Bamboo charcoal fiberboard and preparation method thereof

By adopting the design of honeycomb filled skeleton and porous structure in the bamboo charcoal fiber board, the problem of poor elasticity of the existing bamboo charcoal fiber board is solved, and better ability to absorb formaldehyde and noise is achieved. It is suitable for a variety of decoration and sound-absorbing materials.

CN115847964BActive Publication Date: 2024-10-01HUBEI YISEN BUILDING MATERIALS TECHNOLOGY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211560904.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-12-07
Publication Date
2024-10-01
Estimated Expiration
2042-12-07

AI Technical Summary

Technical Problem

Existing bamboo charcoal fiberboards are easily dented after being impacted, have poor elasticity, and cannot effectively absorb noise and harmful gases.

Method used

A foamed aluminum plate is used as the base lining plate, and a honeycomb filling skeleton is set along the circumferential edge of the foamed aluminum plate. The interior is filled with resin, paraffin wax and bamboo charcoal powder to form a porous structure, and paraffin is precipitated at a temperature of 80-120°C to form a roughly circular hollow. The porous structure, resin and bamboo charcoal powder serve as the supporting structure, and the elastic modulus is set at 10%-25%.

Benefits of technology

The elasticity and adsorption capacity of the bamboo charcoal fiber board are improved, and it can effectively absorb formaldehyde and noise. The elasticity rate is between 10% and 25%, and it is suitable for a variety of decoration and sound-absorbing materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115847964B_ABST
    Figure CN115847964B_ABST
Patent Text Reader

Abstract

The present invention provides a bamboo charcoal fiberboard and a preparation method, wherein the bamboo charcoal fiberboard comprises: a foamed aluminum plate as a base lining plate, a honeycomb filling skeleton integrated with the foamed aluminum plate is arranged along the inner side of the circumferential edge of the foamed aluminum plate; a filling layer mainly composed of resin, paraffin and bamboo charcoal powder is arranged inside the filling skeleton, and after filling and shaping, it is inverted and placed in a precipitation device at a temperature of 80-120°C to melt and precipitate the paraffin; after the paraffin is precipitated, the temperature is lowered to 60-80°C for stabilization for 2-4 hours, and when the filling layer is stabilized, a decorative layer is bonded to the upper part of the filling layer. By constructing a porous structure, the formed bamboo charcoal fiberboard has strong adsorption, and the adsorption has two aspects, one is that the porous structure composed of bamboo charcoal has a strong effect of adsorbing formaldehyde, which has the same mechanism as activated carbon; the other is that the porous structure has a good ability to absorb noise.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of bamboo charcoal fiberboards, in particular to a bamboo charcoal fiberboard and a preparation method thereof. Background Art

[0002] The existing bamboo charcoal fiberboard is basically made by putting resin, bamboo charcoal, stabilizer and binder into an extruder to extrude the bamboo charcoal fiberboard. The bamboo charcoal fiberboard obtained in this way has good density and high strength, is a good choice for decorative materials, and has a wide range of uses, such as interior decoration, train set (motor vehicle, train and subway) decoration, car decoration, etc.; but the disadvantage is that it has poor elasticity and the surface is easily dented after being impacted. Summary of the invention

[0003] In view of this, the main purpose of the present invention is to provide a bamboo charcoal fiberboard and a preparation method thereof.

[0004] The technical solution adopted by the present invention is as follows:

[0005] Bamboo charcoal fiberboard, including:

[0006] A foamed aluminum plate is used as a base lining plate, and a honeycomb filling frame integrated with the foamed aluminum plate is arranged along the inner side of the circumferential edge of the foamed aluminum plate;

[0007] A filling layer mainly composed of resin, paraffin and bamboo charcoal powder is arranged inside the filling frame. After filling and shaping, it is placed upside down in a precipitation device at a temperature of 80-120°C to melt the paraffin and precipitate; after the paraffin is precipitated, the temperature is lowered to 60-80°C to stabilize the shape for 2-4 hours.

[0008] After the filler layer is stabilized, a decorative layer is bonded on the upper part of the filler layer.

[0009] Furthermore, after the paraffin is precipitated from the filling layer, a roughly circular hollow porous structure is formed; and the porous structure uses resin and bamboo charcoal powder as a supporting structure body.

[0010] Furthermore, the ratio of the resin to the bamboo charcoal powder is 3:1-1.5.

[0011] Furthermore, the porous structure has a set elastic modulus, and the elastic modulus is set such that when the porous structure is squeezed, the deformation amount of the porous structure is between 10% and 25%.

[0012] The present invention also provides a method for preparing a bamboo charcoal fiberboard, comprising the following steps:

[0013] Step 1) preparing a base lining plate for standby use: using a foamed aluminum plate as the base lining plate, and arranging a honeycomb filling frame integrated with the foamed aluminum plate along the inner side of the circumferential edge of the foamed aluminum plate;

[0014] Step 2) beating the paraffin into paraffin particles for later use;

[0015] Step 3) placing the resin in a processing tank to melt and then keep warm, adding bamboo charcoal powder and stirring thoroughly; then adding paraffin particles and stirring thoroughly to form a filling mixture;

[0016] Step 4) placing the base liner in a mold, and then filling the filling mixture into the mold to cool and shape to form a prefabricated board;

[0017] Step 5) After cooling and shaping, the prefabricated board is taken out from the mold, and then the prefabricated board is placed upside down in a precipitation device at a temperature of 80-120°C to melt the paraffin and precipitate; after the paraffin is precipitated, the temperature is lowered to 60-80°C to stabilize for 2-4 hours.

[0018] Step 6) After the filler layer is stabilized, a decorative layer is bonded on top of the filler layer.

[0019] Further, in step 3), the temperature of the treatment tank is first raised to 200-220°C, and the resin is added to be completely melted;

[0020] After it is completely melted, the temperature drops to 170-190℃, then add the bamboo charcoal powder and stir thoroughly;

[0021] The temperature was lowered to 170-180°C and the paraffin wax pellets were added and stirred thoroughly to form a filling mixture.

[0022] Furthermore, in step 4), the mold is a continuous open mold.

[0023] The open mold comprises: a mold body, a plurality of grooves corresponding to the specifications of the base lining plate are opened inside the mold body, the top of the groove is open; and there are isolation plates between the grooves.

[0024] Furthermore, in step 3), the usage ratio of the resin, bamboo charcoal powder and paraffin is 3:1-1.5:0.6-0.8.

[0025] Furthermore, in step 5), the prefabricated plate is placed in a precipitation device at a temperature of 80-120° C. to melt the paraffin and precipitate;

[0026] After the paraffin wax is precipitated, a roughly circular hollow porous structure is formed;

[0027] The porous structure uses resin and bamboo charcoal powder as the main supporting structure.

[0028] Furthermore, the porous structure has a set elastic modulus, and the elastic modulus is set such that when the porous structure is squeezed, the deformation amount of the porous structure is between 10% and 25%.

[0029] In the present application, a new preparation process is adopted, in which a foamed aluminum plate is used as a base lining plate, and a honeycomb filling skeleton which is integrated with the foamed aluminum plate is arranged along the inner side of the circumferential edge of the foamed aluminum plate; a filling layer with resin, paraffin and bamboo charcoal powder as the main body is arranged inside the filling skeleton, and after filling and shaping, it is inverted and placed in a precipitation device at a temperature of 80-120°C to melt the paraffin and precipitate it; after the paraffin is precipitated, the temperature is lowered to 60-80°C to stabilize for 2-4 hours, and after the paraffin is precipitated from the filling layer, a roughly circular hollow porous structure is formed; and the porous structure uses resin and bamboo charcoal powder as the main supporting structure; the porous structure has a set elastic modulus, and the elastic modulus is set as follows: when the porous structure is squeezed, the deformation amount of the porous structure caused is between 10% and 25%.

[0030] By constructing a porous structure, the formed bamboo charcoal fiberboard has strong adsorption. The adsorption has two aspects. First, the porous structure composed of bamboo charcoal has a strong effect of adsorbing formaldehyde, which has the same mechanism as activated carbon; second, the porous structure has a good ability to adsorb noise. BRIEF DESCRIPTION OF THE DRAWINGS

[0031] The following drawings are only used to illustrate and explain the present invention, and are not used to limit the scope of the present invention, wherein:

[0032] Figure 1 It is a structural schematic diagram of the bamboo charcoal fiberboard of the present invention;

[0033] Figure 2 It is a schematic structural diagram of the filling skeleton of the present invention. DETAILED DESCRIPTION

[0034] In order to make the purpose, technical solution, design method and advantages of the present invention clearer, the present invention is further described in detail by specific embodiments in conjunction with the accompanying drawings. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.

[0035] Embodiment 1, the present application provides a bamboo charcoal fiberboard, comprising:

[0036] A foamed aluminum plate is used as a base lining plate, and a honeycomb filling frame integrated with the foamed aluminum plate is arranged along the inner side of the circumferential edge of the foamed aluminum plate;

[0037] A filling layer mainly composed of resin, paraffin and bamboo charcoal powder is arranged inside the filling frame. After filling and shaping, it is placed upside down in a precipitation device at a temperature of 80-120°C to melt the paraffin and precipitate; after the paraffin is precipitated, the temperature is lowered to 60-80°C to stabilize the shape for 2-4 hours.

[0038] After the filler layer is stabilized, a decorative layer is bonded on the upper part of the filler layer.

[0039] After the paraffin is precipitated from the filling layer, a roughly circular hollow porous structure is formed; and the porous structure uses resin and bamboo charcoal powder as a supporting structure body.

[0040] The ratio of the resin to the bamboo charcoal powder is 3:1-1.5.

[0041] The porous structure has a set elastic modulus, and the elastic modulus is set such that when the porous structure is squeezed, the deformation amount of the porous structure is between 10% and 25%.

[0042] Reference Figure 1 , Figure 1 The invention describes a bamboo charcoal fiberboard, which includes a base lining board 5, a honeycomb filling frame 4 is arranged on the upper part of the base lining board 5; a filling layer 2 mainly composed of resin and bamboo charcoal powder is filled in the filling frame 4; and a decorative layer 1 is arranged on the upper part of the filling layer. There are certain gaps 3 between the filling frames 4, and the setting of the gaps 3 helps to effectively absorb formaldehyde and noise to the filling layer with a porous structure.

[0043] Embodiment 2, the present application provides a method for preparing a bamboo charcoal fiberboard, comprising the following steps:

[0044] Step 1) preparing a base lining plate for standby use: using a foamed aluminum plate as the base lining plate, and arranging a honeycomb filling frame integrated with the foamed aluminum plate along the inner side of the circumferential edge of the foamed aluminum plate;

[0045] Step 2) beating the paraffin into paraffin particles for later use;

[0046] Step 3) placing the resin in a processing tank to melt and then keep warm, adding bamboo charcoal powder and stirring thoroughly; then adding paraffin particles and stirring thoroughly to form a filling mixture;

[0047] Step 4) placing the base liner in a mold, and then filling the filling mixture into the mold to cool and shape to form a prefabricated board;

[0048] Step 5) After cooling and shaping, the prefabricated board is taken out from the mold, and then the prefabricated board is placed upside down in a precipitation device at a temperature of 80°C to melt the paraffin and precipitate; after the paraffin is precipitated, the temperature is lowered to 60°C to stabilize for 2 hours.

[0049] Step 6) After the filler layer is stabilized, a decorative layer is bonded on top of the filler layer.

[0050] In step 3), the temperature of the treatment tank is first raised to 200°C, and the resin is added to completely melt it;

[0051] After it is completely melted, the temperature drops to 170°C, then add the bamboo charcoal powder and stir thoroughly;

[0052] The temperature was lowered to 170°C and the paraffin wax pellets were added and stirred thoroughly to form a filling mixture.

[0053] In step 4), the mold is a continuous open mold.

[0054] The open mold comprises: a mold body, a plurality of grooves corresponding to the specifications of the base lining plate are opened inside the mold body, the top of the groove is open; and there are isolation plates between the grooves.

[0055] Furthermore, in step 3), the usage ratio of the resin, bamboo charcoal powder and paraffin is 3:1:0.6.

[0056] In step 5), the prefabricated plate is placed in a precipitation device at a temperature of 80° C. to melt the paraffin and precipitate;

[0057] After the paraffin wax is precipitated, a roughly circular hollow porous structure is formed;

[0058] The porous structure uses resin and bamboo charcoal powder as the main supporting structure.

[0059] After testing, the porous structure has a set elastic modulus, and the elastic modulus is set as follows: when the porous structure is squeezed by a set pressure, 400-800N pressure, the maximum deformation amount of the porous structure caused is 25%.

[0060] Embodiment 3, the present application provides a method for preparing a bamboo charcoal fiberboard, comprising the following steps:

[0061] Step 1) preparing a base lining plate for standby use: using a foamed aluminum plate as the base lining plate, and arranging a honeycomb filling frame integrated with the foamed aluminum plate along the inner side of the circumferential edge of the foamed aluminum plate;

[0062] Step 2) beating the paraffin into paraffin particles for later use;

[0063] Step 3) placing the resin in a processing tank to melt and then keep warm, adding bamboo charcoal powder and stirring thoroughly; then adding paraffin particles and stirring thoroughly to form a filling mixture;

[0064] Step 4) placing the base liner in a mold, and then filling the filling mixture into the mold to cool and shape to form a prefabricated board;

[0065] Step 5) After cooling and shaping, the prefabricated board is taken out from the mold, and then the prefabricated board is placed upside down in a precipitation device at a temperature of 120°C to melt the paraffin and precipitate; after the paraffin is precipitated, the temperature is lowered to 80°C to stabilize for 4 hours.

[0066] Step 6) After the filler layer is stabilized, a decorative layer is bonded on top of the filler layer.

[0067] In step 3), the temperature of the treatment tank is first raised to 220°C, and the resin is added to completely melt it;

[0068] After it is completely melted, the temperature drops to 1190°C, then add the bamboo charcoal powder and stir thoroughly;

[0069] The temperature was lowered to 1180°C and the paraffin wax particles were added and stirred thoroughly to form a filling mixture.

[0070] In step 4), the mold is a continuous open mold.

[0071] The open mold comprises: a mold body, a plurality of grooves corresponding to the specifications of the base lining plate are opened inside the mold body, the top of the groove is open; and there are isolation plates between the grooves.

[0072] Furthermore, in step 3), the usage ratio of the resin, bamboo charcoal powder and paraffin is 3:1.5:0.8.

[0073] In step 5), the prefabricated plate is placed in a precipitation device at a temperature of 120° C. to melt the paraffin and precipitate;

[0074] After the paraffin wax is precipitated, a roughly circular hollow porous structure is formed;

[0075] The porous structure uses resin and bamboo charcoal powder as the main supporting structure.

[0076] After testing, the porous structure has a set elastic modulus, which is set as follows: when the porous structure is squeezed by a set pressure, 400-800N pressure, the maximum deformation of the porous structure is 15%, and the minimum deformation is 10%.

[0077] Embodiment 4, the present application provides a method for preparing a bamboo charcoal fiberboard, comprising the following steps:

[0078] Step 1) preparing a base lining plate for standby use: using a foamed aluminum plate as the base lining plate, and arranging a honeycomb filling frame integrated with the foamed aluminum plate along the inner side of the circumferential edge of the foamed aluminum plate;

[0079] Step 2) beating the paraffin into paraffin particles for later use;

[0080] Step 3) placing the resin in a processing tank to melt and then keep warm, adding bamboo charcoal powder and stirring thoroughly; then adding paraffin particles and stirring thoroughly to form a filling mixture;

[0081] Step 4) placing the base liner in a mold, and then filling the filling mixture into the mold to cool and shape to form a prefabricated board;

[0082] Step 5) After cooling and shaping, the prefabricated board is taken out from the mold, and then the prefabricated board is placed upside down in a precipitation device at a temperature of 100°C to melt the paraffin and precipitate; after the paraffin is precipitated, the temperature is lowered to 70°C to stabilize for 3 hours.

[0083] Step 6) After the filler layer is stabilized, a decorative layer is bonded on top of the filler layer.

[0084] In step 3), the temperature of the treatment tank is first raised to 210°C, and the resin is added to completely melt it;

[0085] After it is completely melted, the temperature drops to 180°C, then add the bamboo charcoal powder and stir thoroughly;

[0086] The temperature was lowered to 175°C and the paraffin wax pellets were added and stirred thoroughly to form a filling mixture.

[0087] In step 4), the mold is a continuous open mold.

[0088] The open mold comprises: a mold body, a plurality of grooves corresponding to the specifications of the base lining plate are opened inside the mold body, the top of the groove is open; and there are isolation plates between the grooves.

[0089] Furthermore, in step 3), the usage ratio of the resin, bamboo charcoal powder and paraffin is:

[0090]

[0091] In step 5), the prefabricated plate is placed in a precipitation device at a temperature of 100° C. to melt the paraffin and precipitate;

[0092] After the paraffin wax is precipitated, a roughly circular hollow porous structure is formed;

[0093] The porous structure uses resin and bamboo charcoal powder as the main supporting structure.

[0094] After testing, the porous structure has a set elastic modulus, which is set as follows: when the porous structure is squeezed by a set pressure, 400-800N pressure, the maximum deformation of the porous structure is 20%, and the minimum deformation is 15%.

[0095] Embodiment 5, the present application provides a method for preparing a bamboo charcoal fiberboard, comprising the following steps:

[0096] Step 1) preparing a base lining plate for standby use: using a foamed aluminum plate as the base lining plate, and arranging a honeycomb filling frame integrated with the foamed aluminum plate along the inner side of the circumferential edge of the foamed aluminum plate;

[0097] Step 2) beating the paraffin into paraffin particles for later use;

[0098] Step 3) placing the resin in a processing tank to melt and then keep warm, adding bamboo charcoal powder and stirring thoroughly; then adding paraffin particles and stirring thoroughly to form a filling mixture;

[0099] Step 4) placing the base liner in a mold, and then filling the filling mixture into the mold to cool and shape to form a prefabricated board;

[0100] Step 5) After cooling and shaping, the prefabricated board is taken out from the mold, and then the prefabricated board is placed upside down in a precipitation device at a temperature of 115°C to melt the paraffin and precipitate; after the paraffin is precipitated, the temperature is lowered to 75°C to stabilize the shape for 3.5 hours.

[0101] Step 6) After the filler layer is stabilized, a decorative layer is bonded on top of the filler layer.

[0102] In step 3), the temperature of the treatment tank is first raised to 215°C, and the resin is added to completely melt it;

[0103] After it is completely melted, the temperature drops to 185°C, then add the bamboo charcoal powder and stir thoroughly;

[0104] The temperature was lowered to 178°C and the paraffin wax pellets were added and stirred thoroughly to form a filling mixture.

[0105] In step 4), the mold is a continuous open mold.

[0106] The open mold comprises: a mold body, a plurality of grooves corresponding to the specifications of the base lining plate are opened inside the mold body, the top of the groove is open; and there are isolation plates between the grooves.

[0107] Furthermore, in step 3), the usage ratio of the resin, bamboo charcoal powder and paraffin is 3:1.3:0.75.

[0108] In step 5), the prefabricated plate is placed in a precipitation device at a temperature of 115° C. to melt the paraffin and precipitate;

[0109] After the paraffin wax is precipitated, a roughly circular hollow porous structure is formed;

[0110] The porous structure uses resin and bamboo charcoal powder as the main supporting structure.

[0111] After testing, the porous structure has a set elastic modulus, which is set as follows: when the porous structure is squeezed by a set pressure, 400-800N pressure, the maximum deformation of the porous structure is 23%, and the minimum deformation is 18%.

[0112] Examples 1-4 provide different usage ratios of resin and bamboo charcoal powder, and obtain different deformation amounts. However, in different applications, reasonable matching should be carried out.

[0113] By constructing a porous structure, the formed bamboo charcoal fiberboard has strong adsorption. The adsorption has two aspects. First, the porous structure composed of bamboo charcoal has a strong effect of adsorbing formaldehyde, which has the same mechanism as activated carbon; second, the porous structure has a good ability to adsorb noise.

[0114] If you want to enhance the adsorption of formaldehyde, you need to add a slightly larger amount of bamboo charcoal powder, but the corresponding elasticity will be worse.

[0115] In the present application, a honeycomb filling skeleton is arranged on the foamed aluminum plate; the honeycomb filling skeleton divides the filling layer into several units, and the units are not associated with each other, so that each unit exists independently; therefore, the filling layer is actually composed of multiple independent units filled with resin, paraffin and bamboo charcoal powder as the main body. The advantage of this arrangement is that when precipitation is carried out in the precipitation device, the filling layer is placed downward, and after the filling layer is heated, the paraffin is melted, and then precipitated from each independent unit under the action of gravity; the independent unit speeds up the precipitation process. It is beneficial to the efficiency of board formation.

[0116] It should be pointed out that in the present application, the processing tank can be a commonly used temperature-controlled stirring tank; the precipitation device can be a drying tunnel furnace, and the precipitated paraffin can be reused after condensation.

[0117] In the present application, the resin refers to commonly used ABS resin.

[0118] In the present application, a new preparation process is adopted, in which a foamed aluminum plate is used as a base lining plate, and a honeycomb filling skeleton which is integrated with the foamed aluminum plate is arranged along the inner side of the circumferential edge of the foamed aluminum plate; a filling layer with resin, paraffin and bamboo charcoal powder as the main body is arranged inside the filling skeleton, and after filling and shaping, it is inverted and placed in a precipitation device at a temperature of 80-120°C to melt the paraffin and precipitate it; after the paraffin is precipitated, the temperature is lowered to 60-80°C to stabilize for 2-4 hours, and after the paraffin is precipitated from the filling layer, a roughly circular hollow porous structure is formed; and the porous structure uses resin and bamboo charcoal powder as the main supporting structure; the porous structure has a set elastic modulus, and the elastic modulus is set as follows: when the porous structure is squeezed, the deformation amount of the porous structure caused is between 10% and 25%.

[0119] The present application also provides a method for continuously preparing prefabricated panels;

[0120] The embodiments of the present invention have been described above, and the above description is exemplary, not exhaustive, and is not limited to the disclosed embodiments. Many modifications and variations will be apparent to those of ordinary skill in the art without departing from the scope and spirit of the described embodiments. The selection of terms used herein is intended to best explain the principles of the embodiments, practical applications, or technical improvements in the market, or to enable other persons of ordinary skill in the art to understand the embodiments disclosed herein.

Claims

1. Bamboo charcoal fiberboard, characterized in that: include: A foamed aluminum plate is used as a base lining plate, and a honeycomb filling frame integrated with the foamed aluminum plate is arranged along the inner side of the circumferential edge of the foamed aluminum plate; A filling layer mainly composed of resin, paraffin and bamboo charcoal powder is arranged inside the filling frame. After filling and shaping, it is placed upside down in the precipitation device, and the paraffin is melted and precipitated at a temperature of 80-120°C; after the paraffin is precipitated, the temperature is lowered to 60-80°C to stabilize for 2-4 hours. When the filler layer is stabilized, a decorative layer is bonded on the upper part of the filler layer; After the paraffin is separated out from the filler layer, a roughly circular hollow porous structure is formed; and the porous structure uses resin and bamboo charcoal powder as the main supporting structure.

2. The bamboo charcoal fiberboard according to claim 1, characterized in that: The mass ratio of the resin to the bamboo charcoal powder is 3:1-1.

5.

3. The bamboo charcoal fiberboard according to claim 1, characterized in that: The porous structure has a set elastic modulus, and the elastic modulus is set such that when the porous structure is squeezed, the deformation amount of the porous structure is between 10% and 25%.

4. A method for preparing a bamboo charcoal fiberboard, characterized in that: The steps include: Step 1) Prepare a base lining plate for standby use: a foamed aluminum plate is used as the base lining plate, and a honeycomb filling frame integrated with the foamed aluminum plate is arranged along the inner side of the circumferential edge of the foamed aluminum plate; Step 2) Beat the paraffin into paraffin particles for later use; Step 3) placing the resin in a processing tank to melt and then keep warm, adding bamboo charcoal powder and stirring thoroughly; then adding paraffin particles and stirring thoroughly to form a filling mixture; Step 4) placing the base liner in the mold, and then filling the filling mixture into the filling skeleton to cool and shape to form a prefabricated board; Step 5) After cooling and shaping, the prefabricated board is taken out from the mold, and then the prefabricated board is placed upside down in the precipitation device, and the paraffin is melted and precipitated at a temperature of 80-120°C; after the paraffin is precipitated, the temperature is lowered to 60-80°C to stabilize for 2-4 hours. Step 6) After the filler layer is stabilized, a decorative layer is bonded on the upper part of the filler layer; In step 3), the temperature of the treatment tank is first raised to 200-220°C, and the resin is added to completely melt it; After it is completely melted, the temperature drops to 170-190℃, then add the bamboo charcoal powder and stir thoroughly; Lower the temperature to 170-180°C, add the paraffin wax particles and stir thoroughly to form a filling mixture; In step 4), the mold is a continuous open mold. The open mold includes: a mold body, a plurality of slots corresponding to the specifications of the base liner are opened inside the mold body, the top of the slot is open; and there are isolation plates between the slots; The mass ratio of the resin, bamboo charcoal powder and paraffin is: 3:1-1.5:0.6-0.8; In step 5), the prefabricated plate is placed in a precipitation device, and the paraffin is melted and precipitated at a temperature of 80-120°C; After the paraffin wax is precipitated, a roughly circular hollow porous structure is formed; The porous structure uses resin and bamboo charcoal powder as the main supporting structure.

5. The method for preparing the carbon fiber board according to claim 4, characterized in that: The porous structure has a set elastic modulus, and the elastic modulus is set such that when the porous structure is squeezed, the deformation amount of the porous structure is between 10% and 25%.