxy-3-methyl-1-phenyl-4-pyrazolyl)-1-benzophenone, 15vol% TOPO (trioctylphosphine oxide) and 5vol% P350 (dimethylheptyl methylphosphonate) are dissolved in 62vol% S150 solvent to form an organic phase. The mother liquor of lithium precipitation does not need to add alkali and is directly used as the aqueous phase. The organic phase and the aqueous phase are subjected to three-stage continuous countercurrent extraction in an extraction clarification tank at a volume ratio of 1:1, and the lithium extraction rate is measured to be >99%. The organic phase loaded with lithium continues to wash the co-extracted sodium with 0.5mol / L hydrochloric acid in the extraction clarification tank at a volume ratio of 10:1, and the washing is repeated for 2 stages, and the washing liquid is returned to the entrance of the aqueous phase; the washed organic phase continues to be stripped with 5mol / L hydrochloric acid in the extraction clarification tank at a volume ratio of 10:1, and the stripping is repeated for 2 stages to obtain a LiCl solution with a lithium concentration of 32-35g / L. The organic phase after stripping is returned to the extraction section for recycling. The lithium chloride solution is precipitated with sodium carbonate at 80°C with a stoichiometric ratio of 0.7 times the lithium to obtain battery-grade lithium carbonate with a purity of >99.6%.
[0046] Example 5
[0047] The solution to be treated is a mixed solution containing 0.12 g / L lithium, 35 g / L sodium and 10 g / L potassium, obtained by nanofiltration of oilfield brine to remove calcium and magnesium.
[0048] 25vol% 4-(1-hydroxyphenylmethylene)-5-methyl-2-benzyl-2,4-dihydro-3-pyrazolone, 20vol% TRPO and 10vol% trioctyl phosphate are dissolved in 45vol% S150 solvent to form an organic phase. NaOH is added to the lithium-containing solution to make the NaOH concentration 0.02mol / L to form an aqueous phase. The organic phase and the aqueous phase are subjected to 4-stage continuous countercurrent extraction in an extraction clarification tank at a volume ratio of 1:50, and the extraction rate of lithium is >98%. The loaded organic phase continues to be washed with 0.8mol / L hydrochloric acid in a volume ratio of 10:1 in the extraction clarification tank for 3 stages, and the washing liquid is returned to the inlet of the aqueous phase; the washed organic phase continues to be back-extracted with 10mol / L hydrochloric acid in a volume ratio of 10:1 in the extraction clarification tank for 2 stages to obtain a LiCl solution with a lithium concentration of 55-60g / L. The organic phase after stripping is returned to the extraction section for recycling. The lithium chloride solution is evaporated and crystallized to obtain a lithium chloride product with a purity of >99.6%.
[0049] Example 6
[0050] The solution to be treated is pharmaceutical wastewater, containing 8.2 g / L lithium and 65 g / L sodium.
[0051] 20vol% (Z)-3-hydroxy-1-phenyl-3-dodecene-1-one, 20vol% TRPO and 15vol% trihexyl phosphate are dissolved in 20vol% kerosene and 25vol% S150 solvent to form an organic phase. NaOH is added to the lithium-containing solution to make the NaOH concentration 1.3mol / L to form an aqueous phase. The organic phase and the aqueous phase are subjected to 4-stage continuous countercurrent extraction in an extraction clarification tank at a volume ratio of 1.5:1, and the lithium extraction rate is measured to be >99%. The organic phase loaded with lithium continues to be washed with 1.0mol / L hydrochloric acid in a volume ratio of 10:1 in the extraction clarification tank to extract the co-extracted sodium, washed for 3 stages, and the washing liquid is returned to the inlet of the aqueous phase; the washed organic phase continues to be stripped with 8mol / L hydrochloric acid in a volume ratio of 10:1 in the extraction clarification tank, stripped for 3 stages, and a LiCl solution with a lithium concentration of 50-55g / L is obtained. The organic phase after stripping is returned to the extraction section for recycling. The lithium chloride solution is evaporated and crystallized to obtain lithium chloride crystals with a purity of >99.6%.
[0052] Example 7
[0053] The solution to be treated is underground brine, which contains 0.26 g / L lithium, 102 g / L sodium, and 24 g / L potassium after nanofiltration to remove calcium and magnesium.
[0054] 15vol% 2-hydroxybenzoic acid octyl ester, 15vol% TRPO and 5vol% tributyl phosphate are dissolved in 65vol% kerosene solvent to form an organic phase. NaOH is added to the lithium-containing solution to make the NaOH concentration 0.045mol / L to form an aqueous phase. The organic phase and the aqueous phase are subjected to three-stage continuous countercurrent extraction in an extraction clarification tank at a volume ratio of 1:15, and the lithium extraction rate is measured to be >99%. The organic phase loaded with lithium continues to be washed with 0.6mol / L hydrochloric acid in a volume ratio of 10:1 in the extraction clarification tank to extract the co-extracted sodium, wash for one stage, and the washing liquid is returned to the entrance of the aqueous phase; the washed organic phase continues to be stripped with 6mol / L hydrochloric acid in a volume ratio of 10:1 in the extraction clarification tank, stripped for two stages, and a LiCl solution with a lithium concentration of 35-39g / L is obtained. The stripped organic phase is returned to the extraction section for recycling. The lithium chloride solution is precipitated with sodium carbonate at 80°C with a stoichiometric ratio of 0.7 times the lithium to obtain battery-grade lithium carbonate with a purity of >99.6%.
[0055] Example 8
[0056] The lithium-containing solution to be treated is old brine from a salt lake. After magnesium is removed by nanofiltration, the resulting solution contains 1.2 g / L lithium, 14 g / L sodium, and 2.5 g / L potassium.
[0057] 20vol% N,N-dibutyl-2-hydroxybenzamide, 20vol% TRPO and 10vol% dimethylheptyl methylphosphonate are dissolved in 50vol% kerosene solvent to form an organic phase. NaOH is added to the lithium-containing solution to make the NaOH concentration 0.2mol / L to form an aqueous phase. The organic phase and the aqueous phase are subjected to three-stage continuous countercurrent extraction in an extraction clarification tank at a volume ratio of 1:4, and the lithium extraction rate is measured to be >99%. The organic phase loaded with lithium continues to be washed with 0.8mol / L hydrochloric acid in a volume ratio of 10:1 in the extraction clarification tank to extract the co-extracted sodium, washing for one stage, and the washing liquid is returned to the inlet of the aqueous phase; the washed organic phase continues to be stripped with 7mol / L hydrochloric acid in a volume ratio of 10:1 in the extraction clarification tank, stripping for two stages to obtain a LiCl solution with a lithium concentration of 45-48g / L. The stripped organic phase is returned to the extraction section for recycling. The lithium chloride solution is precipitated with sodium carbonate at 80°C with a stoichiometric ratio of 0.7 times the lithium to obtain battery-grade lithium carbonate with a purity of >99.6%.
Claims
1. A solvent extraction system for efficient extraction of lithium, comprising a carbonyl enol, an organophosphorus having a structure shown in Formula IIA, IIB, IIC or IID, and an optional polar hydrophobic additive; In formula IIA, IIB, IIC, and IID, R1, R2, and R3 are the same or different and are each independently C1-C 15 An alkyl or aryl group; The carbonyl enol is 1-(5-hydroxy-3-methyl-1-phenyl-4-pyrazolyl)-1-benzophenone, 4-(1-hydroxyphenylmethylene)-5-methyl-2-benzyl-2,4-dihydro-3-pyrazolone, 2-hydroxybenzoic acid octyl ester, N,N-dibutyl-2-hydroxybenzamide; The molar ratio of the carbonyl enol to the organic phosphorus is 10:1-1:
10.
2. The solvent extraction system for efficient lithium extraction according to claim 1, wherein the polar hydrophobic additive is one or two of alcohols, ketones, ethers, esters, and a mixture of multiple thereof.
3. The solvent extraction system for efficient extraction of lithium according to claim 1, wherein the molar ratio of the carbonyl enol to the organophosphorus is 1:1-1:4; and the amount of the additive is 0 vol%-30 vol%, based on the total volume of the carbonyl enol, the organophosphorus and the additive.
4. A method for efficiently extracting lithium using the solvent extraction system according to any one of claims 1 to 3, the method comprising the following steps: (1) dissolving the solvent extraction system according to any one of claims 1 to 3 in a diluent to prepare an organic phase, wherein the volume concentration of the extraction system is 3 vol% to 95 vol%, based on the total volume of the organic phase; (2) measuring the lithium concentration in the lithium-containing solution to be tested, adding an appropriate amount of alkali thereto, and obtaining an aqueous phase to be extracted; (3) introducing the organic phase prepared in step (1) and the aqueous phase obtained in step (2) into an extraction device to perform a countercurrent extraction reaction to obtain an organic phase loaded with lithium; (4) countercurrently washing the lithium-loaded organic phase of step (3) with a washing liquid to obtain a washed organic phase; (5) subjecting the organic phase washed in step (4) to countercurrent stripping to obtain a stripped organic phase and a high-purity lithium salt solution; (6) The organic phase after stripping is returned to the organic phase storage tank and recycled for countercurrent extraction of lithium.
5. The method according to claim 4, wherein in step (1), the diluent is an alkane, an aromatic hydrocarbon or a mixture thereof; in step (2), the alkali is sodium hydroxide, potassium hydroxide, aqueous ammonia, sodium carbonate, potassium carbonate or a mixture thereof, and the amount of alkali added to the solution is controlled so that the concentration of the alkali is 0.5-3.0 times the molar concentration of lithium, based on the molar concentration of lithium in the lithium-containing solution to be measured.
6. The method according to claim 4, wherein in step (3), the volume ratio of the organic phase to the aqueous phase is 1:50-50:
1.
7. The method according to claim 4, wherein in step (4), the washing liquid is water, dilute hydrochloric acid or dilute sulfuric acid, the concentration of hydrochloric acid or sulfuric acid is 0.01-3.0 mol / L; and the volume ratio of the organic phase to the washing liquid is 1:50-50:
1.
8. The method according to claim 4, wherein in step (5), hydrochloric acid solution or sulfuric acid solution is used as the stripping solution, the concentration of hydrochloric acid or sulfuric acid is 0.1-12.0 mol / L; and the volume ratio of the organic phase to the stripping solution is 1:50-50:
1.
9. Use of the solvent extraction system for efficient lithium extraction according to any one of claims 1 to 3 for extracting lithium from salt lake brine, oil field brine, battery leachate, ore leachate, lithium precipitation mother liquor, and lithium-containing wastewater.
Citation Information
Cited By
Short-distance and efficient electrochemical method for extracting lithium from original halogen and application of short-distance and efficient electrochemical method
CN121294885A