Extreme ultraviolet (EUV) masks, methods for using EUV masks, and patterning methods

By using a cap feature material with low solid carbon solubility in the EUV mask, the effects of carbon contamination and oxidants on the EUV mask were resolved, achieving stable reflectivity and optimized exposure energy, thus improving the efficiency and economy of the lithography process.

CN115877649BActive Publication Date: 2026-11-17TAIWAN SEMICONDUCTOR MANUFACTURING CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202210859358.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2022-05-19
Filing Date
2022-07-21
Publication Date
2026-11-17
Estimated Expiration
2042-07-21

AI Technical Summary

Technical Problem

Existing extreme ultraviolet (EUV) masks are susceptible to carbon contamination and oxidants during manufacturing, leading to non-uniformity of critical dimensions and changes in reflectivity, increasing exposure energy requirements and affecting the efficiency and cost of photolithography processes.

Method used

The cap feature material with low solid carbon solubility, including an amorphous cap layer and a multilayer cap layer, is used to protect the reflective multilayer stack from carbon contamination and oxidants, and to achieve patterning by absorbing and reflecting incident radiation.

Benefits of technology

This improves the resistance of EUV masks to carbon contamination, maintains stable reflectivity, reduces exposure energy requirements, and enhances the efficiency and cost-effectiveness of the lithography process.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115877649B_ABST
    Figure CN115877649B_ABST
Patent Text Reader

Abstract

This disclosure relates to extreme ultraviolet (EUV) masks, methods of using EUV masks, and patterning methods. An EUV mask includes a substrate, a reflective multilayer stack on the substrate, and a single-layer or multilayer cap feature on the reflective multilayer stack. The cap feature includes one or more cap layers comprising a material having an amorphous structure. Other described embodiments include one or more cap layers comprising one or more elements having a first solid carbon solubility of less than about 3. In multilayer cap feature embodiments, the elements of each cap layer have different solid carbon solubility characteristics.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This disclosure generally relates to the field of semiconductor technology, and more specifically to extreme ultraviolet (EUV) masks, methods of using EUV masks, and patterning methods. Background Technology

[0002] The semiconductor industry has experienced exponential growth. Technological advancements in materials and design have led to multiple generations of integrated circuits (ICs), each featuring smaller and more complex circuits than the previous generation. In the evolution of ICs, functional density (i.e., the number of interconnect devices per chip area) typically increases, while geometry (i.e., the smallest component or line that can be produced using manufacturing processes) decreases. This miniaturization process generally provides the benefits of increased production efficiency and reduced associated costs.

[0003] Photolithography can be used to form components or lines on semiconductor wafers. One example of photolithography technology utilizes extreme ultraviolet (EUV) energy and a patterned absorption layer of an EUV mask. Summary of the Invention

[0004] According to one embodiment of the present disclosure, an extreme ultraviolet (EUV) mask is provided, comprising: a substrate; a reflective multilayer stack on the substrate; a cap feature on the reflective multilayer stack, the cap feature including a first cap layer comprising a material having an amorphous structure; and a patterned absorption layer on the cap feature.

[0005] According to another embodiment of this disclosure, a method of using an EUV mask is provided, the method comprising: exposing an EUV mask to incident radiation, the EUV mask comprising: a substrate; a reflective multilayer stack located on the substrate; a multilayer cap feature located on the reflective multilayer stack, the multilayer cap feature comprising a first cap layer and a second cap layer, the first cap layer comprising a first alloy containing Rh, Ir, Pt, Au, or Zr, the second cap layer comprising a second alloy containing Rh, Ir, Pt, Au, or Zr, the second alloy being different from the first alloy; and a patterned absorbing layer located on the multilayer cap feature; absorbing a portion of the incident radiation in the patterned absorbing layer; transmitting a portion of the incident radiation through the first cap layer and the second cap layer; reflecting a portion of the incident radiation from the reflective multilayer stack; and guiding the portion of the incident radiation reflected by the reflective multilayer stack to a material to be patterned.

[0006] According to another embodiment of this disclosure, a patterning method is provided, comprising: exposing an EUV mask to incident radiation, the EUV mask comprising: a substrate; a reflective multilayer stack located on the substrate; a cap feature located on the reflective multilayer stack, the cap feature comprising a material comprising an element having a solid carbon solubility of less than 3 atomic percent at the eutectic point of the element and carbon system; and a patterned absorbing layer located on the cap feature; absorbing a portion of the incident radiation in the patterned absorbing layer; absorbing a certain amount of the incident radiation in the cap feature; reflecting a portion of the incident radiation from the reflective multilayer stack; and guiding the portion of the incident radiation reflected by the reflective multilayer stack to the material to be patterned. Attached Figure Description

[0007] The various aspects of this disclosure can be best understood by reading in conjunction with the accompanying drawings through the following detailed description. It should be noted that, according to industry standard practice, the various features are not drawn to scale. In fact, for clarity of discussion, the dimensions of the various features may be arbitrarily enlarged or reduced.

[0008] Figure 1 This is a cross-sectional view of the extreme ultraviolet (EUV) mask according to the first embodiment.

[0009] Figure 2 It is according to some embodiments for manufacturing Figure 1 The flowchart of the EUV mask method.

[0010] Figures 3A to 3J It is based on some embodiments of the state Figure 2 Cross-sectional views of EUV masks at various stages of the manufacturing process.

[0011] Figure 4 This is a cross-sectional view of an extreme ultraviolet (EUV) mask according to the second embodiment.

[0012] Figure 5 It is according to some embodiments for manufacturing Figure 4 The flowchart of the EUV mask method.

[0013] Figures 6A to 6L It is based on some embodiments of the state Figure 5 Cross-sectional views of EUV masks at various stages of the manufacturing process.

[0014] Figure 7 This is a flowchart of a method for using an EUV mask according to some embodiments.

[0015] Figure 8 This is a flowchart of a method for using an EUV mask according to some embodiments.

[0016] Figure 9 This is a diagram illustrating the assessment results of the thickness of carbon contamination on the cap layer according to an embodiment of the present disclosure. Detailed Implementation

[0017] The following disclosure provides numerous different embodiments or examples for implementing various features of the proposed subject matter. Specific examples of components and arrangements are described below to simplify this disclosure. Of course, these are merely examples and not intended to be limiting. For example, in the following description, forming a first feature on or over a second feature may include embodiments in which the first and second features are formed in direct contact, and may also include embodiments in which an additional feature may be formed between the first and second features such that the first and second features are not in direct contact. Furthermore, reference numerals and / or letters may be repeated in various examples throughout this disclosure. Such repetition is for simplicity and clarity and does not in itself indicate a relationship between the various embodiments and / or configurations discussed.

[0018] In addition, this document may use spatially related terms (e.g., "below," "under," "down," "above," "up," etc.) to facilitate the description of the relationship between one element or feature shown in the accompanying drawings and another element(s) or feature(s). Besides the orientations shown in the accompanying drawings, these spatially related terms are also intended to cover different orientations of the device during use or operation. The device may be oriented in other ways (rotated 90 degrees or in other orientations), and the spatially related descriptors used herein can be interpreted similarly.

[0019] In the manufacture of integrated circuits (ICs), patterns representing the different layers of an IC are created using a series of reusable photomasks (also referred to herein as photolithographic masks or masks) to transfer the design of each layer of the IC onto a semiconductor substrate during the semiconductor device manufacturing process.

[0020] As IC dimensions shrink, extreme ultraviolet (EUV) light (e.g., with a wavelength of 13.5 nm) is employed in photolithography processes to enable the transfer of very small patterns (e.g., nanoscale patterns) from a mask to a semiconductor wafer. Since most materials have high absorptivity at 13.5 nm, EUV lithography uses a reflective EUV mask. This mask has a reflective multilayer for reflecting incident EUV light and an absorbing layer on top of the reflective multilayer for absorbing radiation in areas not intended to be reflected by the mask. The reflective multilayer and the absorbing layer are located on a substrate of low thermal expansion material. The reflective multilayer reflects the incident EUV light, and the patterned absorbing layer on top absorbs light in areas not intended to be reflected by the mask. The mask pattern is defined by the absorbing layer and transferred to the semiconductor wafer by reflecting EUV light away from the reflective surface portion of the EUV mask.

[0021] The ongoing demand for integrated devices with denser packaging has led to changes in photolithography processes to enable the formation of smaller individual feature sizes. The minimum feature size or “critical size” (CD) achievable by the process is approximately determined by the formula CD = k1 * λ / NA, where k1 is a process-specific coefficient, λ is the wavelength of the applied light / energy, and NA is the numerical aperture of the optical lens as viewed from the substrate or wafer.

[0022] This disclosure describes various embodiments of EUV masks that exhibit resistance to carbon contamination and utilize a durable cap feature that protects the underlying reflective multilayer stack from oxidants during mask fabrication, even after exposure to etching or cleaning processes. Carbon contamination can negatively impact the critical dimensions of features formed in the absorber layer and cap feature of the EUV mask. For example, some materials used as the cap layer may possess numerous free radicals that react with carbon atoms near the EUV mask surface during exposure to EUV energies. During exposure, hydrocarbon molecules near the EUV mask surface may break down upon exposure to high energies and deposit on the exposed surfaces of the EUV mask (e.g., sidewalls and bottom or trenches in the absorber material). The breakdown of hydrocarbon molecules may generate carbon atoms that can react with free radicals. It has been observed that the thickness of carbon deposited on the exposed surfaces of a mask located near the mask center is greater than that on the exposed surfaces located near the mask edges. In some embodiments, the amount of carbon formed on the exposed surface near the center of the mask is three times the thickness of the carbon formed on the exposed surface near the edges of the mask. Hydrocarbons can originate from a variety of sources, including gas release from materials within the EUV tool, such as the tool's structure, photoresist, or a hard mask used in the tool. The resulting carbon atoms or carbon-containing molecules react with or are absorbed by the material they come into contact with, and build up on the surface of the EUV mask. This carbon buildup on the surface of the EUV mask (e.g., the surface of the cap layer or the sidewalls of features in the absorbing material) negatively impacts the EUV mask's ability to pattern features on the substrate that satisfy critical dimensional conditions (e.g., critical dimensional uniformity (CDU)). For example, carbon absorbs EUV wavelengths more readily than other materials constituting the EUV mask. Therefore, when unwanted carbon is present on the EUV mask, the amount of exposure energy or incident EUV energy required to achieve the desired level of EUV radiation reflected from the mask is greater than when unwanted carbon is absent. In some embodiments, the exposure energy required when carbon is present on the EUV mask may be 10% or more higher than when carbon is absent, depending on the critical dimensions of the features on the wafer and the features on the mask. This increased exposure energy requirement will either increase the energy cost required for effective exposure of the wafer or increase the time required to achieve the desired exposure level.

[0023] Some embodiments of the EUV masks disclosed herein exhibit enhanced strength and / or resistance to etching and cleaning processes to which the EUV mask material is exposed during mask fabrication. This strength and / or resistance to etching and cleaning processes to which the EUV mask material is exposed during mask fabrication is important because weak or damaged layers of the mask are susceptible to infiltration of oxidants (e.g., oxygen). Oxygen infiltrating a damaged or weak layer of the mask can react with the material of the reflective multilayer and form an unwanted oxide layer on the top surface of the reflective multilayer.

[0024] Embodiments of this disclosure generally provide a photolithographic mask including a cap feature located on a reflective multilayer stack of the mask. In some embodiments, the cap feature includes a single cap material, while in other embodiments, the cap feature includes multiple cap layers of cap material. In some embodiments, the cap feature includes a first cap layer comprising a material having an amorphous structure. The first cap layer may be combined with a second cap layer comprising a material having an amorphous structure. In some embodiments, the material of the first cap layer includes an element having a solid carbon solubility of less than 3 atomic percent at the eutectic point of a system containing the element and carbon. Examples of elements that can be used in the cap layer of the cap feature according to embodiments of this disclosure include Rh, Ir, Pt, Au, and Zr or alloys thereof. In other embodiments, the cap layer of the cap feature according to embodiments of this disclosure includes Hf, Nb, or N. In other embodiments, the cap layer of the cap feature according to embodiments of this disclosure includes Ag or Cu. In other embodiments, the cap layer of the cap feature according to embodiments of this disclosure includes Pd. According to embodiments of this disclosure, a single-layer cap feature is employed to reduce carbon build-up or contamination on the surface of the EUV mask. The material of the cap layer formed according to this disclosure reduces the sensitivity of the cap feature to hydrocarbon molecule or carbon atom contamination. The material of the cap feature formed according to this disclosure also protects the underlying reflective multilayer from exposure to oxidants and the formation of unwanted oxide layers.

[0025] In examples of this disclosure relating to multilayer cap features, the material of one cap layer for the multilayer cap feature differs in composition from the material of another cap layer for the multilayer cap feature. Such a material may be consistent with the description in the preceding paragraphs concerning materials for cap features comprising only a single cap layer. In some embodiments, the material of one cap layer exhibits a different solid-state carbon solubility characteristic than the material of another cap layer of the multilayer cap feature. For example, in some embodiments, the multilayer cap feature is configured to include a first cap layer formed of a material comprising an element having a first carbon solubility characteristic. The multilayer cap feature includes at least another cap layer formed of a material comprising an element having a second carbon solubility characteristic, the second carbon solubility characteristic differing from the first carbon solubility characteristic of the element in the first cap layer. In some embodiments, the solid-state carbon solubility of the elements of the first and second cap layers at the eutectic point of the system containing the element and carbon is less than 3 atomic%. Solid-state carbon solubility characteristic refers to the maximum carbon solubility of the solid phase of the system in equilibrium with the liquid phase of the system at the eutectic point containing the element and carbon. The solid-state carbon solubility of the elements in the capping layer material is an indicator of the tendency of the elements in the capping layer to react with, retain, attract, or absorb carbon atoms or carbon-containing molecules. When carbon atoms are attracted to and retained by the capping layer material, or absorbed, or react with the capping layer material, they can accumulate and contaminate the capping layer. In some cases, the carbon accumulation or contamination completely covers the exposed portion of the capping layer. In other cases, the carbon accumulation or contamination partially covers the capping layer. In still other cases, the carbon accumulation or contamination at least partially covers some portions of the sidewalls of the mask's absorbing material. The presence of a carbon contamination layer alters the mask's dimensions and EUV transmission characteristics. This change in size and / or the change in incident EUV energy required to produce the desired intensity of reflected EUV energy can lead to the negative problems described in the preceding paragraphs. According to embodiments of this disclosure, a multilayer capping feature comprising multiple individual capping layers is employed to protect the EUV mask from carbon accumulation or contamination on the surface of the EUV mask. The material of the capping layer formed according to this disclosure reduces the sensitivity of the multilayer capping feature to contaminants having hydrocarbon molecules or carbon atoms. The material forming the cap feature according to this disclosure also protects the underlying reflective multilayer from exposure to oxidants and the formation of unwanted oxide layers.

[0026] In embodiments of this disclosure, the EUV mask includes a multilayer cap feature comprising at least one cap layer comprising a material containing an element with low solid-state carbon solubility. The solid-state carbon solubility of the element is characterized by the maximum carbon solubility of the solid phase of the system at equilibrium with the liquid phase of the system at the eutectic point of the element and carbon. An example of an element with low solid-state carbon solubility is an element having a solid-state carbon solubility of less than about 3 atomic percent. Examples of elements with low atomic percent solid-state carbon solubility include, but are not limited to, elements having a solid-state carbon solubility of less than about 3 atomic percent, and in some embodiments, elements having a solid-state carbon solubility of less than 2 atomic percent. For example, in some embodiments, the cap layer material does not have a solid-state carbon solubility of less than about 3 atomic percent, but still provides resistance to carbon build-up or contamination on the material surface. An element with low solid-state carbon solubility that can be used in embodiments of this disclosure may alternatively be characterized by an effective solid-state carbon solubility of less than 1.6 at 1000°C. The effective solid carbon solubility of this element at 1000°C is obtained by multiplying the solid carbon solubility value at the eutectic point by 1000°C / the eutectic point of the element and the carbon system. According to some embodiments of the multilayer cap feature of this disclosure, the solid carbon solubility of one or more elements of the material of one or more cap layers differs from the solid carbon solubility of one or more elements of the material of another cap layer forming the multilayer cap feature. In some embodiments, the material of at least one layer of the multilayer cap feature includes an element whose EUV extinction coefficient for EUV radiation at a wavelength of 13.5 nm is greater than or less than the EUV extinction coefficient for EUV radiation at a wavelength of 13.5 nm of an element of another layer of the multilayer cap feature. When the respective cap layers of the multilayer cap feature include materials containing elements with different EUV extinction coefficients for EUV radiation at a wavelength of 13.5 nm, the incident EUV energy absorbed in one cap layer differs quantitatively from the EUV energy absorbed in another cap layer of the multilayer cap feature. For example, in some embodiments, elements of the material of one cap layer have an EUV extinction coefficient between 0 and 0.1 for EUV radiation at a wavelength of 13.5 nm, while elements of the material of another cap layer have an EUV extinction coefficient for EUV radiation at a wavelength of 13.5 nm that is different from the EUV extinction coefficient of the elements of the first cap layer. In other embodiments, the material of the first cap layer includes elements having an EUV extinction coefficient between 0 and 0.08, between 0 and 0.06, or between 0 and 0.04 for EUV radiation at a wavelength of 13.5 nm. Materials including elements having EUV extinction coefficients within the aforementioned ranges for EUV radiation at a wavelength of 13.5 nm will not cause a reduction in transmitted EUV energy by an undesirable amount that would require an increase in the incident EUV energy level.The material of the cap layer used for the multi-layer cap feature according to this embodiment should not absorb EUV energy in amounts corresponding to: the amount of EUV energy required to be increased incident on the EUV mask, or the amount of exposure time required to be increased undesirably. Furthermore, the materials of the individual cap layer or the cap layer of the multi-layer cap feature according to the disclosed embodiments exhibit good adhesion to each other, and also good adhesion to: the material on which (one or more) cap layers are deposited, or the material deposited on (one or more) cap layers. Elements suitable as materials for cap layers according to embodiments of this disclosure include elements exhibiting a binding energy of less than about 285 electron volts (eV) to carbon. Examples of elements having a binding energy of less than about 285 eV to carbon include Rh, Ir, and Pt. Elements having a binding energy of less than about 285 eV to carbon are not limited to Rh, Ir, and Pt. Other elements having a binding energy of less than about 285 eV to carbon may also be used as elements for materials in cap layers according to this disclosure.

[0027] In some embodiments, the cap feature includes at least one cap layer comprising rhodium (Rh), iridium (Ir), platinum (Pt), gold (Au), and / or zirconium (Zr) or alloys thereof. Examples of alloys of Rh, Ir, Pt, Au, or Zr include RuZr, IrZr, RhZr, HfZr, NbZr, and ZnZr. Other examples of alloys of Rh, Ir, Pt, Au, or Zr according to this disclosure include RuRh, RuIr, RuPt, PtIr, RuIrPt, NbIr, NbPt, NbRh, RhN, IrN, RuRhN, RuIrN, RuPtN, PtIrN, RuIrPtN, NbIrN, NbPtN, and NbRhN. For example, the cap layer according to this disclosure may include alloys, such as RuRh (5at% to 100at% Rh), RuIr (5at% to 100at% Ir), RuPt (5at% to 100at% Pt), PtIr (5at% to 100at% Ir), RuIrPt (5at% to 100at% Ir), RuIrPt (5at% to 100at% Pt), NbIr (5at% to 100at% Ir), NbPt (5at% to 100at% Pt), NbRh (5at% to 100at% Rh), RhN (5at% to 100at% Rh), IrN (5at% to 100at% Ir), RuRhN (5at% to 100at% Rh), RuRh N (5at%~100at%N), RuIrN (5at%~100at%Ir), RuIrN (5at%~100at%N), RuPtN (5at% ~100at%Pt), RuPtN (5at% ~ 100at%N), PtIrN (5at% ~ 100at%Ir), PtIrN (5at% ~ 100at %N), RuIrPtN (5at%~100at%Ir), RuIrPtN (5at%~100at%Pt), RuIrPtN (5at%~100a t%N), NbIrN (5at%~100at%Ir), NbPtN (5at%~100at%Pt) or NbRhN (5at%~100at%Rh). In other embodiments, the capping layer according to this disclosure may include an alloy containing Hf, Nb, or N. In other embodiments, the capping layer according to this disclosure may include an alloy containing Ag or Cu. In other embodiments, the capping layer according to this disclosure may include an alloy containing Pd.

[0028] In some embodiments, the single-layer or multi-layer cap feature includes at least one layer comprising a material containing elements having a refractive index greater than 0.87 and less than 0.97. Examples of materials having a refractive index greater than 0.87 and less than 0.97 include, but are not limited to, the materials described above.

[0029] Figure 1 This is a cross-sectional view of the EUV mask 100 according to the first embodiment of this disclosure. (Refer to...) Figure 1 The EUV mask 100 includes a substrate 102, a reflective multilayer stack 110 on the front side of the substrate 102, a cap feature 125 on the reflective multilayer stack 110, and a patterned absorption layer 140P on the cap feature 125, wherein the cap feature 125 includes a patterned first cap layer 120P. The EUV mask 100 also includes a conductive layer 104 on the back side of the substrate 102 opposite to the front side.

[0030] The patterned absorber layer 140P includes a pattern of openings 152, the pattern of which corresponds to a pattern of conductive or non-conductive features to be formed on or in a semiconductor wafer. The pattern of openings 152 is located in a patterned region 100A of the EUV mask 100 that exposes the surface of the patterned first capping layer 120P. The patterned region 100A is surrounded by a peripheral region 100B of the EUV mask 100. The peripheral region 100B corresponds to a non-patterned region of the EUV mask 100 that is not used for exposure processes during IC manufacturing. In some embodiments, the patterned region 100A of the EUV mask 100 is located in the central region of the substrate 102, and the peripheral region 100B is located at the edge portion of the substrate 102. The patterned region 100A is separated from the peripheral region 100B by a trench 154. The trench 154 extends through the patterned absorber layer 140P, the patterned first capping layer 120P, and the reflective multilayer stack 110, exposing the front side of the substrate 102.

[0031] According to some embodiments of this disclosure, the patterned absorption layer 140P is a layer of absorption material, which is an alloy of a transition metal and at least one alloying element. The transition metal is, for example, tantalum (Ta), ruthenium (Ru), chromium (Cr), platinum (Pt), gold (Au), iridium (Ir), titanium (Ti), niobium (Nb), rhodium (Rh), molybdenum (Mo), tungsten (W), or palladium (Pd). The at least one alloying element is selected from: ruthenium (Ru), chromium (Cr), tantalum (Ta), platinum (Pt), palladium (Pd), tungsten (W), gold (Au), iridium (Ir), titanium (Ti), niobium (Nb), rhodium (Rh), molybdenum (Mo), hafnium (Hf), boron (B), nitrogen (N), oxygen (O), silicon (Si), zirconium (Zr), or vanadium (V).

[0032] Figure 2This is a flowchart of a method 200 for manufacturing an EUV mask (e.g., EUV mask 100) according to embodiments of the present disclosure. Figure 3A Figure 3L is a cross-sectional view of an EUV mask 100 at various stages of the manufacturing process according to some embodiments. Method 200 is discussed in detail below with reference to EUV mask 100. In some embodiments, additional operations are performed before, during, and / or after method 200, or some of the operations described are replaced and / or eliminated. In some embodiments, some of the features described below are replaced or eliminated. Those skilled in the art will understand that although some embodiments have been discussed using operations performed in a particular order, these operations may be performed in a different logical order.

[0033] Reference Figure 2 and Figure 3A According to some embodiments, method 200 includes operation 202, in which a reflective multilayer stack 110 is formed on substrate 102. Figure 3A This is a cross-sectional view of the initial structure of an EUV mask 100 after a reflective multilayer stack 110 has been formed on a substrate 102, according to some embodiments.

[0034] Reference Figure 3A The initial structure of the EUV mask 100 includes a substrate 102 made of glass, silicon, quartz, or other low thermal expansion materials. Low thermal expansion materials help minimize pattern distortion caused by heat during use of the EUV mask 100. In some embodiments, the substrate 102 includes fused silicon, fused silica, calcium fluoride, silicon carbide, black diamond, or titanium oxide-doped silicon oxide (SiO2 / TiO2). In some embodiments, the thickness of the substrate 102 ranges from about 1 mm to about 7 mm. In some examples, if the thickness of the substrate 102 is too small, the risk of breakage or warping of the EUV mask 100 increases. On the other hand, in some examples, if the thickness of the substrate is too large, the weight and cost of the EUV mask 100 unnecessarily increase.

[0035] In some embodiments, a conductive layer 104 is disposed on the back side of a substrate 102. In some embodiments, the conductive layer 104 is in direct contact with the back side of the substrate 102. The conductive layer 104 is adapted to provide electrostatic coupling between the EUV mask 100 and an electrostatic mask jig (not shown) during the fabrication and use of the EUV mask 100. In some embodiments, the conductive layer 104 comprises chromium nitride (CrN) or tantalum boride (TaB). In some embodiments, the conductive layer 104 is formed by a deposition process such as chemical vapor deposition (CVD), plasma-enhanced chemical vapor deposition (PECVD), or physical vapor deposition (PVD). The thickness of the conductive layer 104 is controlled such that the conductive layer 104 is optically transparent.

[0036] A reflective multilayer stack 110 is disposed on the front side of the substrate 102, opposite to the back side. In some embodiments, the reflective multilayer stack 110 is in direct contact with the front side of the substrate 102. The reflective multilayer stack 110 provides high reflectivity to EUV light. In some embodiments, the reflective multilayer stack 110 is configured to achieve a reflectivity of about 60% to about 75% at the peak EUV irradiation wavelength (e.g., EUV irradiation at 13.5 nm). Specifically, when EUV light is applied to the surface of the reflective multilayer stack 110 at an incident angle of 6°, the maximum reflectivity of light near the 13.5 nm wavelength is about 60%, about 62%, about 65%, about 68%, about 70%, about 72%, or about 75%.

[0037] In some embodiments, the reflective multilayer stack 110 comprises alternating layers of high-refractive-index material and low-refractive-index material. On the one hand, materials with high refractive indices tend to scatter EUV light, while on the other hand, materials with low refractive indices tend to transmit EUV light. Pairing these two types of materials together provides a resonant reflectivity. In some embodiments, the reflective multilayer stack 110 comprises alternating layers of molybdenum (Mo) and silicon (Si). In some embodiments, the reflective multilayer stack 110 comprises alternating layers of Mo and Si, with Si located on the top layer. In some embodiments, the molybdenum layer is in direct contact with the front side of the substrate 102. In some other embodiments, the silicon layer is in direct contact with the front side of the substrate 102. Alternatively, the reflective multilayer stack 110 comprises alternating layers of Mo and beryllium (Be).

[0038] The thickness of each layer in the reflective multilayer stack 110 depends on the EUV wavelength and the incident angle of the EUV light. The thickness of the alternating layers in the reflective multilayer stack 110 is adjusted to maximize the constructive interference of the EUV light reflected at each interface and minimize the overall absorption of the EUV light. In some embodiments, the reflective multilayer stack 110 includes 30 to 60 pairs of alternating Mo and Si layers. The thickness of each Mo / Si pair ranges from about 2 nm to about 7 nm, and the total thickness ranges from about 100 nm to about 300 nm. In some embodiments, the thickness of the alternating layers in the reflective multilayer stack 110 is different.

[0039] In some embodiments, the layers in the reflective multilayer stack 110 are deposited on and beneath the substrate 102 using ion beam deposition (IBD) or DC magnetron sputtering. The deposition method used helps ensure that the thickness uniformity of the reflective multilayer stack 110 on the substrate 102 is better than about 0.85. For example, to form the Mo / Si reflective multilayer stack 110, a Mo target is used as the sputtering target and argon (Ar) gas (at a pressure of 1.3 × 10⁻⁶) is used. -2 Pa up to 2.7 × 10 -2Mo layers were deposited using an ion acceleration voltage of 300V to 1500V and a deposition rate of 0.03nm / sec to 0.30nm / sec, with a Si target as the sputtering gas and Ar gas (pressure 1.3 × 10⁻⁶ Pa) as the sputtering gas. -2 Pa up to 2.7 × 10 -2 Si layers are deposited using Pa as the sputtering gas and an ion acceleration voltage of 300V to 1500V at a deposition rate of 0.03nm / sec to 0.30nm / sec. A Mo / Si reflective multilayer stack is deposited by stacking Si and Mo layers for 40 to 50 cycles, each cycle including the above steps.

[0040] Reference Figure 2 and Figure 3B According to some embodiments, method 200 proceeds to operation 204, in which a first capping layer 120 is deposited on the reflective multilayer stack 110. Figure 3B According to some embodiments Figure 3A The structure is a cross-sectional view after the first capping layer 120 is deposited on the reflective multilayer stack 110.

[0041] Reference Figure 3B , ( Figure 1 and Figure 3C The first cap layer 120 (of the cap feature 125) is disposed on the topmost surface of the reflective multilayer stack 110. As described herein, the first cap layer 120 comprises a material in an amorphous state. In some embodiments, the material has low solid carbon solubility, which serves to prevent carbon contamination of the mask or reduce the amount of carbon contamination in the mask.

[0042] Materials in an amorphous state include those that are solid and lack long-range order (a characteristic of crystals). Materials in an amorphous state are sometimes referred to as being in a glassy or glassy state. "Glassy solid" or "amorphous solid" is considered a general concept, with glass being the specific case; glass is an amorphous solid stable below its glass transition temperature. Polymers are typically amorphous. Other types of amorphous solids include gels, thin films, and nanostructured materials. Materials in an amorphous state have an internal structure composed of interconnected structural blocks. These blocks can be analogous to the basic structural units found in the corresponding crystalline phases of the same material. Nanocrystalline materials are examples of materials in an amorphous state and are characterized in this disclosure by grain sizes less than 5 nm, less than 4 nm, less than 3 nm, or less than 2 nm. Materials in an amorphous state that can be used as capping layers according to this disclosure include the materials described above for capping layers.

[0043] In some embodiments, the first capping layer 120 comprises a material less susceptible to carbon contamination compared to conventional materials used as capping layers. Such materials have been described above. As mentioned above, such materials comprise elements having a low effective solid carbon solubility in that element at 1000°C, for example, less than 1.6 atomic percent effective solid carbon solubility at 1000°C. Other examples of materials comprising elements having a low atomic percentage effective solid carbon solubility at 1000°C include, but are not limited to, materials comprising elements having an effective solid carbon solubility of less than about 1.3 atomic percent at 1000°C. In some embodiments, the capping layer material comprises elements that do not have an effective solid carbon solubility of less than about 1.6 atomic percent or less than about 1.3 atomic percent, but still provide resistance to carbon build-up or contaminants on the material surface. Figure 1In some embodiments, the material of the first cap layer 120 includes elements having an EUV extinction coefficient between 0 and 0.1, 0 and 0.08, 0 and 0.06, 0 and 0.04, or 0 and 0.02 for EUV radiation at a wavelength of 13.5 nm. Materials including elements having EUV extinction coefficients within the aforementioned range for EUV radiation at a wavelength of 13.5 nm will not reduce the transmitted EUV energy by an amount that would require an undesirable increase in the incident EUV energy level. The material of the cap layer for the cap feature according to this embodiment should not absorb an amount of EUV energy that would be large enough to require an increase in the amount of EUV energy incident on the EUV mask, or an undesirable increase in the exposure time. Furthermore, the material of the cap layer for the cap feature according to this embodiment exhibits good adhesion to materials on which the cap layer is deposited, or materials deposited on the cap layer. According to embodiments of this disclosure, carbides of the aforementioned elements are unsuitable as materials for the first cap layer 120 because carbon atoms from the carbides may diffuse into the underlying layers during their heat treatment. In some embodiments, the multilayer cap feature 125 includes at least one layer 120 comprising a material containing an element having a refractive index less than 0.97 for EUV radiation at a wavelength of 13.5 nm. In some embodiments, the multilayer cap feature 125 includes at least one layer 120 comprising a material containing an element having a refractive index greater than 0.87 for EUV radiation at a wavelength of 13.5 nm. Examples of materials containing elements having a refractive index less than 0.97 or greater than 0.87 for EUV radiation at a wavelength of 13.5 nm include, but are not limited to, the materials described above. In some embodiments, the thickness of the first cap layer 120 ranges from about 0.5 nm to 5 nm. A thickness of the first cap layer 120 ranging from about 0.5 nm to 5 nm is sufficient to prevent or reduce carbon contamination without being so thick as to cause an undesirable reduction in EUV transmission. Embodiments of this disclosure are not limited to EUV masks including a first capping layer 120 having a thickness of 0.5 nm to about 5 nm. Embodiments of this disclosure also include: EUV masks including a first capping layer 120 having a thickness of less than 0.5 nm, and EUV masks including a first capping layer 120 having a thickness of greater than about 5 nm.

[0044] In some embodiments, a deposition process such as IBD, chemical vapor deposition (CVD), physical vapor deposition (PVD), atomic layer deposition (ALD), thermal ALD, PE-ALD, PECVD, electron beam evaporation, thermal evaporation, ion beam induced deposition, sputtering, electrodeposition, or electrodeposition-free deposition is used to form the first capping layer 120.

[0045] Reference Figure 2 and Figure 3CAccording to various embodiments, method 200 proceeds to operation 208, in which an absorber layer 140 is deposited on the first cap layer 120. Figure 3C According to some embodiments Figure 3B The structure is a cross-sectional view after the absorption layer 140 is deposited on the first cap layer 120.

[0046] Reference Figure 3C The absorption layer 140 is configured to be in direct contact with the first cap layer 120. The absorption layer 140 can be used to absorb EUV wavelength radiation projected onto the EUV mask 100.

[0047] The absorbing layer 140 comprises an absorbing material having a high extinction coefficient κ and a low refractive index n for EUV wavelengths. In some embodiments, the absorbing layer 140 comprises an absorbing material having a high extinction coefficient and a low refractive index at a wavelength of 13.5 nm. In other embodiments, the absorbing layer comprises an absorbing material having a low extinction coefficient and a high refractive index for EUV radiation at a wavelength of 13.5 nm. According to some embodiments of this disclosure, the refractive index and extinction coefficient of the material of the absorbing layer 140 are related to light at a wavelength of about 13.5 nm. According to some embodiments, the thickness of the absorbing layer 140 is less than about 80 nm. According to other embodiments, the thickness of the absorbing layer 140 is less than about 60 nm. Other embodiments use an absorbing layer 140 with a thickness of less than about 50 nm.

[0048] In some embodiments, the absorbent material is in a polycrystalline state, characterized by having grains, grain boundaries, and different forming phases. In other embodiments, the absorbent material is in an amorphous state, for example, characterized by having grains smaller than 5 nanometers, smaller than 3 nanometers, smaller than 2 nanometers, or without grain boundaries, and a single phase. According to some embodiments of this disclosure, the absorbent material includes interstitial elements selected from nitrogen (N), oxygen (O), boron (B), carbon (C), or combinations thereof. As used herein, an interstitial element refers to an element located in the interstices between materials comprising a main alloy and alloying elements in the absorbent material formed according to this disclosure.

[0049] The absorber layer 140 is formed using deposition techniques such as PVD, CVD, ALD, RF magnetron sputtering, DC magnetron sputtering, or IBD. The deposition process can be performed in the presence of an element described as an interstitial element (e.g., B or N). Performing deposition in the presence of an interstitial element results in the interstitial element being included in the material of the absorber layer 140.

[0050] According to embodiments of this disclosure, various combinations of alloy materials from different families can be used as absorbent materials. Each of the different alloys from different families includes a main alloying element selected from transition metals and at least one alloying element. According to some embodiments, the main alloying element accounts for up to 90 atomic percent of the alloy used as an absorbent material. In some embodiments, the main alloying element accounts for more than 50 atomic percent of the alloy used as an absorbent material. In some embodiments, the main alloying element accounts for about 50 to 90 atomic percent of the alloy used as an absorbent material.

[0051] According to some embodiments, the main alloying element is a transition metal selected from the following: ruthenium (Ru), chromium (Cr), tantalum (Ta), platinum (Pt), gold (Au), iridium (Ir), titanium (Ti), niobium (Nb), rhodium (Rh), molybdenum (Mo), tungsten (W), and palladium (Pd). According to some embodiments, at least one alloying element is a transition metal, a metalloid, or a reactive nonmetal. Examples of at least one alloying element as a transition metal include ruthenium (Ru), chromium (Cr), tantalum (Ta), platinum (Pt), palladium (Pd), tungsten (W), gold (Au), iridium (Ir), titanium (Ti), niobium (Nb), rhodium (Rh), molybdenum (Mo), hafnium (Hf), zirconium (Zr), and vanadium (V). Examples of at least one alloying element as a metalloid include boron (B) and silicon (Si). Examples of at least one alloying element as a reactive nonmetal include nitrogen (N) or oxygen (O).

[0052] Different materials can be used to etch the different absorbent materials disclosed herein, and different materials can be used as hard mask layers with different absorbent materials. For example, in some embodiments, the absorbent layer 140 is dry-etched using a chlorine-containing gas or a fluorine-containing gas, such as Cl2 or BCl3, and the fluorine-containing gas such as NF3. Ar can be used as a carrier gas. In some embodiments, oxygen (O2) may also be included as a carrier gas. For example, a chlorine-based etchant, a chlorine-oxygenated etchant, or an etchant that is a mixture of chlorine-based and fluorine-based (e.g., carbon tetrafluoride and carbon tetrachloride) will etch an alloy comprising a main alloying element and at least one alloying element, the main alloying element comprising ruthenium (Ru), chromium (Cr), tantalum (Ta), platinum (Pt), or gold (Au), the at least one alloying element being selected from ruthenium (Ru), chromium (Cr), tantalum (Ta), platinum (Pt), palladium (Pd), tungsten (W), gold (Au), iridium (Ir), niobium (Nb), rhodium (Rh), molybdenum (Mo), hafnium (Hf), or vanadium (V). In some embodiments, fluorine-based etchants are suitable for etching alloys in which the main alloying element includes iridium (Ir), titanium (Ti), niobium (Ni), or rhodium (Rh), and at least one alloying element is selected from boron (B), nitrogen (N), oxygen (O), silicon (Si), tantalum (Ta), zirconium (Zr), niobium (Ni), molybdenum (Mo), rhodium (Rh), titanium (Ti), or ruthenium (Ru). In some embodiments, fluorine-based etchants or fluorine-based oxygen-added etchants are suitable for etching alloys in which the main alloying element includes molybdenum (Mo), tungsten (W), or palladium (Pd), and at least one alloying element is selected from ruthenium (Ru), palladium (Pd), tungsten (W), iridium (Ir), titanium (Ti), niobium (Nb), rhodium (Rh), molybdenum (Mo), silicon (Si), or zirconium (Zr).

[0053] According to some embodiments, SiN, TaBO, TaO, SiO, SiON, and SiOB are examples of materials that can be used for the hard mask layer 160 using the following alloys for the absorber layer 140: the main alloying element of the alloy includes ruthenium (Ru), chromium (Cr), tantalum (Ta), platinum (Pt), or gold (Au), and at least one alloying element of the alloy is selected from ruthenium (Ru), chromium (Cr), tantalum (Ta), platinum (Pt), palladium (Pd), tungsten (W), gold (Au), iridium (Ir), niobium (Nb), rhodium (Rh), molybdenum (Mo), hafnium (Hf), or vanadium (V). CrO and CrON are examples of materials that can be used for the hard mask layer 160 of the absorber layer 140 using the following alloys: the main alloying element of the alloy includes iridium (Ir), titanium (Ti), niobium (Ni), or rhodium (Rh), and at least one alloying element of the alloy is selected from boron (B), nitrogen (N), oxygen (O), silicon (Si), tantalum (Ta), zirconium (Zr), niobium (Ni), molybdenum (Mo), rhodium (Rh), titanium (Ti), or ruthenium (Ru). SiN, TaBO, TaO, CrO, and CrON are examples of materials that can be used for the hard mask layer 160 of the absorber layer 140 using the following alloys: the main alloying element of the alloy includes molybdenum (Mo), tungsten (W), or palladium (Pd), and at least one alloying element of the alloy is selected from ruthenium (Ru), palladium (Pd), tungsten (W), iridium (Ir), titanium (Ti), niobium (Nb), rhodium (Rh), molybdenum (Mo), silicon (Si), or zirconium (Zr). In other embodiments, a buffer layer (not shown) with a composition similar to the hard mask layer may be present between the cap feature 125 and the absorbent material layer 140. In some embodiments, the material of the hard mask layer 160 may be the same as or different from the material of the buffer layer. Embodiments of the invention are not limited to the types of materials described above for the hard mask layer 160 or the buffer layer.

[0054] In some embodiments, the absorber layer 140 is deposited as an amorphous layer. By maintaining the amorphous phase, the overall roughness of the absorber layer 140 is improved. The thickness of the absorber layer 140 is controlled to provide an absorption rate between 95% and 99.5% for EUV light at 13.5 nm. In some embodiments, the thickness of the absorber layer 140 can range from about 30 nm to about 70 nm. Embodiments according to this disclosure include absorber layers having thicknesses of less than 30 nm and greater than 70 nm. If the thickness of the absorber layer 140 is too small, the absorber layer 140 cannot absorb a sufficient amount of EUV light to produce contrast between reflective and non-reflective regions. On the other hand, if the thickness of the absorber layer 140 is too large, the precision of the pattern formed in the absorber layer 140 is generally low.

[0055] Reference Figure 2 and Figure 3DAccording to some embodiments, method 200 proceeds to operation 210, in which a resist stack including a hard mask layer 160 and a photoresist layer 170 is deposited on absorber layer 140. Figure 3D According to some embodiments Figure 3C The structure is a cross-sectional view after the hard mask layer 160 and the photoresist layer 170 are sequentially deposited on the absorber layer 140.

[0056] Reference Figure 3D A hard mask layer 160 is disposed on the absorber layer 140. In some embodiments, the hard mask layer 160 is in direct contact with the absorber layer 140. In some embodiments, the hard mask layer 160 comprises a dielectric oxide or a dielectric nitride, such as silicon dioxide or silicon nitride. In some embodiments, the hard mask layer 160 is formed using a deposition process such as CVD, PECVD, or PVD. In some embodiments, the thickness of the hard mask layer 160 ranges from about 2 nm to 10 nm. Embodiments of this disclosure are not limited to hard mask layers 160 with a thickness ranging from about 2 nm to 10 nm.

[0057] A photoresist layer 170 is disposed on the hard mask layer 160. The photoresist layer 170 includes a photosensitive material operable to be patterned by radiation. In some embodiments, the photoresist layer 170 includes a positive photoresist material, a negative photoresist material, or a hybrid photoresist material. In some embodiments, the photoresist layer 170 is applied to the surface of the hard mask layer 160, for example, by spin coating.

[0058] Reference Figure 2 and Figure 3E According to some embodiments, method 200 proceeds to operation 212, in which the photoresist layer 170 is photolithographically patterned to form a patterned photoresist layer 170P. Figure 3E According to some embodiments Figure 3D The structure is a cross-sectional view after the photoresist layer 170 was photolithographically patterned to form the patterned photoresist layer 170P.

[0059] Reference Figure 3EFirst, the photoresist layer 170 is patterned by subjecting it to patterning irradiation. Next, depending on whether a positive or negative resist is used in the photoresist layer 170, the exposed or unexposed portions of the photoresist layer 170 are removed using a resist developer, thereby forming a patterned photoresist layer 170P with a pattern of openings 172. Openings 172 expose portions of the hard mask layer 160. Openings 172 are located in the patterned area 100A and appear alongside the pattern of openings 152 on the EUV mask 100. Figure 1 The position corresponds to the one in the diagram.

[0060] Reference Figure 2 and Figure 3F According to some embodiments, method 200 proceeds to operation 214, in which a patterned photoresist layer 170P is used as an etch mask to etch a hard mask layer 160 to form a patterned hard mask layer 160P. Figure 3F According to some embodiments Figure 3E The structure is a cross-sectional view after etching the hard mask layer 160 to form a patterned hard mask layer 160P.

[0061] Reference Figure 3F The portion of the hard mask layer 160 exposed by the opening 172 is etched to form an opening 162 extending through the hard mask layer 160. The opening 162 exposes portions of the underlying absorber layer 140. In some embodiments, the hard mask layer 160 is etched using anisotropic etching with a fluorine-containing gas or a chlorine-containing gas (e.g., CF4, SF6, or Cl2). In some embodiments, the anisotropic etching is dry etching (e.g., reactive ion etching (RIE)), wet etching, or a combination thereof. This etching removes material providing the hard mask layer 160 and optionally material providing the absorber layer 140. The remaining portion of the hard mask layer 160 constitutes a patterned hard mask layer 160P. If the patterned photoresist layer 170P is not completely consumed during the etching of the hard mask layer 160, the patterned photoresist layer 170P is removed from the surface of the patterned hard mask layer 160P after etching, for example, by wet stripping or plasma ashing followed by wet cleaning.

[0062] Reference Figure 2 and Figure 3G According to some embodiments, method 200 proceeds to operation 216, in which a patterned hard mask layer 160P is used as an etch mask to etch the absorber layer 140 to form the patterned absorber layer 140P. Figure 3G According to some embodiments Figure 3F The structure is a cross-sectional view after etching the absorption layer 140 to form the patterned absorption layer 140P.

[0063] Reference Figure 3G The portion of the absorber layer 140 exposed by the opening 162 is etched to form an opening 142 extending through the absorber layer 140. The opening 142 exposes a portion of the first capping layer 120. In some embodiments, an anisotropic etching process is used to etch the absorber layer 140. In some embodiments, the anisotropic etching is a dry etching (e.g., RIE), wet etching, or a combination thereof, which removes material providing the absorber layer 140 and optionally removes material providing the underlying first capping layer 120. For example, in some embodiments, the absorber layer 140 is dry-etched using a chlorine-containing gas or a fluorine-containing gas, such as Cl2 or BCl3, and such as CF4, SF3, or NF3. Ar can be used as a carrier gas. In some embodiments, oxygen (O2) may also be included as a carrier gas. The etching rate and etching selectivity depend on the etchant gas, etchant flow rate, power, pressure, and substrate temperature. After etching, the remaining portion of the absorber layer 140 constitutes a patterned absorber layer 140P. According to embodiments of this disclosure, when the absorbent layer 140 comprises multiple layers of absorbent material, and when each layer of absorbent material has different etching properties, different etchants can be used to etch each layer of absorbent material individually. When each layer of absorbent material does not have different etching properties, each layer of absorbent material can be etched simultaneously.

[0064] In some embodiments, etching of the absorber layer 140 also removes a portion of the first capping layer 120. In other embodiments, etching of the absorber layer 140 does not remove any portion of the first capping layer 120. The opening 142 exposes the portion of the first capping layer 120 located at the bottom of the trench formed in the absorber layer 140. After etching the absorber layer 140, the patterned hard mask layer 160P is removed from the surface of the patterned absorber layer 140P, for example, using oxygen plasma or wet etching.

[0065] The openings 142 in the patterned absorber layer 140P define the pattern of the openings 152 in the EUV mask 100. According to embodiments of this disclosure, the portion of the patterned first capping layer 120 exposed through the patterned absorber layer 140 exhibits reduced sensitivity to carbon deposition or carbon contamination. Furthermore, due to the amorphous structure of the material of the first capping layer 120, the first capping layer 120 resists weakening caused by etchants, cleaning agents, or processes using such etchants or cleaning agents performed during the manufacture of the EUV mask 100. This resistance to weakening caused by etchants, cleaning agents, or processes using such etchants or cleaning agents not only increases the mask's lifetime but also increases the first capping layer 120's resistance to oxidant penetration, which can react with the underlying reflective multilayer stack to form unwanted oxides.

[0066] Reference Figure 2 and Figure 3H According to some embodiments, method 200 proceeds to operation 220, in which a patterned photoresist layer 180P including a pattern of openings 182 is formed on the patterned absorber layer 140P and the first capping layer 120. Figure 3H According to some embodiments Figure 3G The structure is a cross-sectional view after a patterned photoresist layer 180P including an opening 182 is formed on the patterned absorption layer 140P and the first capping layer 120.

[0067] Reference Figure 3H The opening 182 exposes a portion of the patterned absorber layer 140P located at the periphery of the patterned absorber layer 140P. The opening 182 corresponds to the trench 154 to be formed in the peripheral region 100B of the EUV mask 100. To form the patterned photoresist layer 180P, a photoresist layer (not shown) is applied to the first capping layer 120 and the patterned absorber layer 140P. The photoresist layer fills the openings located in the patterned absorber layer 140P. In some embodiments, the photoresist layer includes a positive photoresist material, a negative photoresist material, or a hybrid photoresist material. In some embodiments, the photoresist layer includes materials that are compatible with the above-mentioned materials. Figure 3D The photoresist layer 170 described herein is made of the same material. In some embodiments, the photoresist layer comprises a different material from the photoresist layer 170. In some embodiments, the photoresist layer is formed, for example, by spin coating. The photoresist layer is then patterned by exposing the photoresist layer to a radiation pattern and removing the exposed or unexposed portions of the photoresist layer using a resist developer, depending on whether a positive or negative resist is used. The remaining portion of the photoresist layer constitutes the patterned photoresist layer 180P.

[0068] Reference Figure 2 and Figure 3I According to some embodiments, method 200 proceeds to operation 222, in which a patterned photoresist layer 180P is used as an etching mask to etch a patterned absorber layer 140P, a first capping layer 120 and a reflective multilayer stack 110 to form a trench 154 in a peripheral region 100B of the substrate 102. Figure 3I The cross-sectional view of FIG3K according to some embodiments is after etching a patterned absorption layer 140P, a first capping layer 120 and a reflective multilayer stack 110 to form a trench 154 in the peripheral region 100B of the substrate 102.

[0069] Reference Figure 3IThe trench 154 extends through the patterned absorption layer 140P, the first capping layer 120, and the reflective multilayer stack 110 to expose the surface of the substrate 102. The trench 154 surrounds the patterned region 100A of the EUV mask 100, separating the patterned region 100A from the peripheral region 100B.

[0070] In some embodiments, a single anisotropic etching process is used to etch the patterned absorber layer 140P, the first cap layer 120, and the reflective multilayer stack 110. The anisotropic etching can be dry etching (e.g., RIE), wet etching, or a combination thereof, which removes corresponding material from the patterned absorber layer 140P, the first cap layer 120, and the reflective multilayer stack 110, optionally removing material providing the substrate 102. In some embodiments, multiple different anisotropic etching processes are used to etch the patterned absorber layer 140P, the first cap layer 120, and the reflective multilayer stack 110. Each anisotropic etching can be dry etching (e.g., RIE), wet etching, or a combination thereof.

[0071] Reference Figure 2 and Figure 3J According to some embodiments, method 200 proceeds to operation 224, in which the patterned photoresist layer 180P is removed. Figure 3J According to some embodiments Figure 3I The cross-sectional view of the structure after the patterned photoresist layer 180P has been removed.

[0072] Reference Figure 3J For example, the patterned photoresist layer 180P is removed from the patterned region 100A and peripheral region 100B of the substrate 102 by wet stripping or plasma ashing. Removing the patterned photoresist layer 180P from the opening 142 in the patterned absorber layer 140P re-exposes the surface of the first capping layer 120 located in the patterned region 100A.

[0073] This forms an EUV mask 100. The EUV mask 100 includes a substrate 102, a reflective multilayer stack 110 on the front side of the substrate 102, a first capping layer 120P on the reflective multilayer stack 110, and a patterned absorption layer 140P on the first capping layer 120. The EUV mask 100 also includes a conductive layer 104 on the back side of the substrate 102 opposite to the front side. According to embodiments of this disclosure, the first capping layer 120 protects the EUV mask from carbon contamination by reducing or preventing the deposition, formation, or absorption of carbon on the exposed surface of the first capping layer 120. Therefore, by reducing or preventing adverse effects due to carbon formation or carbon contamination on the EUV mask (e.g., the need for increased EUV energy or negative impacts on the CDU), the pattern on the EUV mask 100 can be precisely projected onto the silicon wafer. Due to the amorphous structure of the material of the first cap layer 120, the first cap layer 120 resists weakening caused by etchants, cleaning agents, or processes using such etchants or cleaning agents performed during the fabrication of the EUV mask 100. This resistance to weakening caused by etchants, cleaning agents, or processes using such etchants or cleaning agents increases the first cap layer 120's ability to resist oxidant penetration, which can react with the underlying reflective multilayer stack to form unwanted oxides.

[0074] After removing the patterned photoresist layer 180P, the EUV mask 100 is cleaned to remove any contaminants resulting therefrom. In some embodiments, the EUV mask 100 is cleaned by immersing it in an ammonium hydroxide (NH4OH) solution. In some embodiments, the EUV mask 100 is cleaned by immersing it in a diluted hydrofluoric acid (HF) solution.

[0075] The EUV mask 100 is then irradiated with UV light, for example, at a wavelength of 193 nm, to inspect for any defects in the patterned area 100A. Foreign objects can be detected from diffuse light. If a defect is detected, the EUV mask 100 is further cleaned using a suitable cleaning process.

[0076] Figure 4 This is a cross-sectional view of an EUV mask 400 according to a second embodiment of the present disclosure. The EUV mask 400 is similar in some respects to the one described above. Figure 1 Similar to the EUV mask 100 described in Figure 3. The EUV mask 400 differs from the EUV mask 100 in that the EUV mask 400 includes a multi-layered cap feature comprising two or more cap layers, as described in more detail below. Common structures and features between the EUV mask 400 and the EUV mask 100 are identified by the same reference numerals, and the above description applies to these features. (Refer to...) Figure 4The EUV mask 400 includes a substrate 102, a reflective multilayer stack 110 on the front side of the substrate 102, a patterned first capping layer 120P' on the reflective multilayer stack 110, a patterned second capping layer 130P', and a patterned absorption layer 140P on the patterned second capping layer 130P'. The composition of the patterned first capping layer 120P' of the EUV mask 400 differs from the composition of the patterned second capping layer 130P'. According to... Figure 4 The relevant embodiments of this disclosure. The above description of the composition and material of the first cap layer 12 applies to patterned first cap layer 120P' and patterned second cap layer 130P'. In other words, the materials of the first cap layer 120P' and the second cap layer 130P' can be selected from... Figure 1 The first cap layer 120 of the embodiment shown in Figure 3 is made of the material described above. The EUV mask 400 also includes a conductive layer 104 located on the back side of the substrate 102 opposite to the front side. Although Figure 4 The embodiments are shown and described with reference to a multi-layer cap feature 125 comprising two cap layers, but embodiments of this disclosure also include EUV masks comprising a multi-layer cap feature comprising more than two cap layers.

[0077] Figure 5 This is a flowchart of a method 500 for manufacturing an EUV mask (e.g., EUV mask 400) according to some embodiments. Figures 6A to 6L This is a cross-sectional view of an EUV mask 400 at various stages of the manufacturing process according to some embodiments. Method 500 is discussed in detail below with reference to EUV mask 400. In some embodiments, additional operations are performed before, during, and / or after method 500, or some operations in the described operations are replaced and / or eliminated. In some embodiments, some features of the features described below are replaced or eliminated. Those skilled in the art will understand that although some embodiments have been discussed using operations performed in a particular order, these operations may be performed in a different logical order.

[0078] Reference Figure 5 and Figure 6A According to some embodiments, method 500 includes operation 502, in which a reflective multilayer stack 110 is formed on substrate 102. Figure 6A This is a cross-sectional view of the initial structure of the EUV mask 100 after a reflective multilayer stack 110 has been formed on substrate 102 according to some embodiments. The materials and formation process of the reflective multilayer stack 110 are the same as described above. Figure 3A The materials and forming processes described in the previous section are similar, so they will not be described in detail here.

[0079] Reference Figure 5 and Figure 6BAccording to some embodiments, method 500 proceeds to operation 504, in which a first capping layer 120' is deposited on the reflective multilayer stack 110. Figure 6B According to some embodiments Figure 6A The structure is a cross-sectional view after the first capping layer 120' has been deposited on the reflective multilayer stack 110. The material and formation process of the first capping layer 120' are the same as those described above for... Figure 3B The materials and forming processes of the first cap layer 120 are similar to those described in the previous section, so they will not be described in detail here.

[0080] Reference Figure 5 and Figure 6C According to some embodiments, method 500 proceeds to operation 506, in which a second capping layer 130' is deposited on the first capping layer 120'. Figure 6C According to some embodiments Figure 6B The structure is a cross-sectional view after a second cap layer 130' has been deposited on the cap layer 120'. Figure 6C In one embodiment, the first cap layer 120' and the second cap layer 130' constitute a multi-layer cap feature 125.

[0081] Reference Figure 6C A second capping layer 130' is disposed on the first capping layer 120'. In some embodiments, the second capping layer 130 has different etch characteristics from the absorption layer subsequently formed thereon, and can therefore be used as an etch stop layer to prevent damage to the capping layer 120' during patterning of the absorption layer. Furthermore, the second capping layer 130' can also be subsequently used as a sacrificial layer for focused ion beam repair of defects in the absorption layer. In some embodiments, the second capping layer 130' is selected from the materials described above (which can be used as...). Figure 1 The material of the first cap layer 120 in the embodiment of Figure 3 is one of the following. For example, the second cap layer 130' comprises a material containing an extinction coefficient κ with respect to the EUV wavelength in the range of 0 to 0.1 and a refractive index n in the range of 0.87 to 0.97. By using a material having an extinction coefficient κ and a refractive index n in these ranges, the material of the second cap layer 130' is able to transmit the desired level of incident EUV light without undesirably affecting the phase of the incident EUV light.

[0082] In some embodiments, the second capping layer 130' is deposited by thermal ALD, PE-ALD, CVD, PECVD, PVD electron beam evaporation, thermal evaporation, ion beam induced deposition, sputtering, electrodeposition, or electrodeposition-free deposition. In some embodiments, the thickness of the second capping layer ranges from about 0.5 nm to 5 nm. The thickness of the second capping layer 130', ranging from about 0.5 nm to 5 nm, is sufficient to protect the underlying first capping layer 120' and / or multilayer stack 110 from oxidation or chemical etchants during mask forming processes or semiconductor processes using masks. When the thickness of the second capping layer 130' is 0.5 nm to 5 nm, it is not so thick that it causes an undesirable reduction in EUV transmission. Embodiments according to this disclosure are not limited to EUV masks including a second capping layer 130' having a thickness of about 0.5 nm to about 5 nm. Embodiments according to this disclosure also include: an EUV mask including a second capping layer 130' having a thickness of less than 0.5 nm, and an EUV mask including a second capping layer 130' having a thickness of more than about 5 nm.

[0083] In some embodiments, the material of the second capping layer 130' comprises elements having a different solid-state carbon solubility than the elements in the material of the first capping layer 120'. For example, in some embodiments, the solid-state carbon solubility of elements in the material of the second capping layer 130' is greater than or less than the solid-state carbon solubility of the material of the first capping layer 120'. According to Figure 4 In some embodiments, the material of the second cap layer 130' comprises elements with EUV extinction coefficients that are less than those of elements in the material of another layer (e.g., the first cap layer 120' of the multilayer cap feature 125'). Figure 4 In other embodiments, the elemental composition of the material of the second capping layer 130' has an EUV extinction coefficient for EUV radiation at a wavelength of 13.5 nm that is greater than the elemental composition of the material of the first capping layer 120' of the multilayer capping feature 125' for EUV radiation at a wavelength of 13.5 nm. Furthermore, the material of the second capping layer 130' used in the multilayer capping feature according to this embodiment exhibits good adhesion to both the first capping layer 120' and the material deposited on the second capping layer 130.

[0084] The forming process of the second cap layer 130' is the same as that of the above-mentioned... Figure 3C The formation process of the first capping layer 120 is similar to that described in the text, so it will not be described in detail here.

[0085] Reference Figure 5 and Figure 6D According to various embodiments, method 500 proceeds to operation 508, in which an absorber layer 140 is deposited on the second cap layer 130'. Figure 6DAccording to some embodiments Figure 6C The structure is a cross-sectional view after the absorption layer 140 has been deposited on the second cap layer 130'. The material and formation process of the absorption layer 140 are the same as those described above. Figure 3C The materials and forming processes described in the previous section are similar, so they will not be described in detail here.

[0086] Reference Figure 5 and Figure 6E According to some embodiments, method 500 proceeds to operation 509, in which a resist stack including a hard mask layer 160 and a photoresist layer 170 is deposited on absorber layer 140. Figure 6E According to some embodiments Figure 6D The structure is a cross-sectional view after the hard mask layer 160 and the photoresist layer 170 are sequentially deposited on the absorber layer 140. The corresponding materials and formation processes of the hard mask layer 160 and the photoresist layer 170 are the same as those in the... Figure 3D The materials and forming processes described in the previous section are similar, so they will not be described in detail here.

[0087] Reference Figure 5 and Figure 6F According to some embodiments, method 500 proceeds to operation 510, in which the photoresist layer 170 is photolithographically patterned to form a patterned photoresist layer 170P. Figure 6F According to some embodiments Figure 6E The structure is a cross-sectional view after photolithographic patterning of the photoresist layer 170 to form the patterned photoresist layer 170P. The etching process of the photoresist layer 170 is similar to that in... Figure 3E The etching process described in the previous section is similar, so it will not be described in detail here.

[0088] Reference Figure 5 and Figure 6G According to some embodiments, method 500 proceeds to operation 512, in which a patterned photoresist layer 170P is used as an etch mask to etch a hard mask layer 160 to form a patterned hard mask layer 160P. Figure 6G According to some embodiments Figure 6F The structure is a cross-sectional view after etching the hard mask layer 160 to form a patterned hard mask layer 160P. The etching process of the hard mask layer 160 is similar to that in... Figure 3F The etching process described in the previous section is similar, so it will not be described in detail here.

[0089] Reference Figure 5 and Figure 6HAccording to some embodiments, method 500 proceeds to operation 514, in which a patterned hard mask layer 160P is used as an etch mask to etch the absorber layer 140 to form the patterned absorber layer 140P. Figure 6H According to some embodiments Figure 6G The structure is a cross-sectional view after etching the absorption layer 140 to form a patterned absorption layer 140P. The etching process of the absorption layer 140 is similar to that in... Figure 3G The etching process described herein is similar and will not be described in detail here. The patterned absorber layer 140P includes a plurality of openings 142 that expose the underlying second cap layer 130'. After etching the absorber layer 140, the patterned hard mask layer 160P is removed from the surface of the patterned absorber layer 140P, for example, using oxygen plasma or wet etching. The resulting structure is... Figure 6I As shown in the image.

[0090] According to Figure 4 In some embodiments up to Figure 6, the steps of etching the absorber layer 140 to form the patterned absorber layer 140P and / or removing the photoresist layer 170 and / or the patterned hard mask layer 160P can remove a portion of the upper surface of the second cap layer 130'. Such embodiments in Figure 4 As shown by reference numeral 131, at this location, a portion of the patterned second capping layer 130P' is removed by etching the absorber layer 140 or by removing the photoresist layer 170 and / or the patterned hard mask layer 160P. According to an embodiment where a portion of the upper surface of the patterned second capping layer 130P' has been removed, a certain amount of the upper surface of the patterned second capping layer 130P' remains, for example, at least a few nanometers of the patterned second capping layer 130P' remains. Examples of these few nanometers include 1 nm to 2 nm. According to... Figure 4 In other embodiments up to Figure 6, the steps of etching the absorber layer 140 to form the patterned absorber layer 140P and / or removing the photoresist layer 170 and / or the patterned hard mask layer 160P do not remove portions of the second capping layer 130'. Such embodiments in... Figure 4 It is shown in the figure by reference numeral 133. Figure 6I An embodiment is shown in which the second capping layer 130' is not removed by the absorption layer, photoresist, or hard mask removal steps.

[0091] Reference Figure 5 and Figure 6J According to some embodiments, method 500 proceeds to operation 516, in which a patterned photoresist layer 180P including a pattern of openings 182 is formed on the patterned absorber layer 140P and the second capping layer 130'. Figure 6J According to some embodiments Figure 6I The structure is a cross-sectional view after a patterned photoresist layer 180P, including an opening 182, is formed on the patterned absorption layer 140P and the second capping layer 130'. The material and manufacturing process of the patterned photoresist layer 180P are similar to those in... Figure 3H The materials and manufacturing processes described in the previous section are similar, so they will not be described in detail here.

[0092] Reference Figure 5 and Figure 6K According to some embodiments, method 500 proceeds to operation 518, in which a patterned photoresist layer 180P is used as an etching mask to etch a patterned absorber layer 140P, a second capping layer 130', a first capping layer 120', and a reflective multilayer stack 110 to form a trench 154 in the peripheral region 100B of the substrate 102. Figure 6K According to some embodiments Figure 6J The structure is a cross-sectional view after etching a patterned absorption layer 140P, a second capping layer 130', a first capping layer 120', and a reflective multilayer stack 110 to form a trench 154 in the peripheral region 100B of the substrate 102.

[0093] Reference Figure 6K The trench 154 extends through the patterned absorption layer 140P, the second capping layer 130', the first capping layer 120', and the reflective multilayer stack 110 to expose the surface of the substrate 102. The trench 154 surrounds the patterned region 100A of the EUV mask 400, separating the patterned region 100A from the peripheral region 100B.

[0094] In some embodiments, a single anisotropic etching process is used to etch the patterned absorber layer 140P, the second cap layer 130', the first cap layer 120', and the reflective multilayer stack 110. The anisotropic etching can be dry etching (e.g., RIE), wet etching, or a combination thereof, which removes corresponding material from the patterned absorber layer 140P, the second cap layer 130', the first cap layer 120', and the reflective multilayer stack 110, optionally removing material providing the substrate 102. In some embodiments, multiple different anisotropic etching processes are used to etch the patterned absorber layer 140P, the second cap layer 130', the first cap layer 120', and the reflective multilayer stack 110. Each anisotropic etching can be dry etching (e.g., RIE), wet etching, or a combination thereof.

[0095] Reference Figure 5 and Figure 6L According to some embodiments, method 500 proceeds to operation 520, in which the patterned photoresist layer 180P is removed. Figure 6L According to some embodiments Figure 6KThe cross-sectional view of the structure after the patterned photoresist layer 180P has been removed.

[0096] Reference Figure 6L For example, the patterned photoresist layer 180P is removed from the patterned region 100A and peripheral region 100B of the substrate 102 by wet stripping or plasma ashing. Removing the patterned photoresist layer 180P from the openings 142 in the patterned absorber layer 140P re-exposes the surface of the second capping layer 130' located in the patterned region 100A. The openings 142 in the patterned absorber layer 140P define a pattern of openings in the EUV mask 400 corresponding to the circuit patterns to be formed on the semiconductor wafer.

[0097] This forms an EUV mask 400. The EUV mask 400 includes a substrate 102, a reflective multilayer stack 110 on the front side of the substrate 102, a patterned first capping layer 120P' on the reflective multilayer stack 110, a patterned second capping layer 130P' on the patterned first capping layer 120P', and a patterned absorption layer 140P on the patterned second capping layer 130P'. The EUV mask 400 also includes a conductive layer 104 on the back side of the substrate 102, opposite to the front side. Figure 4 In the embodiment shown in Figure 6, the second capping layer 130' resists carbon contamination by reducing or preventing the deposition, formation, or absorption of carbon on its exposed surface, thereby protecting the underlying first capping layer 120P' and the reflective multilayer stack 110 from carbon contamination. Therefore, by reducing or preventing adverse effects due to carbon formation or carbon contamination on the EUV mask (e.g., the need for increased EUV energy or negative impacts on the CDU), the pattern on the EUV mask 100 can be precisely projected onto the silicon wafer. Due to the amorphous structure of the materials of the first capping layer 120' and / or the second capping layer 130', the first capping layer 120' and / or the second capping layer 130' resist weakening caused by etchants, cleaning agents, or processes performed during the manufacture of the EUV mask 400 using such etchants or cleaning agents. This resistance to weakening caused by etchants, cleaners, or processes using such etchants or cleaners increases the ability of the first capping layer 120′' and the second capping layer 130′ to resist oxidant penetration, which may react with the underlying reflective multilayer stack to form unwanted oxides.

[0098] After removing the patterned photoresist layer 180P, the EUV mask 400 is cleaned to remove any contaminants resulting from it. In some embodiments, the EUV mask 400 is cleaned by immersing it in an ammonium hydroxide (NH4OH) solution. In some embodiments, the EUV mask 400 is cleaned by immersing it in a diluted hydrofluoric acid (HF) solution.

[0099] The EUV mask 400 is then irradiated with UV light, for example, at a wavelength of 193 nm, to inspect for any defects in the patterned area 100A. Foreign objects can be detected from diffuse light. If a defect is detected, the EUV mask 400 is further cleaned using a suitable cleaning process.

[0100] Figure 7 A method 1200 using an EUV mask according to an embodiment of the present disclosure is illustrated. Method 1200 includes a step 1202 of exposing an EUV mask to incident radiation (e.g., EUV radiation). Examples of EUV masks used in step 1202 include the EUV mask 100 or EUV mask 400 described above. In step 1204, a portion of the incident radiation is absorbed in a patterned absorbing layer of the EUV mask. In step 1206, a portion of the incident radiation is transmitted through a capping layer having an amorphous structure. An example of a capping layer having an amorphous structure is shown below. Figure 1 To the first cap layer 120 depicted in Figure 3. In an optional step 1208 relating to a method employing a multilayer cap feature according to an embodiment of the present disclosure, a portion of the incident radiation is transmitted through a second cap layer having a second solid carbon solubility or a second EUV extinction characteristic, which differs from the first carbon solubility or the first EUV extinction characteristic of the first cap layer. Examples of cap layers having a second solid carbon solubility or a second EUV extinction characteristic include the aforementioned first cap layer 120' or second cap layer 130'. In step 1209, a portion of the incident radiation is reflected from the reflective multilayer stack. In step 1210, the portion of the incident radiation reflected by the reflective multilayer stack is directed to the material to be patterned. In embodiments where optional step 1208 is omitted, the reflected incident radiation is back-transmitted through the first cap layer having an amorphous structure. In embodiments including optional step 1208, the reflected incident radiation is back-transmitted along its path through the first and second cap layers to reach the material to be patterned. After the material to be patterned has been exposed to radiation reflected from the EUV mask, in step 1212, the portions of the material that were exposed to or not exposed to radiation reflected from the EUV mask are removed.

[0101] Figure 8A method 800 using an EUV mask according to an embodiment of the present disclosure is illustrated. Method 800 includes a step 802 of exposing an EUV mask to incident radiation (e.g., EUV radiation). An example of an EUV mask used in step 802 includes the EUV mask 400 described above. In step 804, a portion of the incident radiation is absorbed in a patterned absorbing layer of the EUV mask. In step 806, a first amount of the incident radiation is absorbed in a first capping layer, the first capping layer comprising elements having a first solid carbon solubility and a first EUV extinction coefficient. An example of a capping layer having the first carbon solubility and the first EUV extinction characteristic includes the second capping layer 130' described above. In step 808, a second amount of the incident radiation is absorbed by a second capping layer, the second capping layer comprising elements having a second solid carbon solubility and / or a second EUV extinction coefficient, the second solid carbon solubility and / or the second EUV extinction coefficient being different from the first solid carbon solubility and / or the first EUV extinction coefficient. In some embodiments, the amount of incident radiation absorbed by the first capping layer differs from the amount of incident radiation absorbed by the second capping layer. An example of the second capping layer includes the first capping layer 120' described above. In step 809, a portion of the incident radiation is reflected from the reflective multilayer stack. In step 810, the portion of the incident radiation reflected by the reflective multilayer stack is directed to the material to be patterned. The reflected incident radiation is transmitted back along its path through the first and second capping layers to reach the material to be patterned. After the material to be patterned has been exposed to radiation reflected from the EUV mask, in step 812, the portion of the material exposed to or not exposed to radiation reflected from the EUV mask is removed.

[0102] Figure 9 The analysis results of the thickness of carbon contamination on a cap feature containing an Rh-containing alloy (e.g., RuRh) according to an embodiment of the present disclosure are shown. Figure 9 As shown, the thickness of the carbon contamination is approximately 6.5 nm. In contrast, carbon contamination not formed according to this disclosure and exposed to [other materials] was observed. Figure 9 The carbon contamination thickness on the cap feature under the same photolithographic conditions is greater, for example, about 11.7 nm. The cap layer according to this disclosure achieves a reduction of approximately 40% in carbon contamination thickness.

[0103] One aspect of this description relates to an EUV mask. The EUV mask includes a substrate, a reflective multilayer stack on the substrate, and a cap feature on the reflective multilayer stack. The cap feature includes a first cap layer comprising a material having an amorphous structure. In some embodiments, the amorphous structure comprises a nanocrystalline structure having a grain size of less than 2 nm. The EUV mask also includes a patterned absorption layer on the multilayer cap feature. In some embodiments, the first cap layer comprises a material containing an element having a solid carbon solubility of less than 3 atomic percent at the eutectic point of a system comprising the element and carbon. This EUV mask exhibits a reduced tendency for carbon build-up or contamination, which negatively impacts the mask's ability to produce patterns that meet critical size criteria. Furthermore, this EUV cap feature exhibits resistance to weakening caused by etchants or cleaning agents exposed to the cap layer during EUV mask fabrication.

[0104] Another aspect of this description relates to a method using an EUV mask. The method includes exposing an EUV mask to incident radiation. The EUV mask includes a substrate, a reflective multilayer stack on the substrate, and a multilayer cap feature on the reflective multilayer stack. The multilayer cap feature includes a first cap layer and a second cap layer, the first cap layer comprising a first alloy containing Rh, Ir, Pt, Au, or Zr, and the second cap layer comprising a second alloy containing Rh, Ir, Pt, Au, or Zr, the second alloy being different from the first alloy. The EUV mask includes a patterned absorbing layer on the multilayer cap feature. The method includes absorbing a portion of the incident radiation in the patterned absorbing layer. Transmitting a portion of the incident radiation through the first and second cap layers. Reflecting a portion of the incident radiation from the reflective multilayer stack and directing it to the material to be patterned. In some embodiments, the first and second alloys are selected from RuZr, IrZr, RhZr, HfZr, and NbZr, wherein the Zr content of the first and second alloys is at least 5 atomic%.

[0105] Another aspect of this description relates to another method using an EUV mask. This method includes exposing an EUV mask to incident radiation. The EUV mask includes a substrate, a reflective multilayer stack on the substrate, a cap feature, and a patterned absorbing layer on the cap feature. The cap feature includes a material comprising an element having a solid carbon solubility of less than 3 atomic percent at the eutectic point of the element and carbon. The method also includes causing a portion of the incident radiation to be absorbed in the patterned absorbing layer. In this method, a portion of the incident radiation is absorbed in the cap layer. The method continues until a portion of the incident radiation is reflected from the reflective multilayer stack and directed to the material to be patterned.

[0106] The foregoing outlines features of several embodiments to enable those skilled in the art to better understand various aspects of this disclosure. Those skilled in the art should appreciate that they can readily use this disclosure as a basis for designing or modifying other processes and structures to achieve the same purposes and / or advantages as the embodiments introduced herein. Those skilled in the art should also recognize that these equivalent constructions do not depart from the spirit and scope of this disclosure, and that various changes, substitutions, and modifications can be made without departing from the spirit and scope of this disclosure.

[0107] Example 1 is an extreme ultraviolet (EUV) mask comprising: a substrate; a reflective multilayer stack on the substrate; a cap feature on the reflective multilayer stack, the cap feature including a first cap layer comprising a material having an amorphous structure; and a patterned absorption layer on the cap feature.

[0108] Example 2 is an EUV mask according to Example 1, wherein the amorphous structure comprises a nanocrystalline structure having a grain size of less than 5 nanometers.

[0109] Example 3 is an EUV mask according to Example 1, wherein the amorphous structure comprises a nanocrystalline structure having a grain size of less than 2 nanometers.

[0110] Example 4 is an EUV mask according to Example 1, wherein the cap feature further includes a second cap layer comprising a material having an amorphous structure, the material of the second cap layer being different from the material of the first cap layer.

[0111] Example 5 is an EUV mask according to Example 4, wherein the elements comprising the material of the first cap layer have EUV extinction coefficients for EUV radiation at a wavelength of 13.5 nm that are different from the elements comprising the material of the second cap layer that have EUV extinction coefficients for EUV radiation at a wavelength of 13.5 nm.

[0112] Example 6 is an EUV mask according to Example 5, wherein the elemental extinction coefficient of the material of the first cap layer for EUV radiation at a wavelength of 13.5 nm is between 0 and 0.1.

[0113] Example 7 is an EUV mask according to Example 5, wherein the elemental extinction coefficient of the material of the second cap layer for EUV radiation at a wavelength of 13.5 nm is between 0 and 0.1.

[0114] Example 8 is an EUV mask according to Example 4, wherein the material of the first cap layer comprises an element having a solid carbon solubility of less than 3 atomic percent at the eutectic point of the system containing the element and carbon.

[0115] Example 9 is an EUV mask according to Example 4, wherein the material of the second cap layer comprises an element having a solid carbon solubility of less than 3 atomic percent at the eutectic point of the system containing the element and carbon.

[0116] Example 10 is an EUV mask according to Example 1, wherein the material of the first cap layer is selected from alloys containing one or more elements selected from Rh, Ir, Pt, Au and Zr.

[0117] Example 11 is an EUV mask according to Example 4, wherein the material of the second cap layer is selected from alloys containing one or more elements selected from Rh, Ir, Pt, Au and Zr, or the alloy contains an alloy of Rh, Ir, Pt, Au and Zr.

[0118] Example 12 is an EUV mask according to Example 10, wherein the alloy of the first cap layer further includes Hf, Nb, or N.

[0119] Example 13 is an EUV mask according to Example 11, wherein the alloy of the second cap layer further includes Hf, Nb, or N.

[0120] Example 14 is a method of using an EUV mask, the method comprising: exposing an EUV mask to incident radiation, the EUV mask comprising: a substrate; a reflective multilayer stack on the substrate; a multilayer cap feature on the reflective multilayer stack, the multilayer cap feature comprising a first cap layer and a second cap layer, the first cap layer comprising a first alloy containing Rh, Ir, Pt, Au, or Zr, the second cap layer comprising a second alloy containing Rh, Ir, Pt, Au, or Zr, the second alloy being different from the first alloy; and a patterned absorbing layer on the multilayer cap feature; absorbing a portion of the incident radiation in the patterned absorbing layer; transmitting a portion of the incident radiation through the first cap layer and the second cap layer; reflecting a portion of the incident radiation from the reflective multilayer stack; and directing the portion of the incident radiation reflected by the reflective multilayer stack to a material to be patterned.

[0121] Example 15 is the method according to Example 14, wherein the first alloy and the second alloy are selected from RuZr, IrZr, RhZr, HfZr and NbZr, wherein the Zr content of the first alloy and the second alloy is at least 5 atoms.

[0122] Example 16 is the method according to Example 14, wherein the first alloy and the second alloy are selected from RuRh, RuIr, RuPt, PtIr, RuIrPt, NbIr, NbPt, NbRh, RhN, IrN, RuRhN, RuIrN, RuPtN, PtIrN, RuIrPtN, NbIrN, NbPtN and NbRhN.

[0123] Example 17 is a patterning method comprising: exposing an EUV mask to incident radiation, the EUV mask comprising: a substrate; a reflective multilayer stack located on the substrate; a cap feature located on the reflective multilayer stack, the cap feature comprising a material containing an element having a solid carbon solubility of less than 3 atomic percent at the eutectic point of the element and carbon system; and a patterned absorbing layer located on the cap feature; absorbing a portion of the incident radiation in the patterned absorbing layer; absorbing a certain amount of the incident radiation in the cap feature; reflecting a portion of the incident radiation from the reflective multilayer stack; and directing the portion of the incident radiation reflected by the reflective multilayer stack to the material to be patterned.

[0124] Example 18 is the method according to Example 17, wherein the material of the cap feature includes RuZr, IrZr, RhZr, HfZr or NbZr, wherein the Zr content is at least 5 atoms.

[0125] Example 19 is the method according to Example 17, wherein the material of the cap feature is an alloy selected from RuRh, RuIr, RuPt, PtIr, RuIrPt, NbIr, NbPt, NbRh, RhN, IrN, RuRhN, RuIrN, RuPtN, PtIrN, RuIrPtN, NbIrN, NbPtN, and NbRhN.

[0126] Example 20 is the method according to Example 17, wherein the solubility of solid carbon at the eutectic point is less than 2 atoms.

Claims

1. An extreme ultraviolet (EUV) mask, comprising: Substrate; A reflective multilayer stack located on the substrate; A cap feature located on the reflective multilayer stack, the cap feature comprising a first cap layer comprising a material having an amorphous structure, wherein the material of the first cap layer is an alloy selected from IrZr, RhZr, HfZr, NbZr, and ZnZr; and A patterned absorption layer located on the cap feature.

2. The EUV mask according to claim 1, wherein, The amorphous structure includes nanocrystalline structures with a grain size of less than 5 nanometers.

3. The EUV mask according to claim 1, wherein, The amorphous structure includes nanocrystalline structures with a grain size of less than 2 nanometers.

4. The EUV mask of claim 1, wherein, The cap feature also includes a second cap layer, the second cap layer comprising a material having an amorphous structure, the material of the second cap layer being different from the material of the first cap layer.

5. The EUV mask according to claim 4, wherein, The elements in the material of the first cap layer have different EUV extinction coefficients for EUV radiation with a wavelength of 13.5 nm compared to the elements in the material of the second cap layer with a wavelength of 13.5 nm.

6. The EUV mask according to claim 5, wherein, The elemental extinction coefficient of the material of the first cap layer for EUV radiation with a wavelength of 13.5 nm is between 0 and 0.

1.

7. The EUV mask according to claim 5, wherein, The elemental extinction coefficient of the material of the second cap layer for EUV radiation at a wavelength of 13.5 nm is between 0 and 0.

1.

8. The EUV mask according to claim 4, wherein, The material of the first cap layer includes the following elements: The element has a solid carbon solubility of less than 3 atomic percent at the eutectic point of the system containing the element and carbon.

9. The EUV mask of claim 4, wherein, The material of the second cap layer includes the following elements: The element has a solid carbon solubility of less than 3 atomic percent at the eutectic point of the system containing the element and carbon.

10. The EUV mask of claim 4, wherein, The material of the second cap layer is selected from alloys containing one or more elements selected from Rh, Ir, Pt, Au and Zr.

11. The EUV mask according to claim 10, wherein, The alloy of the second cap layer also includes Hf, Nb, or N.

12. A method using an EUV mask, the method comprising: Expose an EUV mask to incident radiation, the EUV mask comprising: Substrate; A reflective multilayer stack located on the substrate; A multi-layer cap feature located on the reflective multilayer stack, the multi-layer cap feature including a first cap layer and a second cap layer, the first cap layer including a first alloy, the second cap layer including a second alloy, the second alloy being different from the first alloy, wherein the first alloy and the second alloy are selected from IrZr, RhZr, HfZr, NbZr and ZnZr; and A patterned absorption layer located on the multi-layered cap feature; A portion of the incident radiation is absorbed in the patterned absorption layer; A portion of the incident radiation is transmitted through the first cap layer and the second cap layer; A portion of the incident radiation is reflected from the reflective multilayer stack; and The portion of the incident radiation reflected by the multilayer stack of reflective materials is guided to the material to be patterned.

13. The method of claim 12, wherein, The Zr content of the first alloy and the second alloy is at least 5 atoms.

14. A patterning method, comprising: Expose an EUV mask to incident radiation, the EUV mask comprising: Substrate; A reflective multilayer stack located on the substrate; A cap feature located on the reflective multilayer stack, the cap feature comprising a material containing elements having a solid carbon solubility of less than 3 atomic percent at the eutectic point of the element and carbon system, wherein the material of the cap feature is an alloy selected from IrZr, RhZr, HfZr, NbZr, and ZnZr; and A patterned absorption layer located on the cap feature; A portion of the incident radiation is absorbed in the patterned absorption layer; A certain amount of the incident radiation is absorbed in the cap feature; A portion of the incident radiation is reflected from the reflective multilayer stack; and The portion of the incident radiation reflected by the multilayer stack of reflective materials is guided to the material to be patterned.

15. The method of claim 14, wherein, The Zr content is at least 5 atoms.

16. The method of claim 14, wherein, The solubility of solid carbon at the eutectic point is less than 2 atoms.

Citation Information

Patent Citations

  • Lithographic mask with amorphous cap layer

    CN113253562A

  • EUV photomask and manufacturing method thereof

    CN113253563A

  • Reflective mask blank for EUV lithography and substrate with functional film for the same

    US20080318140A1

  • Reflective Photomask Blanks and Reflective Photomasks

    US20150010854A1

  • Mask and method for forming the same

    US20210018828A1