A method for preparing a silicon-carbon composite material, its product and application in lithium-ion batteries
By combining silicon carbon dust removal powder with polymer microsphere emulsion, a uniformly coated silicon carbon composite material is formed, which solves the problems of too small particle size and too large specific surface area of silicon carbon dust removal powder in lithium-ion batteries, and achieves high temperature Improved cycle performance and Coulombic efficiency, and efficient use of resources.
Patent Information
- Application Number
- CN202211181280.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-09-27
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2042-09-27
AI Technical Summary
The silicon carbon dust removal powder used in existing lithium-ion batteries has too small particle size and too large specific surface area, resulting in rapid battery capacity attenuation, poor cycle performance, and serious waste of resources. There is a lack of effective preparation methods to solve these problems.
Using a combination of silicon carbon dust removal powder and polymer microsphere emulsion, through spray drying and high temperature carbonization, a silicon carbon composite material with a uniform carbon layer coating is formed to improve its electrochemical performance and effectively utilize resources.
The prepared silicon-carbon composite material shows excellent high-temperature cycle performance and high first Coulombic efficiency in lithium-ion batteries, solving the problem of resource waste and improving the cycle stability of the battery.
Smart Images

Figure CN115872386B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of lithium-ion batteries, and in particular to a method for preparing a silicon-carbon composite material, a product thereof, and an application of the same in lithium-ion batteries. Background Art
[0002] Driven by the new energy wave, lithium-ion batteries have been continuously updated and replaced, and have now been commercialized. They are now in good shape when installed in portable electronic products and power tools. This is due to the advantages of lithium-ion batteries such as high energy density and long service life. The current mainstream negative electrode material for commercial lithium-ion batteries is still graphite. Compared with other carbon material negative electrodes, graphite negative electrodes have the advantages of high initial efficiency and good cycle stability. However, the theoretical capacity of graphite negative electrodes is only 372mAh / g, which can no longer keep up with the needs of downstream industries.
[0003] Silicon-based materials are considered to be the most promising new negative electrode materials to replace graphite, with a theoretical capacity of up to 4200mAh / g. However, during the charge and discharge process, as lithium ions are inserted and removed, the volume of silicon-based materials will expand and contract rapidly, which will cause the active material to fall off the current collector and the material to pulverize. At the same time, the solid electrolyte interface film will regenerate repeatedly, resulting in capacity loss and cycle attenuation, which hinders the commercialization of silicon-based materials.
[0004] Silicon-carbon materials in silicon-based materials are a type of negative electrode material with a higher specific capacity. Compared with silicon alone, the introduction of carbon materials into silicon materials can alleviate the volume change of active silicon during the lithium insertion and extraction process. In addition, silicon-carbon materials also have the advantages of low operating voltage and good safety. Therefore, they have gradually become a research hotspot in recent years.
[0005] The silicon-carbon materials prepared in the prior art are mostly coarse particles that need to be crushed and sieved. The silicon-carbon materials that are classified due to their small particle size (median particle size D50 is about 0.1-3.0 μm) are called silicon-carbon dust removal powder. 2 / g), when used as negative electrode material of lithium-ion battery, it will irreversibly consume electrolyte during charging and discharging, which will lead to rapid battery capacity decay, that is, poor cycle performance; in addition, silicon-carbon dust removal powder is prone to uncontrollable agglomeration during the process of making electrode sheets, resulting in poor processing performance of electrode sheets. However, if it is not utilized, continuous accumulation will cause serious waste of resources, so a technology is urgently needed to solve this problem. Summary of the invention
[0006] In view of the above-mentioned problems existing in the prior art, the present invention discloses a method for preparing a silicon-carbon composite material, which directly uses silicon-carbon dust removal powder as raw material. The lithium-ion battery assembled with the prepared silicon-carbon composite material has excellent high-temperature cycle performance and high first coulomb efficiency; and effectively solves the problem of serious waste of resources caused by large-scale accumulation of silicon-carbon dust removal powder.
[0007] The specific technical solutions are as follows:
[0008] A method for preparing a silicon-carbon composite material comprises the following steps:
[0009] (1) mixing silicon-carbon dust removal powder with water to obtain a suspension, and blending the suspension with a polymer microsphere emulsion to obtain a slurry;
[0010] The median particle size of the silicon-carbon dust removal powder is 0.1 to 3.0 μm;
[0011] The polymer microsphere emulsion is prepared by using styrene monomers, propylene monomers and unsaturated alcohol monomers as raw materials and polymerized by an initiator.
[0012] (2) spray drying the slurry to obtain a silicon-carbon material precursor;
[0013] (3) subjecting the silicon-carbon material precursor to high-temperature carbonization treatment to obtain the silicon-carbon composite material.
[0014] The preparation method disclosed in the present invention uses silicon-carbon dust removal powder with a median particle size D50 of 0.1 to 3.0 μm as raw material, and evenly mixes the raw material with a polymer microsphere emulsion composed of multiple monomers polymerized in a specific ratio to form a granulation slurry, which is then spray-dried. Through this process, secondary granulation of the silicon-carbon dust removal powder and simultaneous polymer coating can be achieved, and finally a silicon-carbon composite material is obtained under high-temperature carbonization.
[0015] The experiment found that the composition of the polymer microsphere emulsion in the preparation method is particularly critical. Its raw material composition includes three monomers selected from styrene monomers, propylene monomers and unsaturated alcohol monomers. Styrene monomers can improve the bonding force with silicon-carbon dust removal powder, help to form a coating layer, and after high-temperature treatment, it is more conducive to forming a carbon layer structure in the form of a single-layer particle, uniformly coating the surface of the silicon-carbon material, and improving the charge and discharge cycle performance; propylene monomers can give polymer microspheres good lithium ion conductivity, and at the same time can enhance the bonding force between the negative electrode active particles and the current collector; and the introduction of hydroxyl-containing unsaturated alcohol monomers can further regulate the glass transition temperature (T g ), so that T gMatch the spray drying process conditions of silicon-carbon materials. During spray drying, the silicon-carbon dust removal powder can be secondary granulated, and the secondary particles of the obtained silicon-carbon material can be regulated to have a suitable particle size. All three are indispensable, otherwise the median particle size of the prepared silicon-carbon composite material will be too large or too small, which will affect the electrochemical performance of the lithium-ion battery assembled therein.
[0016] In step (1):
[0017] The median particle size of the silicon-carbon dust removal powder is 0.1 to 3.0 μm, preferably 0.5 to 3.0 μm, more preferably 0.5 to 1.5 μm, and more preferably 1.5 μm.
[0018] The solid content of the suspension is 1 to 40 wt %, preferably 5 to 25 wt %, and more preferably 10 to 20 wt %.
[0019] The solid content of the polymer microsphere emulsion is 10-50 wt %, specifically, the solid content of the polymer microsphere emulsion is adjusted by adding water, preferably 20-40 wt %, more preferably 30 wt %.
[0020] In step (1), the mass comparison of the added silicon-carbon dust removal powder and the dry weight in the polymer microsphere emulsion is the key. Preferably, the mass ratio of the two is controlled to be 1:0.1-0.2. It has been found through experiments that within this ratio range, the polymer microspheres can be coated on the surface of the secondary particles of the silicon-carbon material in the form of a single layer, and after high-temperature carbonization treatment, the carbon layer can be uniformly coated on the surface of the secondary particles; by adjusting this ratio, the thickness of the coated carbon layer in the final prepared silicon-carbon composite material can also be adjusted. When the ratio of the two is too low, that is, the dry weight of the added polymer microsphere emulsion is too much, it may cause the polymer microspheres to agglomerate and fail to be coated in the form of a single layer, which in turn leads to uneven thickness of the coated carbon layer, which ultimately affects its electrochemical performance.
[0021] Further preferably, the mass ratio of the dry weight of the silicon-carbon dust removal powder to the polymer microsphere emulsion is 1:0.15.
[0022] In step (1):
[0023] The styrene monomer is selected from one or more of styrene, 2-methylstyrene, 3-methylstyrene, 4-methylstyrene, 2-chlorostyrene, 3-chlorostyrene, 4-chlorostyrene, 2-fluorostyrene, 3-fluorostyrene, and 4-fluorostyrene; preferably styrene and / or 2-methylstyrene, more preferably styrene.
[0024] The acrylic monomer is selected from one or more of acrylic acid ester monomers, methacrylic acid ester monomers, acrylonitrile, and methacrylonitrile; preferably, it is an acrylic acid ester monomer and / or a methacrylic acid ester monomer.
[0025] The acrylic acid ester monomer is selected from one or more of methyl acrylate, ethyl acrylate, propyl acrylate, butyl acrylate, pentyl acrylate, hexyl acrylate, heptyl acrylate, octyl acrylate, nonyl acrylate and decyl acrylate.
[0026] The methacrylate monomer is selected from one or more of methyl methacrylate, ethyl methacrylate, propyl methacrylate, butyl methacrylate, pentyl methacrylate, hexyl methacrylate, heptyl methacrylate, octyl methacrylate, nonyl methacrylate and decyl methacrylate.
[0027] The unsaturated alcohol monomer is selected from one or more of propenol, butenol, pentenol, hexenol, heptenol, octenol, nonenol, decenol, 2-chloropropenol, and 3-chloro-propenol; preferably propenol and / or 2-chloropropenol, more preferably propenol.
[0028] The initiator is selected from the common initiator types in the art, such as azo initiators and peroxide initiators.
[0029] The azo initiator is selected from azobisisobutyronitrile, azobisisoheptanenitrile, etc.;
[0030] The peroxide initiator is selected from hydroperoxides, acyl peroxides, dialkyl peroxides, ester peroxides, ketone peroxides, dicarbonate peroxides, etc., specifically tert-butyl hydroperoxide, isopropylbenzene hydroperoxide, benzoyl peroxide BPO, dodecyl peroxide LPO, lauroyl peroxide, diisopropyl peroxide, tert-butyl perbenzoate, tert-butyl pervalerate, methyl ethyl ketone peroxide, cyclohexanone peroxide, diisopropyl peroxydicarbonate, dicyclohexyl peroxydicarbonate, etc.
[0031] The polymerization may be any one of solution polymerization, emulsion polymerization, precipitation polymerization and suspension polymerization, and the specific polymerization process adopts conventional technical means in the art.
[0032] In the present invention, the dry weight of the polymer microsphere emulsion is the product of the total weight of the polymer microsphere emulsion and the solid content. Taking the total dry weight of the polymer microsphere emulsion as 100%, the content of the unsaturated alcohol monomer in the raw material composition is 0.5-20%.
[0033] Preferably, based on the total dry weight of the polymer microsphere emulsion as 100%, the raw material composition includes:
[0034]
[0035] Further preferred:
[0036] The content of the unsaturated alcohol monomer is 2-7% based on the total dry weight of the polymer microsphere emulsion as 100%;
[0037] More preferably, based on the total dry weight of the polymer microsphere emulsion as 100%, the raw material composition includes:
[0038] Most preferably, the content of the unsaturated alcohol monomer is 4.5%.
[0039] Experiments have shown that with the continuous optimization of the raw material composition in the polymer microsphere emulsion, the glass transition temperature of the prepared polymer microspheres is more closely matched with the process parameters of spray drying. The silicon-carbon composite material finally prepared has a more suitable median particle size and has better electrochemical performance when used as a negative electrode material.
[0040] In step (2):
[0041] When spray drying silicon-carbon materials, it is necessary to consider the problem that the spray drying temperature is too low, resulting in the inability to completely dry the material, and the problem that the spray drying temperature is too high, resulting in too large a D50 of the dried material and too high energy consumption. Therefore, after comprehensive consideration, the spray drying is controlled, and the air inlet temperature is 160-220°C, and more preferably 185-200°C. It has been found through experiments that the polymer microsphere emulsion composed of the above special raw materials can increase the T of the polymer microspheres coated on the surface of the silicon-carbon material. g When the temperature is adjusted to match the above-mentioned spray drying process parameters, the D50 of the finally prepared silicon-carbon composite material can be further affected, and the D50 can be controlled within the range of 5 to 13 μm, and more preferably within the range of 5 to 10 μm.
[0042] Preferably, in the spray drying, the feed rate is 0.01 to 3.0 kg / min and the air pressure is 0.1 to 0.8 MPa; more preferably, the feed rate is 0.05 to 0.2 kg / min and the air pressure is 0.1 to 0.5 MPa.
[0043] In step (3):
[0044] The heating carbonization treatment is carried out under an inert atmosphere, firstly heating to 250-400° C., keeping the temperature for 0.5-4.0 hours, then heating to 750-1000° C., keeping the temperature for 2-20 hours.
[0045] The inert atmosphere is selected from one or more of nitrogen, helium, neon and argon.
[0046] Preferably, the heating rate is selected from 1 to 10° C. / min.
[0047] The experiment found that compared with the single heating, the secondary heating can reduce the specific surface area of the prepared silicon-carbon composite material, and the assembled lithium-ion battery has a higher cycle capacity retention rate and a higher specific capacity.
[0048] The present invention also discloses a silicon-carbon composite material prepared according to the above method, comprising secondary particles of the silicon-carbon material and a pyrolytic carbon layer covering the secondary particles of the silicon-carbon material.
[0049] Preferably, the median particle size of the silicon-carbon composite material is 5 to 13 μm, more preferably 5 to 10 μm, and even more preferably 5.5 to 6.5 μm.
[0050] Preferably, the thickness of the pyrolytic carbon layer is 5 to 10 nm.
[0051] Preferably, the specific surface area of the silicon-carbon composite material is 1 to 4 m 2 / g, more preferably 2.5 to 3.2 m 2 / g.
[0052] The present invention also discloses the use of the silicon-carbon composite material in the preparation of a lithium-ion battery. The assembled lithium-ion battery has excellent high-temperature cycle performance and high first coulombic efficiency.
[0053] Compared with the prior art, the present invention has the following beneficial effects:
[0054] The invention discloses a method for preparing a silicon-carbon composite material, which directly uses silicon-carbon dust removal powder as raw material, effectively solving the problem of serious waste of resources caused by large-scale accumulation of silicon-carbon dust removal powder; the prepared silicon-carbon composite material has a suitable median particle size and specific surface area, and the carbon layer coated on the surface is also extremely uniform. The lithium-ion battery assembled with the silicon-carbon composite material as the negative electrode material has excellent high-temperature cycle performance and high first coulomb efficiency. BRIEF DESCRIPTION OF THE DRAWINGS
[0055] Figure 1 This is a SEM image of the silicon-carbon material precursor prepared in Example 1;
[0056] Figure 2 TEM image of the silicon-carbon composite material prepared in Example 1;
[0057] Figure 3 TEM image of the silicon-carbon composite material prepared in Comparative Example 5;
[0058] Figure 4 The first charge and discharge curve of a button battery assembled using the silicon-carbon composite material prepared in Example 1 as the negative electrode material;
[0059] Figure 5This is a high temperature cycle curve of a small soft-pack battery assembled with the silicon-carbon composite material prepared in Example 1 as the negative electrode material. DETAILED DESCRIPTION
[0060] In order to make the purpose, technical solution and effect of the present invention clearer and more specific, the present invention is further described in detail below in conjunction with the embodiments and drawings. However, it should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.
[0061] The performance parameters of the intermediate products and final products in the following examples and comparative examples are measured according to the following methods.
[0062] 1. Median particle size D50: measured using a laser particle size analyzer (Malvern Mastersizer 2000).
[0063] 2. Glass transition temperature T g : The polymer microsphere emulsion was first dried in a vacuum drying oven at 100°C to obtain a solid substance, and then tested using a differential scanning calorimeter (DSC).
[0064] 3. Specific surface area BET: measured using a BET specific surface area tester (TriStar II 3020).
[0065] Example 1
[0066] (1) Preparation of silicon-carbon dust removal powder suspension
[0067] 100 g of silicon-carbon dust removal powder (D50 is 1.5 μm, purchased from Zhejiang Lichen New Material Technology Co., Ltd.) was added to 500 g of deionized water, and the mixture was fully stirred and dispersed for 3 h to obtain a suspension having a solid content of 16.7%.
[0068] (2) Preparation of polymer microsphere emulsion
[0069] Based on 100 parts of total dry weight, 100 parts of deionized water were added to the emulsion reactor, the temperature was raised to 75°C, 0.5 parts of a 20% deionized ammonium persulfate solution by mass (equivalent to 0.1 parts of ammonium persulfate by dry weight) was added, and then 37.5 parts of styrene, 57.9 parts of ethyl acrylate, and 4.5 parts of propenol were added to the reactor, stirred and blended at 500 rpm, and added at a uniform speed for 2 hours. After the addition, the reaction was continued for 3 hours, and then vacuumed to -70 kPa. The reaction was carried out under this condition for 1 hour, and finally cooled to below 40°C to stop the reaction, and passed through a 100-mesh sieve to obtain a polymer microsphere emulsion, and 133.3 parts of deionized water were added to adjust the solid content of the finally prepared polymer microsphere emulsion to 30%.
[0070] The median particle size D50 of the polymer microspheres in the prepared polymer microsphere emulsion was measured by a laser particle size analyzer to be 0.38 μm. The prepared polymer microsphere emulsion was dried in a vacuum drying oven at 110° C. to a solid substance, and then sintered at 1200° C. in a nitrogen atmosphere for 2 hours. After testing, the residual carbon content was 33.9%.
[0071] The glass transition temperature T of the polymer microspheres in the prepared polymer microsphere emulsion was determined by DSC. g It is 219℃.
[0072] (3) Preparation of slurry
[0073] 50 g of the polymer microsphere emulsion prepared in step (2) (equivalent to 15 g of dry weight) was added to the suspension prepared in step (1), and stirred at 75° C. and 500 rpm for 1 hour to prepare a slurry having a solid content of 17.6%.
[0074] (4) Preparation of silicon-carbon material precursor
[0075] Using a spray dryer, setting the inlet air temperature to 200° C., the exhaust air temperature to 70° C., the feed rate to 0.1 kg / min, and the gas pressure to 0.2 MPa, the slurry obtained in step (3) is spray-dried to obtain a granulated and coated powder material, i.e., a silicon-carbon material precursor;
[0076] (5) Preparation of silicon-carbon composite materials
[0077] The silicon-carbon material precursor prepared in step (4) is loaded into a crucible with a filling amount of 50 wt %. Under the protection of a nitrogen atmosphere, the temperature is increased to 300 ° C at a heating rate of 6 ° C / min, and the temperature is kept for 2 h. Then, the temperature is increased to 880 ° C at a heating rate of 6 ° C / min, and the temperature is kept for 5 h. The crucible is naturally cooled and the silicon-carbon composite material is collected.
[0078] Figure 1 This is an SEM image of the silicon-carbon material precursor prepared in step (4) of this embodiment. By observing the image, it can be found that the polymer microspheres are coated on the surface of the prepared silicon-carbon material secondary particles in the form of a single layer. After heating and carbonization treatment, the carbon layer can be evenly coated on the surface of the secondary particles.
[0079] Figure 2 This is a TEM image of the silicon-carbon composite material prepared in this example at a high magnification. From the image, it can be observed that the carbon layer is very evenly coated on the surface of the silicon-carbon material secondary particles, and it can be found that the thickness of the carbon coating layer is 6.0 nm.
[0080] After testing, the D50 of the silicon-carbon composite material finally prepared in this embodiment is 6.01 μm; the specific surface area is 2.89 m 2 / g.
[0081] Example 2
[0082] The preparation process is basically the same as that of Example 1, except that in step (2), the monomer raw materials added to the reactor are 40.0 parts of styrene, 59.4 parts of ethyl acrylate and 0.5 parts of allyl alcohol.
[0083] The glass transition temperature T of the polymer microspheres in the polymer microsphere emulsion prepared in this example is g The data are listed in Table 1 below.
[0084] The D50 and specific surface area of the silicon-carbon composite material prepared in this example are also listed in Table 1 below.
[0085] Example 3
[0086] The preparation process is substantially the same as that of Example 1, except that in step (2), the monomer raw materials added to the reactor are 35.0 parts of styrene, 49.9 parts of ethyl acrylate and 15.0 parts of allyl alcohol.
[0087] The glass transition temperature T of the polymer microspheres in the polymer microsphere emulsion prepared in this example is g The data are listed in Table 1 below.
[0088] The D50 and specific surface area of the silicon-carbon composite material prepared in this example are also listed in Table 1 below.
[0089] Example 4
[0090] The preparation process is substantially the same as that of Example 1, except that in step (2), the monomer raw materials added to the reactor are 39.0 parts of styrene, 58.9 parts of ethyl acrylate and 2 parts of allyl alcohol.
[0091] The glass transition temperature T of the polymer microspheres in the polymer microsphere emulsion prepared in this example is g The data are listed in Table 1 below.
[0092] The D50 and specific surface area of the silicon-carbon composite material prepared in this example are also listed in Table 1 below.
[0093] Example 5
[0094] The preparation process is substantially the same as that of Example 1, except that in step (2), the monomer raw materials added to the reactor are 36.5 parts of styrene, 56.4 parts of ethyl acrylate and 7.0 parts of allyl alcohol.
[0095] The glass transition temperature T of the polymer microspheres in the polymer microsphere emulsion prepared in this example is g The data are listed in Table 1 below.
[0096] The D50 and specific surface area of the silicon-carbon composite material prepared in this example are also listed in Table 1 below.
[0097] Example 6
[0098] The preparation process is substantially the same as that of Example 1, except that in step (2), the added styrene is replaced by an equal weight portion of 2-methylstyrene.
[0099] The glass transition temperature T of the polymer microspheres in the polymer microsphere emulsion prepared in this example is g The data are listed in Table 1 below.
[0100] The D50 and specific surface area of the silicon-carbon composite material prepared in this example are also listed in Table 1 below.
[0101] Example 7
[0102] The preparation process is basically the same as that of Example 1, except that in step (2), the added styrene is replaced by an equal weight portion of 3-chloro-styrene.
[0103] The glass transition temperature T of the polymer microspheres in the polymer microsphere emulsion prepared in this example is g The data are listed in Table 1 below.
[0104] The D50 and specific surface area of the silicon-carbon composite material prepared in this example are also listed in Table 1 below.
[0105] Example 8
[0106] The preparation process is basically the same as that of Example 1, except that in step (2), the added ethyl acrylate is replaced by an equal weight portion of decyl methacrylate.
[0107] The glass transition temperature T of the polymer microspheres in the polymer microsphere emulsion prepared in this example is g The data are listed in Table 1 below.
[0108] The D50 and specific surface area of the silicon-carbon composite material prepared in this example are also listed in Table 1 below.
[0109] Example 9
[0110] The preparation process is basically the same as that of Example 1, except that in step (2), the added ethyl acrylate is replaced by an equal weight portion of acrylonitrile.
[0111] The glass transition temperature T of the polymer microspheres in the polymer microsphere emulsion prepared in this example is g The data are listed in Table 1 below.
[0112] The D50 and specific surface area of the silicon-carbon composite material prepared in this example are also listed in Table 1 below.
[0113] Example 10
[0114] The preparation process is basically the same as that of Example 1, except that in step (2), the added allyl alcohol is replaced by an equal weight portion of 2-chloropropenol.
[0115] The glass transition temperature T of the polymer microspheres in the polymer microsphere emulsion prepared in this example is g The data are listed in Table 1 below.
[0116] The D50 and specific surface area of the silicon-carbon composite material prepared in this example are also listed in Table 1 below.
[0117] Embodiment 11
[0118] The preparation process is basically the same as that of Example 1, except that in step (3), 66.67 g of the polymer microsphere emulsion prepared in step (2) (equivalent to 20 g in dry weight) is added.
[0119] The glass transition temperature T of the polymer microspheres in the polymer microsphere emulsion prepared in this example is g The data are listed in Table 1 below.
[0120] The D50 and specific surface area of the silicon-carbon composite material prepared in this example are also listed in Table 1 below.
[0121] The SEM characterization of the silicon-carbon material precursor prepared in step (4) shows that the polymer microspheres are still uniformly coated on the surface of the prepared silicon-carbon material secondary particles in the form of a single layer.
[0122] TEM characterization shows that the carbon layer coated on the surface of the silicon-carbon composite material prepared in this embodiment is very uniform, and the thickness of the carbon layer is about 10 nm.
[0123] Example 12
[0124] The preparation process is basically the same as that in Example 1, the only difference is that in step (1), the silicon-carbon dust removal powder with a D50 of 1.5 μm is replaced with an equal mass of silicon-carbon dust removal powder with a D50 of 0.5 μm, which is purchased from Zhejiang Lichen New Material Technology Co., Ltd.
[0125] The glass transition temperature T of the polymer microspheres in the polymer microsphere emulsion prepared in this example is g The data are listed in Table 1 below.
[0126] The D50 and specific surface area of the silicon-carbon composite material prepared in this example are also listed in Table 1 below.
[0127] Embodiment 13
[0128] The preparation process is basically the same as that in Example 1, the only difference is that in step (1), the silicon-carbon dust removal powder with a D50 of 1.5 μm is replaced with an equal mass of silicon-carbon dust removal powder with a D50 of 3.0 μm, which is purchased from Zhejiang Lichen New Material Technology Co., Ltd.
[0129] The glass transition temperature T of the polymer microspheres in the polymer microsphere emulsion prepared in this example is g The data are listed in Table 1 below.
[0130] The D50 and specific surface area of the silicon-carbon composite material prepared in this example are also listed in Table 1 below.
[0131] Embodiment 14
[0132] The preparation process is basically the same as that of Example 1, except that in step (4), the inlet air temperature is replaced with 189°C.
[0133] The D50 and specific surface area of the silicon-carbon composite material prepared in this example are also listed in Table 1 below.
[0134] Embodiment 15
[0135] The preparation process is basically the same as that of Example 1, except that in step (4), the inlet air temperature is replaced with 169°C.
[0136] The D50 and specific surface area of the silicon-carbon composite material prepared in this example are also listed in Table 1 below.
[0137] Comparative Example 1
[0138] Take 1.0 kg of silicon-carbon dust removal powder (D50 = 1.5 μm) and place it in a chemical vapor deposition furnace. First, introduce nitrogen to maintain an inert atmosphere in the furnace. Set the temperature to 600°C at a rate of 6°C / min, then introduce acetylene gas with a flow rate ratio of acetylene gas to nitrogen of 1:3. Continue to heat to 880°C and keep it at this temperature for 5 hours for vapor deposition to obtain a gas-phase carbon-coated silicon-carbon material.
[0139] The D50 and specific surface area of the silicon-carbon composite material prepared in this comparative example are listed in Table 1 below.
[0140] Comparative Example 2
[0141] The preparation process is substantially the same as that of Example 1, except that in step (2), the monomer raw materials added to the reactor are 95.4 parts of styrene and 4.5 parts of acryl alcohol.
[0142] The glass transition temperature T of the polymer microspheres in the polymer microsphere emulsion prepared in this comparative example is g The data are listed in Table 1 below.
[0143] The D50 and specific surface area of the silicon-carbon composite material prepared in this comparative example are also listed in Table 1 below.
[0144] Comparative Example 3
[0145] The preparation process is basically the same as that of Example 1, except that in step (2), the monomer raw materials added to the reactor are 95.4 parts of ethyl acrylate and 4.5 parts of allyl alcohol.
[0146] The glass transition temperature T of the polymer microspheres in the polymer microsphere emulsion prepared in this comparative example is g The data are listed in Table 1 below.
[0147] The D50 and specific surface area of the silicon-carbon composite material prepared in this comparative example are also listed in Table 1 below.
[0148] Comparative Example 4
[0149] The preparation process is basically the same as that of Example 1, except that in step (2), the monomer raw materials added to the reactor are 40 parts of styrene and 59.90 parts of ethyl acrylate.
[0150] The glass transition temperature T of the polymer microspheres in the polymer microsphere emulsion prepared in this comparative example is g The data are listed in Table 1 below.
[0151] The D50 and specific surface area of the silicon-based composite material prepared in this comparative example are listed in the following Table 1.
[0152] Comparative Example 5
[0153] The preparation process is basically the same as that of Example 1, except that in step (3), 100 g of the polymer microsphere emulsion prepared in step (2) (equivalent to 30 g in dry weight) is added.
[0154] Figure 3 This is a TEM image of the silicon-carbon composite material prepared in this comparative example at a high magnification. From the image, it can be observed that the carbon layer is unevenly coated on the surface of the secondary particles of the silicon-carbon material.
[0155] The D50 and specific surface area of the silicon-based composite material prepared in this comparative example are listed in the following Table 1.
[0156] Comparative Example 6
[0157] The preparation process is basically the same as that of Example 1, with the only difference being that in step (5), the secondary heating is replaced by a single heating, specifically, the temperature is directly increased to 880° C. at a heating rate of 6° C. / min and kept at this temperature for 5 h.
[0158] The glass transition temperature T of the polymer microspheres in the polymer microsphere emulsion prepared in this comparative example is g The data are listed in Table 1 below.
[0159] The D50 and specific surface area of the silicon-based composite material prepared in this comparative example are also listed in the following Table 1.
[0160] Table 1
[0161]
[0162]
[0163] Performance Testing:
[0164] 1. The silicon-carbon composite materials prepared in Examples 1 to 15 and Comparative Examples 1 to 6 were used as negative electrode materials to prepare model 2032 button batteries. The specific steps are as follows: the silicon-carbon composite material, the conductive agent SP, the dispersant CMC, and the binder AONE were mixed in a mass ratio of 70:15:5:10, and water was used as a solvent to prepare a negative electrode slurry; the negative electrode slurry was coated on a copper foil, and a lithium sheet was used as a counter electrode and a Celgard 2400 microporous polypropylene film was used as a separator to prepare a button battery.
[0165] The prepared button battery was subjected to charge and discharge cycles, and the charge and discharge conditions were as follows:
[0166] The charge and discharge cut-off voltage is 0.005-1.5V. The discharge rate is 0.1C to 0.005V, and then 0.02C to 0.005V to fully discharge it. The charge rate is 0.1C to 1.5V. The reversible capacity and first coulomb efficiency of the button battery are tested. The results are shown in Table 2 below.
[0167] The first charge and discharge curve of the button battery assembled in Example 1 is shown in Figure 4 .
[0168] 2. The silicon-carbon composite materials prepared in Examples 1 to 15 and Comparative Examples 1 to 6 were used as negative electrode materials to prepare small soft-pack batteries, and the specific steps were as follows:
[0169] The silicon-carbon composite negative electrode material and commercial artificial graphite (Yunnan Zhongsheng) were mixed in a mass ratio of 10:90 to form an active material with a capacity of 450mAh / g. The active material, binder lithium polyacrylate and conductive agent Super P were dispersed and slurried in a mass ratio of 95.5:4:0.5. After coating, rolling, slitting and other battery preparation processes, and matched with NCM811 positive electrode, a small soft-pack battery was made.
[0170] High temperature cycle performance test: At 60°C, charge the battery to 4.2V at 0.5C constant current and constant voltage, cut off current 0.02C, leave for 5 minutes, then discharge to 2.5V at 1C constant current, leave for 5 minutes. After 300 cycles of charge / discharge, calculate the 300th cycle capacity retention rate. The calculation formula is as follows:
[0171] The 300th cycle capacity retention rate at high temperature (%) = (300th cycle reversible capacity / 1st cycle reversible capacity) × 100%.
[0172] Figure 5 This is the cycle stability curve of the small soft-pack battery assembled in Example 1. The capacity retention rate data of the small soft-pack batteries assembled in each example and each comparative example at the 300th cycle at high temperature are listed in the following Table 2.
[0173] Table 2
[0174]
[0175]
Claims
1. A method for preparing a silicon-carbon composite material, characterized in that: The steps include: (1) mixing silicon-carbon dust removal powder with water to obtain a suspension, and blending the suspension with a polymer microsphere emulsion to obtain a slurry; The median particle size of the silicon-carbon dust removal powder is 0.1-3.0 μm; The polymer microsphere emulsion is prepared by using styrene monomers, propylene monomers and unsaturated alcohol monomers as raw materials and polymerized by an initiator. The styrene monomer is selected from one or more of styrene, 2-methylstyrene, 3-methylstyrene, 4-methylstyrene, 2-chlorostyrene, 3-chlorostyrene, 4-chlorostyrene, 2-fluorostyrene, 3-fluorostyrene, and 4-fluorostyrene; The acrylic monomer is selected from one or more of acrylic acid ester monomers, methacrylic acid ester monomers, acrylonitrile, and methacrylonitrile; The acrylic acid ester monomer is selected from one or more of methyl acrylate, ethyl acrylate, propyl acrylate, butyl acrylate, pentyl acrylate, hexyl acrylate, heptyl acrylate, octyl acrylate, nonyl acrylate, and decyl acrylate; The methacrylate monomer is selected from one or more of methyl methacrylate, ethyl methacrylate, propyl methacrylate, butyl methacrylate, pentyl methacrylate, hexyl methacrylate, heptyl methacrylate, octyl methacrylate, nonyl methacrylate, and decyl methacrylate; The unsaturated alcohol monomer is selected from one or more of propenol, butenol, pentenol, hexenol, heptenol, octenol, nonenol, decenol, 2-chloropropenol, and 3-chloro-propenol; Taking the total dry weight of the polymer microsphere emulsion as 100%, the raw material composition includes: Styrene monomer 30~45%; Propylene monomer 45~65%; Unsaturated alcohol monomer 0.5~15.0%; Initiator 0.01~2.0%; (2) spray drying the slurry to obtain a silicon-carbon material precursor; (3) subjecting the silicon-carbon material precursor to a high-temperature carbonization treatment to obtain the silicon-carbon composite material.
2. The method for preparing the silicon-carbon composite material according to claim 1, characterized in that: In step (1): The solid content of the suspension is 1-40wt%; The solid content of the polymer microsphere emulsion is 10-50wt%; The mass ratio of the dry weight of the silicon-carbon dust removal powder to the polymer microsphere emulsion is 1:0.1~0.
2.
3. The method for preparing the silicon-carbon composite material according to claim 1, characterized in that: Taking the total dry weight of the polymer microsphere emulsion as 100%, the content of the unsaturated alcohol monomer is 2-7%; The styrene monomer is selected from styrene; The acrylic monomer is selected from acrylic ester monomers and / or methacrylic ester monomers; The unsaturated alcohol monomer is selected from acryl alcohol.
4. The method for preparing the silicon-carbon composite material according to claim 1, characterized in that: In step (2): The spray drying has an air inlet temperature of 160-220° C., a feed rate of 0.01-3.0 kg / min, and an air pressure of 0.1-0.8 MPa.
5. The method for preparing the silicon-carbon composite material according to claim 1, characterized in that: In step (3): The heating carbonization treatment is carried out under an inert atmosphere, firstly heating to 250-400° C., keeping the temperature for 0.5-4.0 hours, then heating to 750-1000° C., keeping the temperature for 2-20 hours.
6. A silicon-carbon composite material prepared according to the method according to any one of claims 1 to 5, characterized in that: The invention comprises secondary particles of silicon-carbon material and a pyrolytic carbon layer covering the secondary particles of silicon-carbon material.
7. The silicon-carbon composite material according to claim 6, characterized in that: The median particle size of the silicon-carbon composite material is 5 to 13 μm; The thickness of the pyrolytic carbon layer is 5-10 nm; The specific surface area of the silicon-carbon composite material is 1 to 4 m 2 / g.
8. Use of the silicon-carbon composite material according to claim 6 or 7 in the preparation of lithium-ion batteries.
Citation Information
Patent Citations
Graphite silicon-based composite anode material and preparation method thereof
CN104362307A
Preparation method for silicon-carbon composite anode material of lithium ion battery
CN104916822A
Method for producing si / c composite particles
CN108701809A
High-molecular polymer composite coating material as well as preparation method and application thereof
CN114874576A
Method for producing si / c composite particles
US20200194778A1