Phase change material as well as preparation method and application thereof

By using dual melting point phase change materials and thermal reinforcement in the battery system, the problem of insufficient thermal management effect of the battery system in different temperature ranges is solved, and the temperature uniformity and safety are improved, which extends the battery life and enhances safety. sex.

CN118978894APending Publication Date: 2024-11-19GUANGDONG UNIV OF TECH
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202411048824.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-01
Publication Date
2024-11-19

AI Technical Summary

Technical Problem

The thermal management effect of existing phase change materials in different temperature ranges is insufficient, resulting in temperature unevenness and safety problems of the battery system.

Method used

Using a double melting point phase change material composed of low melting point paraffin and high melting point paraffin, combined with a thermal reinforcement and flame retardant, it is prepared by melting and mixing to form a phase change material with excellent thermal stability and thermal conductivity for power batteries. Thermal safety management of modules.

Benefits of technology

It realizes effective heat management within different temperature ranges, improves the temperature uniformity and safety of the battery system, significantly extends the battery life, and provides additional thermal buffering under high temperature conditions, enhancing the safety of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118978894A_ABST
    Figure CN118978894A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of new energy automobile battery thermal safety, in particular to a phase change material and a preparation method and application thereof. The invention provides a phase change material, which is prepared from the following raw materials in percentage by mass: 60 to 80 percent of phase change matrix, 8 to 12 percent of supporting framework, 1 to 5 percent of heat conduction enhancer and 10 to 25 percent of flame retardant, the phase change matrix comprises low-melting-point paraffin and high-melting-point paraffin; the melting point of the high-melting-point paraffin is higher than that of the low-melting-point paraffin. The phase change material can effectively manage heat in different temperature intervals, and the temperature uniformity and safety of a battery system are improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of thermal safety technology of new energy vehicle batteries, and in particular to a phase change material and a preparation method and application thereof. Background Art

[0002] As the endurance of new energy electric vehicles continues to improve, the specifications and charge and discharge rates of power battery modules are also increasing, bringing new challenges to the development of new energy electric vehicles. If the large amount of heat released by the power battery module during the charging and discharging process cannot be dissipated in time, the overheating phenomenon will accelerate the performance degradation of the power battery, significantly shorten the service life, and even cause thermal safety problems such as spontaneous combustion and explosion. Therefore, limited thermal safety of power battery modules is one of the key factors for the further development of new energy electric vehicles.

[0003] In addition, as an emerging passive battery thermal safety (BTM) technology, phase change material (PCM) can absorb or release a large amount of latent heat during the phase change process, timely absorb the heat generated by the battery and diffuse it into the surrounding environment, thereby stabilizing the internal temperature of the battery. Compared with traditional BTM (air cooling and liquid cooling), phase change energy storage has the advantages of high energy storage density, small size, small temperature change, low cost, and easy matching with the operating system.

[0004] For example, the Chinese patent application number 202310287510.0 discloses a phase change wax phase change material suitable for battery thermal safety, which includes 67% of matrix, 1-8% of elastomer, 1-10% of thermal conductor, 5-30% of flame retardant and 0.5-5% of reinforcing agent by mass percentage; the matrix is ​​one or a combination of No. 52 paraffin, No. 50 paraffin, No. 48 paraffin, No. 54 paraffin, No. 56 paraffin, No. 58 paraffin, No. 50 Fischer-Tropsch wax, No. 52 Fischer-Tropsch wax and No. 54 Fischer-Tropsch wax. The improved new phase change wax phase change material has good high enthalpy value, flame retardancy, thermal conductivity, non-corrosiveness and excellent precipitation resistance, and can be used in lithium battery packs, power batteries and other phase change materials. Chinese patent application number 202211252923.7 discloses a phase change material for a lithium-ion battery thermal safety system, which includes, by mass percentage, 85-92% sodium acetate trihydrate, 3-5% cellulose, and 5-10% silicone potting glue. However, the thermal management effect of the above technical solution in different temperature ranges needs to be improved. Summary of the invention

[0005] The object of the present invention is to provide a phase change material and a preparation method and application thereof, wherein the phase change material can effectively manage heat in different temperature ranges and improve the temperature uniformity and safety of a battery system.

[0006] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:

[0007] The present invention provides a phase change material, which comprises the following raw materials according to the percentage by mass: 60-80% of a phase change matrix, 8-12% of a support skeleton, 1-5% of a thermal conductivity enhancer and 10-25% of a flame retardant;

[0008] The phase change matrix includes low melting point paraffin and high melting point paraffin; the high melting point paraffin has a melting point greater than the low melting point paraffin.

[0009] Preferably, the mass ratio of the low melting point paraffin wax to the high melting point paraffin wax is (1-4):(1-4).

[0010] Preferably, the low melting point paraffin includes one or more of PCM44, PCM46 and PCM48;

[0011] The high melting point paraffin wax includes one or more of PCM116, PCM118 and PCM120.

[0012] Preferably, the material of the supporting skeleton includes one or more of thermoplastic elastic styrene-butadiene rubber, epoxy resin and styrene-butadiene-styrene block copolymer.

[0013] Preferably, the thermal conductivity enhancer includes one or more of expanded graphite, boron nitride and aluminum nitride.

[0014] Preferably, the flame retardant comprises ammonium polyphosphate and / or aluminum hypophosphite.

[0015] Preferably, when the flame retardant comprises ammonium polyphosphate and aluminum hypophosphite, the mass ratio of the ammonium polyphosphate to the aluminum hypophosphite is (1-2): (1-2).

[0016] The present invention also provides a method for preparing the phase change material described in the above technical solution, comprising the following steps:

[0017] The phase change matrix is ​​melted and then mixed with a supporting skeleton, a thermal conductivity enhancer and a flame retardant to obtain the phase change material.

[0018] Preferably, the melting temperature is 130-180°C.

[0019] The present invention also provides the use of the phase change material described in the above technical solution or the phase change material prepared by the preparation method described in the above technical solution in a power battery module.

[0020] The present invention provides a phase change material, which includes the following raw materials according to the percentage by mass: 60-80% of a phase change matrix, 8-12% of a supporting skeleton, 1-5% of a thermal conductivity enhancer and 10-25% of a flame retardant; the phase change matrix includes a low melting point paraffin and a high melting point paraffin; the melting point of the high melting point paraffin is greater than that of the low melting point paraffin. The present invention adopts a dual melting point material, wherein the low melting point material is used for daily thermal management, and the high melting point material is used to delay thermal runaway, thereby providing a wider range of temperature management capabilities; and by adding a flame retardant, the phase change material has flame retardant properties, further improving the safety of the battery. The thermal conductivity enhancer plays a role in improving the thermal conductivity of the phase change polymer. Therefore, the phase change material of the present invention can effectively manage heat in different temperature ranges and improve the temperature uniformity and safety of the battery system.

[0021] Compared with the prior art, the technical solution of the present invention has the following beneficial effects: the phase change material of the present invention has excellent thermal stability and intrinsic anti-leakage performance, and at the same time has good heat storage and thermal conductivity. When applied to battery thermal safety technology, it exhibits good temperature control capability for battery modules, ensuring that the battery is in a suitable operating temperature range, reflecting good application effects and market prospects.

[0022] The present invention also provides a method for preparing the phase change material of the above technical solution, comprising the following steps: after melting the phase change matrix, mixing it with a supporting skeleton, a thermal conductivity enhancer and a flame retardant to obtain the phase change material. The preparation method of the present invention is simple, one-step forming, short reaction time, and the raw materials used are cheap and easy to obtain, environmentally friendly, and the reaction conditions do not require high temperature and high pressure or environmental atmosphere requirements, and can achieve mass production, which has great potential for practical engineering applications. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] Figure 1 It is a schematic diagram of the preparation process of the phase change material described in Examples 1 to 5;

[0024] Figure 2 The mass loss curves of the phase change materials of Comparative Example 1 and Examples 1 to 5 when heated at 70° C. for 25 hours;

[0025] Figure 3 Schematic diagram of shape stability test of the phase change materials of Comparative Example 1 and Examples 1 to 5 when heated at 70° C. for 25 hours;

[0026] Figure 4 The heating plate curves of the phase change material and the blank heating plate described in Example 2;

[0027] Figure 5 This is an infrared image of the phase change material and a blank heating plate described in Example 2;

[0028] Figure 6Schematic diagram of the battery thermal safety system obtained from the application example; wherein 1-battery, 2-connector, 3-phase change material;

[0029] Figure 7 The thermal management temperature curve diagram of the battery module of the phase change material described in Comparative Example 1 and Example 2;

[0030] Figure 8 The temperature difference bar graph of the battery modules of the phase change materials described in Comparative Example 1 and Example 2;

[0031] Fig. 9 This is a schematic diagram of a shape stability test of the phase change material of Comparative Example 2 when heated at 70° C. for 2 hours;

[0032] Fig.10 These are the combustion test diagrams of the cake-shaped samples of Comparative Example 3 and Example 2. DETAILED DESCRIPTION

[0033] The present invention provides a phase change material, which comprises the following raw materials according to the percentage by mass: 60-80% of a phase change matrix, 8-12% of a support skeleton, 1-5% of a thermal conductivity enhancer and 10-25% of a flame retardant;

[0034] The phase change matrix includes low melting point paraffin and high melting point paraffin; the high melting point paraffin has a melting point greater than the low melting point paraffin.

[0035] In the present invention, unless otherwise specified, all preparation raw materials are commercially available products well known to those skilled in the art.

[0036] According to the percentage by mass, the phase change material of the present invention includes 60-80% of the phase change matrix, preferably 65-75%, and more preferably 68-72%. In the present invention, the phase change matrix includes low melting point paraffin and high melting point paraffin; the mass ratio of the low melting point paraffin and the high melting point paraffin is preferably (1-4): (1-4), more preferably (1-3): 1, and most preferably 3: 1 or 1: 1. In the present invention, the low melting point paraffin preferably includes one or more of PCM44 (melting point is 44°C), PCM46 (melting point is 46°C) and PCM48 (melting point is 48°C), more preferably PCM44; when the low melting point paraffin is two or more of the above specific selections, the present invention does not have any special restrictions on the ratio of the above specific substances, and they can be mixed in any ratio. In the present invention, the high melting point paraffin preferably includes one or more of PCM116 (melting point is 116°C), PCM118 (melting point is 118°C) and PCM120 (melting point is 120°C), and more preferably PCM120; when the high melting point paraffin is two or more of the above-mentioned specific options, the present invention has no special limitation on the ratio of the above-mentioned specific substances, and they can be mixed in any ratio.

[0037] In the present invention, the low melting point paraffin will absorb a large amount of heat to undergo phase change (from solid to liquid) when it reaches its melting point, which is latent heat absorption; therefore, the low melting point paraffin can effectively control the battery temperature and prevent overheating by absorbing the heat generated by the battery during operation, thereby extending the battery life and improving safety; when an abnormal condition occurs in the battery (such as thermal runaway) and the temperature reaches the phase change temperature of the high melting point paraffin, the high melting point paraffin will absorb a large amount of heat, delay the sharp rise in battery temperature, provide additional thermal buffering, and thus enhance the safety of the battery.

[0038] According to the percentage by mass, the phase change material of the present invention comprises 8-12% of the support skeleton, preferably 9-11%, and more preferably 10%. In the present invention, the material of the support skeleton preferably comprises one or more of thermoplastic elastic styrene-butadiene rubber (SEBS), epoxy resin (ER) and styrene-butadiene-styrene block copolymer (SBS), more preferably thermoplastic elastic styrene-butadiene rubber. When the material of the support skeleton is two or more of the above-mentioned specific selections, the present invention has no special restrictions on the ratio of the above-mentioned specific substances, and they can be mixed in any ratio.

[0039] In the present invention, the SEBS has good elasticity and mechanical strength, and can provide structural support for the composite material, ensuring that the phase change material maintains a certain shape and stability when switching between solid and liquid states, preventing the material from being lost or deformed during use, thereby ensuring its long-term effectiveness and reliability.

[0040] According to the percentage by mass, the phase change material of the present invention includes 1-5% of thermal conductivity enhancer, preferably 2-4%, and more preferably 3%. In the present invention, the thermal conductivity enhancer preferably includes one or more of expanded graphite (EG), boron nitride (BN) and aluminum nitride (AlN), more preferably expanded graphite. When the thermal conductivity enhancer is two or more of the above-mentioned specific selections, the present invention has no special restrictions on the ratio of the above-mentioned specific substances, and can be mixed in any ratio.

[0041] In the present invention, the expanded graphite has excellent thermal conductivity and can significantly improve the overall thermal conductivity of the phase change material. By quickly conducting the heat generated by the battery to the phase change material, the heat absorption and dissipation process is accelerated, and the thermal management effect and safety performance of the battery are further improved.

[0042] According to the percentage by mass, the phase change material of the present invention comprises 10 to 25% of a flame retardant, preferably 13 to 22%, and more preferably 15 to 20%. In the present invention, the flame retardant preferably comprises ammonium polyphosphate (APP) and / or aluminum hypophosphite (AHP). When the flame retardant comprises ammonium polyphosphate and aluminum hypophosphite, the mass ratio of the ammonium polyphosphate to the aluminum hypophosphite is preferably (1 to 2): (1 to 2), and more preferably 1:1, 1:2 or 2:1.

[0043] In the present invention, the APP and AHP as flame retardants begin to decompose and release non-combustible gases (NH3 and H2O), which dilute the combustible gas and reduce the heat of the flame. As the temperature rises, the flame retardant further decomposes the phosphoric acid compound and polyphosphoric acid, which accelerates the formation of the carbonized layer as a catalyst. Afterwards, the carbon residues are cross-linked and form a continuous and dense carbonized layer of CO and CO2, which effectively isolates the transfer of heat, oxygen and combustible gas, and protects the phase change material from combustion.

[0044] The present invention also provides a method for preparing the phase change material described in the above technical solution, comprising the following steps:

[0045] The phase change matrix is ​​melted and then mixed with a supporting skeleton, a thermal conductivity enhancer and a flame retardant to obtain the phase change material.

[0046] In the present invention, the melting temperature is preferably 130 to 180°C, more preferably 140 to 170°C, and most preferably 150 to 160°C.

[0047] In the present invention, the process of melting the phase change matrix is ​​preferably to melt the high melting point paraffin first, then add the low melting point paraffin and stir until the low melting point paraffin is completely melted. In the present invention, the stirring speed is preferably 400 to 600 rpm, more preferably 450 to 550 rpm, and most preferably 480 to 500 rpm. In the present invention, the stirring is preferably mechanical stirring. In the present invention, the melting is preferably carried out in a constant temperature oil bath.

[0048] In the present invention, the mixing with the support skeleton, the thermal conductivity enhancer and the flame retardant preferably includes sequentially adding the support skeleton to the melted phase change matrix for the first stirring, adding the flame retardant for the second stirring, and adding the thermal conductivity enhancer before the third stirring; when the flame retardant is APP and AHP, it is preferred to add APP first and then AHP. In the present invention, the thermal conductivity enhancer is preferably added in batches, and the batch addition process is preferably 1g / time. The speed of the first stirring is preferably 500-700rpm, more preferably 550-650rpm, and most preferably 600rpm; the speed of the second stirring is preferably 500-600rpm, more preferably 550-600rpm; the time of the second stirring is preferably 25-40min, more preferably 30-35min; the speed of the third stirring is preferably 600rpm, and the time is preferably 20-30min, more preferably 30min. In the present invention, the first stirring, the second stirring and the third stirring are preferably mechanical stirring.

[0049] In the present invention, the support skeleton forms a polymer network structure during the above preparation process, and the phase change matrix is ​​fixed on the skeleton, thereby ensuring that no leakage occurs while providing latent heat.

[0050] The present invention also provides the application of the phase change material described in the above technical solution or the phase change material prepared by the preparation method described in the above technical solution in a power battery module. The present invention does not have any special limitation on the application method, and the application method can be carried out by a method familiar to those skilled in the art.

[0051] The phase change material and its preparation method and application provided by the present invention are described in detail below in conjunction with the embodiments, but they should not be construed as limiting the protection scope of the present invention.

[0052] Example 1

[0053] like Figure 1 As shown, 36 g of PCM120 was poured into a constant temperature oil bath at 150° C. After the PCM120 was completely melted, 36 g of PCM44 was added, and the mixture was stirred at a speed of 500 rpm until the PCM44 was completely melted, thereby obtaining a uniformly mixed phase change matrix.

[0054] Add 10g SEBS to the phase change matrix, stir at a speed of 600rpm by mechanical stirring until SEBS is completely melted, add 15g APP, stir at a speed of 600rpm by mechanical stirring until APP is completely melted, add 3g expanded graphite three times, 1g expanded graphite each time, stir at 600rpm for 30min until the expanded graphite is evenly dispersed, pour the obtained mixture into a mold, cool naturally, and demold to obtain the phase change material;

[0055] Figure 2 is a mass loss curve of the phase change material when heated at 70° C. for 25 h, Figure 3 Schematic diagram of the shape stability test of the phase change material heated at 70°C for 25h. Figures 2-3 It can be seen that after heating at 70°C for 25 hours, the mass loss rate of the phase change material is only 0.23wt%, and the shape remains unchanged. Observing the filter paper on which the sample is placed, there is almost no leakage mark, which indicates that the phase change material has almost no leakage loss during the heating process, reflecting the excellent anti-leakage performance and shape stability of the phase change material under heating. Therefore, the phase change material has excellent anti-leakage and anti-deformation properties, and can solve the problem of easy leakage of phase change materials and module deformation in existing battery thermal safety systems.

[0056] Example 2

[0057] like Figure 1 As shown, 36 g of PCM120 was poured into a constant temperature oil bath at 150° C. After the PCM120 was completely melted, 36 g of PCM44 was added, and the mixture was stirred at a speed of 500 rpm until the PCM44 was completely melted, thereby obtaining a uniformly mixed phase change matrix.

[0058] Add 10g SEBS to the phase change matrix, stir at a speed of 600rpm by mechanical stirring until SEBS is completely melted, then add 10g APP and 5g AHP in sequence, stir at a speed of 600rpm by mechanical stirring until both are completely melted, add 3g expanded graphite three times, 1g expanded graphite each time, stir at 600rpm for 30min until the expanded graphite is evenly dispersed, pour the obtained mixture into a mold, cool naturally, and demold to obtain the phase change material;

[0059] Figure 2 is a mass loss curve of the phase change material when heated at 70° C. for 25 h, Figure 3 Schematic diagram of the shape stability test of the phase change material heated at 70°C for 25h. Figures 2-3It can be seen that after heating at 70°C for 25 hours, the mass loss rate of the phase change material is only 0.13wt%, and the shape remains unchanged. Observing the filter paper on which the sample is placed, there is almost no leakage mark, which indicates that the phase change material has almost no leakage loss during the heating process, reflecting the excellent anti-leakage performance and shape stability of the phase change material under heating. Therefore, the phase change material has excellent anti-leakage and anti-deformation properties, and can solve the problems of easy leakage of phase change materials and module deformation in existing battery thermal safety systems;

[0060] The phase change material is subjected to a heating plate test: the time required for the heating plate coated with the high melting point flame retardant composite phase change material provided in Example 2 to heat up to 180°C is compared with the time required for the blank heating plate not coated with the phase change material to heat up to 180°C; wherein Figure 4 is the heating plate curve of the phase change material and the blank heating plate, Figure 5 is the infrared image of the phase change material and the blank heating plate, Figures 4-5 It can be seen that the blank heating plate without phase change material coating takes 590 seconds to heat up to 180°C, while the heating plate with phase change material coating takes 960 seconds to heat up to 180°C. Compared with the blank group, the heating plate with phase change material coating takes 370 seconds to heat up to 180°C, indicating that the material has good high temperature resistance.

[0061] Example 3

[0062] like Figure 1 As shown, 36 g of PCM120 was poured into a constant temperature oil bath at 150° C. After the PCM120 was completely melted, 36 g of PCM44 was added, and the mixture was stirred at a speed of 500 rpm until the PCM44 was completely melted, thereby obtaining a uniformly mixed phase change matrix.

[0063] 10 g of SEBS was added to the phase change matrix, and the mixture was stirred at a speed of 600 rpm by mechanical stirring until the SEBS was completely melted. Then, 7.5 g of APP and 7.5 g of AHP were added in sequence, and the mixture was stirred at a speed of 600 rpm by mechanical stirring until the two were completely melted. 3 g of expanded graphite was added three times, 1 g of expanded graphite each time, and the mixture was stirred at 600 rpm for 30 min until the expanded graphite was evenly dispersed. The obtained mixture was poured into a mold, naturally cooled, and demolded to obtain the phase change material.

[0064] Figure 2 is a mass loss curve of the phase change material when heated at 70° C. for 25 h, Figure 3 Schematic diagram of the shape stability test of the phase change material heated at 70°C for 25h. Figures 2-3It can be seen that after heating at 70°C for 25 hours, the mass loss rate of the phase change material is only 0.18wt%, and the shape remains unchanged. Observing the filter paper on which the sample is placed, there is almost no leakage mark, which indicates that the phase change material has almost no leakage loss during the heating process, reflecting the excellent anti-leakage performance and shape stability of the phase change material under heating. Therefore, the phase change material has excellent anti-leakage and anti-deformation properties, and can solve the problem of easy leakage of phase change materials and module deformation in existing battery thermal safety systems.

[0065] Example 4

[0066] like Figure 1 As shown, 36 g of PCM120 was poured into a constant temperature oil bath at 150° C. After the PCM120 was completely melted, 36 g of PCM44 was added, and the mixture was stirred at a speed of 500 rpm until the PCM44 was completely melted, thereby obtaining a uniformly mixed phase change matrix.

[0067] Add 10g SEBS to the phase change matrix, stir at a speed of 600rpm by mechanical stirring until SEBS is completely melted, then add 5g APP and 10g AHP in sequence, stir at a speed of 600rpm by mechanical stirring until both are completely melted, add 3g expanded graphite three times, 1g expanded graphite each time, stir at 600rpm for 30min until the expanded graphite is evenly dispersed, pour the obtained mixture into a mold, cool naturally, and demold to obtain the phase change material;

[0068] Figure 2 is a mass loss curve of the phase change material when heated at 70° C. for 25 h, Figure 3 Schematic diagram of the shape stability test of the phase change material heated at 70°C for 25h. Figures 2-3 It can be seen that after heating at 70°C for 25 hours, the mass loss rate of the phase change material is only 0.14wt%, and the shape remains unchanged. Observing the filter paper on which the sample is placed, there is almost no leakage mark, which indicates that the phase change material has almost no leakage loss during the heating process, reflecting the excellent anti-leakage performance and shape stability of the phase change material under heating. Therefore, the phase change material has excellent anti-leakage and anti-deformation properties, and can solve the problem of easy leakage of phase change materials and module deformation in existing battery thermal safety systems.

[0069] Example 5

[0070] like Figure 1As shown, 36 g of PCM120 was poured into a constant temperature oil bath at 150° C. After the PCM120 was completely melted, 36 g of PCM44 was added, and the mixture was stirred at a speed of 500 rpm until the PCM44 was completely melted, thereby obtaining a uniformly mixed phase change matrix.

[0071] 10 g of SEBS was added to the phase change matrix, and the mixture was stirred at a speed of 600 rpm by mechanical stirring until the SEBS was completely melted. Then, 15 g of AHP was added in sequence, and the mixture was stirred at a speed of 600 rpm by mechanical stirring until the two were completely melted. 3 g of expanded graphite was added three times, 1 g of expanded graphite each time, and the mixture was stirred at 600 rpm for 30 min until the expanded graphite was evenly dispersed. The obtained mixture was poured into a mold, naturally cooled, and demolded to obtain the phase change material.

[0072] Figure 2 is a mass loss curve of the phase change material when heated at 70° C. for 25 h, Figure 3 Schematic diagram of the shape stability test of the phase change material heated at 70°C for 25h. Figures 2-3 It can be seen that after heating at 70°C for 25 hours, the mass loss rate of the phase change material is only 0.21wt%, and the shape remains unchanged. Observing the filter paper on which the sample is placed, there is almost no leakage mark, which indicates that the phase change material has almost no leakage loss during the heating process, reflecting the excellent anti-leakage performance and shape stability of the phase change material under heating. Therefore, the phase change material has excellent anti-leakage and anti-deformation properties, and can solve the problem of easy leakage of phase change materials and module deformation in existing battery thermal safety systems.

[0073] Comparative Example 1

[0074] Pour 36g PCM120 into a constant temperature oil bath at 150°C, and after the PCM120 is completely melted, add 36g PCM44, and stir at a speed of 500rpm by mechanical stirring until the PCM44 is completely melted to obtain a uniformly mixed phase change matrix;

[0075] 25 g of SEBS was added to the phase change matrix, and the mixture was stirred at a speed of 600 rpm by mechanical stirring until the SEBS was completely melted. Then, 3 g of expanded graphite was added three times (1 g each time), and the mixture was stirred at 600 rpm for 30 min until the expanded graphite was evenly dispersed. The obtained mixture was poured into a mold, naturally cooled, and demolded to obtain the phase change material;

[0076] Figure 2 is a mass loss curve of the phase change material when heated at 70° C. for 25 h, Figure 3Schematic diagram of the shape stability test of the phase change material heated at 70°C for 25h. Figures 2-3 It can be seen that after heating at 70°C for 25 hours, the mass loss rate of the phase change material is only 0.17wt%, and the shape remains unchanged. Observing the filter paper on which the sample is placed, there is almost no leakage mark, which indicates that the phase change material has almost no leakage loss during the heating process, reflecting the excellent anti-leakage performance and shape stability of the phase change material under heating. Therefore, the phase change material has excellent anti-leakage and anti-deformation properties, and can solve the problem of easy leakage of phase change materials and module deformation in existing battery thermal safety systems.

[0077] Comparative Example 2

[0078] Pour 72 g of PCM44 into a constant temperature oil bath at 150°C, and stir at a speed of 500 rpm until PCM44 is completely melted to obtain a phase change matrix;

[0079] 25 g of SEBS was added to the phase change matrix, and the mixture was stirred at a speed of 600 rpm by mechanical stirring until the SEBS was completely melted. Then, 3 g of expanded graphite was added three times (1 g each time), and the mixture was stirred at 600 rpm for 30 min until the expanded graphite was evenly dispersed. The obtained mixture was poured into a mold, naturally cooled, and demolded to obtain the phase change material;

[0080] Fig. 9 The schematic diagram of the shape stability test of the phase change material after heating at 70°C for 2 hours is shown. Fig. 9 It can be seen that after heating at 70°C for 2 hours, the mass loss rate of the phase change material is 3.17wt%. The filter paper on which the sample is placed shows obvious signs of leakage, which indicates that the phase change material has obvious leakage and shape instability when heated. Therefore, it is difficult for the phase change material to maintain good anti-leakage and anti-deformation properties under high temperature conditions, and it is impossible to effectively solve the problem of easy leakage of phase change materials and module deformation in existing battery thermal safety systems. The PCM120 added in Example 2 has good compatibility with PCM44, which can significantly improve the fluidity of the composite material in the battery module mold. Therefore, it can be obtained that Example 2 not only exhibits excellent anti-leakage effect, but is also easy to use in battery modules.

[0081] Comparative Example 3

[0082] Pour 72 g of PCM44 into a constant temperature oil bath at 150 °C and stir at 500 rpm until PCM44 is completely melted to obtain a uniformly mixed phase change matrix;

[0083] 10 g of SEBS was added to the phase change matrix, and the mixture was stirred at a speed of 600 rpm by mechanical stirring until the SEBS was completely melted. Then, 7.5 g of APP and 7.5 g of AHP were added in sequence, and the mixture was stirred at a speed of 600 rpm by mechanical stirring until the two were completely melted. 3 g of expanded graphite was added three times, 1 g of expanded graphite each time, and the mixture was stirred at 600 rpm for 30 min until the expanded graphite was evenly dispersed. The obtained mixture was poured into a mold, naturally cooled, and demolded to obtain the phase change material.

[0084] Fig.10 The combustion test of the cake-shaped sample of Example 3 and Example 2 is carried out. The process of the combustion test of the cake-shaped sample is to use a spray gun to burn the upper surface of the cake-shaped sample for 10 seconds, wait for it to extinguish, and then use a spray gun to burn at the same position for 30 seconds to observe the combustion of the sample. Fig.10 It can be seen that the samples of Comparative Example 3 and Example 2 can be extinguished within 1 second after the first ignition for 10 seconds, indicating that a sparse insulation layer is initially formed, which blocks heat and oxygen to a certain extent, thereby interrupting combustion. The sample of Comparative Example 3 shows a certain flame retardant effect after secondary ignition. After burning with a spray gun for 30 seconds, the sample of Comparative Example 3 is ignited and extinguished after burning for 10 seconds. The sample of Example 2 shows a significant flame retardant effect after secondary ignition. After burning with a spray gun for 30 seconds, the sample of Example 2 is not ignited. The synergistic flame retardant mechanism of APP and AHP can be attributed to the gas phase mechanism and the condensation phase mechanism. During the combustion process, the APP and AHP composite material begins to decompose and release non-combustible gases (NH3 and H2O), which dilute the combustible gas and reduce the heat of the flame. As the temperature rises, the APP and AHP composite material further decomposes the phosphoric acid compound and polyphosphoric acid, catalytically accelerating the formation of the carbonized layer. The high melting point phase change materials play an important role in this process. They maintain the shape stability of the composite material at higher temperatures, help stabilize and strengthen the structure of the carbonized layer, and thus form a more dense and high temperature resistant thermal insulation barrier than that of Comparative Example 3. Afterwards, the carbon residues are cross-linked and formed by CO and CO2, further forming a continuous and dense carbonized layer, which effectively isolates the transfer of heat, oxygen and combustible gases and protects the phase change material from combustion.

[0085] Application Examples

[0086] The phase change materials of Comparative Example 1 and Examples 1 to 5 are applied to a lithium-ion battery module (using the commercially available Lishen power battery LP2468134SA-23Ah, with a nominal capacity of 23Ah and a nominal voltage of 3.2V). In order to configure the battery module, the single cells are first charged and discharged by a charging and discharging device to screen out batteries with the same capacity. Subsequently, these screened single cells are welded through the connecting piece 3 and assembled into a 2 (series) × 3 (parallel) battery module. The CPCM (composite phase change material) and the battery cells are consistent in height and width. In order to ensure the phase change heat storage performance and minimize the contact thermal resistance, a flat and complete surface must be maintained on the CPCM board so that it fits tightly with the battery (such as Figure 6 shown);

[0087] The composite phase change material of the battery module can not only maintain the normal operating temperature of the battery module, but also balance the temperature difference of the battery module within a reasonable range. Figure 7 The thermal management temperature curves of the battery modules of the phase change materials of Comparative Example 1 and Example 2 are used to compare the temperature control effects of charging / discharging at 1C / 0.5C, 1C / 0.75C and 1C / 1C respectively at a constant temperature of 25°C during 10 cycles ( Figure 7 a is comparative example 1, b is example 2). The temperature difference (ΔT) of various battery modules refers to the difference between the highest temperature and the lowest temperature ( Figure 8 In the figure, a is comparative example 1 and b is example 2). At a discharge rate of 0.5C, both battery modules were maintained within a suitable operating temperature range, but the temperature of the battery module of comparative example 1 was higher than that of the battery module of example 2. However, when the discharge rate was increased to 1C, the maximum temperature in the cycle of comparative example 1 exceeded 48.2°C ( Figure 7 a), and the temperature difference is close to 8.12℃( Figure 8 a) in the figure shows the potential thermal hazard of the battery module. The maximum temperature and temperature difference of the battery module in Example 2 are maintained below 46.6°C and 3.6°C, respectively. EG, APP and AHP in the composite phase change material play a synergistic role in improving the thermal management effect, constructing a stable three-dimensional thermal conductive skeleton to enhance the heat dissipation capacity. Therefore, the battery module with Example 2 is an effective thermal management method to enhance the cooling effect.

[0088] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. A phase change material, characterized in that: According to the percentage by mass, the preparation raw materials include: 60-80% of phase change matrix, 8-25% of support skeleton, 1-5% of thermal conductivity enhancer and 10-25% of flame retardant; The phase change matrix includes low melting point paraffin and high melting point paraffin; the high melting point paraffin has a melting point greater than the low melting point paraffin.

2. The phase change material according to claim 1, characterized in that: The mass ratio of the low melting point paraffin wax to the high melting point paraffin wax is (1-4):(1-4).

3. The phase change material according to claim 1 or 2, characterized in that: The low melting point paraffin wax includes one or more of PCM44, PCM46 and PCM48; The high melting point paraffin wax includes one or more of PCM116, PCM118 and PCM120.

4. The phase change material according to claim 1, characterized in that: The material of the supporting skeleton includes one or more of thermoplastic elastic styrene-butadiene rubber, epoxy resin and styrene-butadiene-styrene block copolymer.

5. The phase change material according to claim 1, characterized in that: The thermal conductivity enhancer includes one or more of expanded graphite, boron nitride and aluminum nitride.

6. The phase change material according to claim 1, characterized in that: The flame retardant includes ammonium polyphosphate and / or aluminum hypophosphite.

7. The phase change material according to claim 6, characterized in that: When the flame retardant includes ammonium polyphosphate and aluminum hypophosphite, the mass ratio of the ammonium polyphosphate to the aluminum hypophosphite is (1-2): (1-2).

8. The method for preparing the phase change material according to any one of claims 1 to 7, characterized in that: The following steps are involved: The phase change matrix is ​​melted and then mixed with a supporting skeleton, a thermal conductivity enhancer and a flame retardant to obtain the phase change material.

9. The preparation method according to claim 8, characterized in that: The melting temperature is 130-180°C.

10. Use of the phase change material according to any one of claims 1 to 7 or the phase change material prepared by the preparation method according to claim 8 or 9 in a power battery module.

Citation Information

Cited By

  • Flame-retardant composite phase change material as well as preparation method and application thereof

    CN120209790A

  • A flame retardant composite phase change material and its preparation method and application

    CN120209790B