A method for manufacturing a sodium ion solid-state battery using a flexible current collector
Through the preparation method of flexible current collector and the application of MXene materials, the poor electrochemical performance and interface stability of sodium ion batteries are solved, and the cycle stability and safety performance of the battery are significantly improved.
Patent Information
- Application Number
- CN202211681922.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-12-26
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2042-12-26
AI Technical Summary
Due to poor electrochemical performance of sodium ion batteries, poor interface stability between solid electrolyte and electrode plate, resulting in poor safety performance and battery performance.
Using flexible current collector preparation method, MXene/reduced graphene oxide film is prepared by combining graphene oxide with MXene material, and polymer solid electrolyte and MXene material are used in sodium ion solid-state batteries to improve the adhesion between the negative and positive electrodes. and interface stability.
It effectively improves the electrochemical performance and cycle stability of sodium ion batteries, prevents active materials from falling off, and improves the safety performance and electrical performance of the batteries.
Abstract
Description
Technical Field
[0001] The invention relates to the field of sodium ion batteries, and specifically discloses a method for manufacturing a sodium ion solid-state battery using a flexible current collector. Background Art
[0002] Currently, the cost of lithium-ion batteries is greatly affected by the rising prices of raw materials. However, sodium-ion batteries are considered to be able to replace lithium-ion batteries in some application scenarios due to their lower raw material prices and better safety performance. Therefore, sodium-ion batteries are gradually attracting the attention of various scientific research institutions, battery companies and universities.
[0003] Since organic solvents are used in liquid electrolytes, this has a certain impact on the safety of the battery and may cause the same safety hazards in sodium-ion batteries as lithium-ion batteries. Solid electrolytes can greatly reduce the amount of organic solvents used and can effectively improve the safety performance of the battery. Therefore, the development of sodium-ion batteries using solid electrolytes can reduce battery costs while improving battery safety. However, sodium-ion materials themselves have problems such as low compaction density and poor adhesion, and the interface stability between the solid electrolyte and the electrode is poor, all of which will lead to poor electrochemical performance of the battery. Summary of the invention
[0004] The purpose of the present invention is to overcome the defects of the prior art and provide a method for manufacturing a sodium ion solid-state battery using a flexible current collector.
[0005] The technical solution to achieve the purpose of the present invention is to provide a method for preparing a flexible current collector, and the specific steps are as follows:
[0006] (1) uniformly dispersing graphene oxide in water, mixing with a MXene aqueous dispersion, and ultrasonically dispersing to obtain a MXene / graphene oxide composite suspension;
[0007] (2) The MXene / graphene oxide composite suspension is filtered and dried in sequence to obtain MXene /
[0008] Graphene oxide film;
[0009] (3) The MXene / graphene oxide film is subjected to high temperature treatment to obtain a MXene / reduced graphene oxide film.
[0010] Furthermore, the thickness of the MXene / reduced graphene oxide film is 7 to 16 μm, and the mass ratio of MXene:reduced graphene oxide is (70% to 90%):(10% to 30%).
[0011] A sodium ion solid-state battery consists of a positive electrode, a negative electrode, and a solid electrolyte. The negative electrode uses a flexible current collector, and the solid electrolyte is a polymer solid electrolyte. The specific production steps are as follows:
[0012] (1) taking a polymer material, a sodium salt, and a solvent, and stirring them evenly by magnetic force to prepare a solid electrolyte solution;
[0013] (2) evenly coating the solid electrolyte solution on the surface of the positive electrode sheet and drying it to obtain a positive electrode sheet / solid electrolyte layer;
[0014] (3) Place the positive electrode sheet / solid electrolyte layer into a battery shell with the solid electrolyte layer facing upward, drop a plasticizer on top of the solid electrolyte layer, and then place the negative electrode sheet on top of the solid electrolyte layer. Install a gasket, a spring, and a battery shell in sequence to produce a sodium ion solid-state battery.
[0015] Furthermore, the specific method for preparing the negative electrode sheet is as follows:
[0016] (1) Dispersing the binder material 1 in pure water and stirring evenly to obtain a high solid content binder solution;
[0017] (2) Add MXene aqueous dispersion to the high solid content binder glue, stir evenly, add conductive agent, continue stirring until evenly, and obtain low solid content conductive glue;
[0018] (3) Add the negative electrode active material to the low solid content conductive glue, stir evenly, add the binder material 2, continue stirring until evenly mixed, and obtain the negative electrode slurry;
[0019] (4) The prepared negative electrode slurry is coated on the surface of the MXene / reduced graphene oxide film, and then dried and punched to obtain a negative electrode sheet.
[0020] Furthermore, the specific method for preparing the positive electrode sheet is as follows:
[0021] (1) adding conductive carbon black to a MXene aqueous dispersion, dispersing the conductive carbon black / MXene dispersion by ultrasonication, filtering and drying the obtained conductive carbon black / MXene dispersion to obtain a conductive carbon black / MXene composite film, grinding and sieving the composite film to obtain a conductive carbon black / MXene composite material;
[0022] (2) dispersing the binder material in a solvent and stirring it evenly to obtain a positive electrode glue solution;
[0023] (3) Adding the conductive carbon black / MXene composite material to the glue solution, stirring evenly, adding the positive electrode active material, stirring evenly, and preparing the positive electrode slurry;
[0024] (4) The prepared positive electrode slurry is coated on aluminum foil, and then dried and punched to obtain a positive electrode sheet.
[0025] Furthermore, the positive electrode active material is a layered oxide, the layered oxide structural formula is NaxMeO2, wherein Me is selected from two or more of magnesium (Mg), manganese (Mn), iron (Fe), cobalt (Co), nickel (Ni), vanadium (V), copper (Cu), chromium (Cr), iridium (Ir), and ruthenium (Ru); the solvent is NMP; and the binder is PVDF.
[0026] Furthermore, the mass ratio of the conductive carbon black / MXene composite material is (80% to 90%): (10% to 20%); the mass ratio of the positive electrode active material: the conductive carbon black / MXene composite material: the binder is (80 to 95): (2.5 to 10): (2.5 to 10), and the solid content of the positive electrode slurry is 40% to 60%. .
[0027] Furthermore, the negative electrode active material is hard carbon, and the negative electrode formula active material: conductive agent: binder 1: binder 2: MXene is in a mass ratio of (80-90):(3-5):(1-5):(2-5):(2-14), and the solid content of the negative electrode slurry is 40%-60%.
[0028] Furthermore, the conductive agent is one or more of conductive carbon black, graphene, acetylene black, carbon nanotubes, and Ketjen black; the binder 1 is sodium carboxymethyl cellulose (CMC); and the binder 2 is one or two of styrene-butadiene rubber (SBR) and polyacrylonitrile emulsion.
[0029] Furthermore, the polymer material in the solid electrolyte is one or more of PEO, PVDF, PVC, and PMMA; the sodium salt is one or two of sodium hexafluorophosphate and sodium perchlorate; the solvent is N-methylpyrrolidone (NMP) or acetonitrile (ACN); and the plasticizer is two or more of ethylene carbonate (EC), diethyl carbonate (DEC), ethyl methyl carbonate (EMC), propylene carbonate (PC), and fluoroethylene carbonate (FEC).
[0030] After adopting the above technical solution, the present invention has the following positive effects:
[0031] (1) The present invention adopts a flexible current collector to replace the negative electrode aluminum foil current collector, which can effectively prevent the shrinkage of the slurry due to surface tension and improve the weak binding force between the active material and the aluminum foil current collector due to the poor adhesion of the hard carbon material itself; and the addition of MXene material to the electrode slurry can effectively increase the binding force with the MXene / reduced graphene oxide film, can accommodate the volume change of the active material particles during the cycle, and prevent the active material from falling off, thereby effectively improving the electrical performance of the sodium ion battery.
[0032] (2) The MXene material of the present invention has rich functional groups and specific surface area, and has a special layered structure, which can effectively withstand the volume change of the active material during the charge and discharge process, effectively prevent the material from falling off, and improve the battery performance.
[0033] (3) In the present invention, since the density of MXene material is relatively small and aqueous solution cannot be used in the positive electrode, in order to prevent uneven dispersion of MXene material in the positive electrode slurry, a pre-mixing process of MXene material and conductive agent is adopted to improve its dispersion effect.
[0034] (4) The negative electrode of the present invention adopts a flexible current collector, which can effectively improve the poor adhesion between the hard carbon material and the conventional current collector, and can effectively improve the battery failure caused by volume change during the charge and discharge process of the battery. At the same time, MXene materials are added to both the positive and negative electrodes. MXene has rich functional groups and high specific surface area, and through a strong interface effect, it effectively improves the interface stability between the solid electrolyte and the electrode. DETAILED DESCRIPTION
[0035] Example 1
[0036] 1. Preparation method of flexible current collector:
[0037] (1) 10% graphene oxide was uniformly dispersed in water, mixed with 90% MXene aqueous dispersion, and ultrasonically dispersed to obtain a MXene / graphene oxide composite suspension (90%:10%);
[0038] (2) filtering and drying the MXene / graphene oxide composite suspension (90%:10%) in sequence to obtain a MXene / graphene oxide film (90%:10%);
[0039] (3) The MXene / graphene oxide film (90%:10%) was subjected to high temperature treatment to obtain a MXene / reduced graphene oxide film (90%:10%) with a thickness of 7 μm.
[0040] 2. Negative electrode preparation method:
[0041] (1) Disperse 1.0% CMC powder in pure water and stir evenly to obtain CMC glue with a solid content of 2.0%;
[0042] (2) Add 2.0% MXene aqueous dispersion to the CMC glue with a solid content of 2.0%, stir evenly, then add 3.0% conductive carbon black, continue stirring until evenly mixed, and obtain a low solid content conductive glue;
[0043] (3) Add 92% hard carbon to the low-solid content conductive glue, stir evenly, then add 2.0% SBR, continue stirring until evenly mixed, and obtain the negative electrode slurry;
[0044] (4) The prepared negative electrode slurry is coated on the surface of the MXene / reduced graphene oxide film, and then dried and punched to obtain a negative electrode sheet.
[0045] 3. Positive electrode preparation method:
[0046] (1) adding 80% conductive carbon black to 20% MXene aqueous dispersion, dispersing by ultrasonic, filtering and drying the obtained conductive carbon black / MXene (80%:20%) dispersion to obtain a conductive carbon black / MXene (80%:20%) composite film, grinding and sieving the composite film to obtain a conductive carbon black / MXene (80%:20%) composite material;
[0047] (2) Dispersing 2.5% PVDF in a solvent and stirring evenly to obtain a positive electrode gel;
[0048] (3) Add 2.5% conductive carbon black / MXene composite material to the glue solution, stir evenly, and add 95% NaNi 0.35 Co 0.33 Mn 0.32 O2, and stirred evenly to obtain a positive electrode slurry;
[0049] (4) The prepared positive electrode slurry is coated on aluminum foil, and then dried and punched to obtain a positive electrode sheet.
[0050] 4. Sodium ion solid-state battery manufacturing method:
[0051] (1) PEO, 1M NaPF6, and ACN were mixed by magnetic force to obtain a solid electrolyte solution;
[0052] (2) evenly coating the solid electrolyte solution on the surface of the positive electrode sheet and drying it to obtain a positive electrode sheet / solid electrolyte layer;
[0053] (3) Place the positive electrode sheet / solid electrolyte layer into the battery shell with the solid electrolyte layer facing upward, drop the plasticizer EC:PC=(1:1) on top of the solid electrolyte layer, then place the negative electrode sheet on top of the solid electrolyte layer, and install the gasket, spring, and battery shell in sequence to produce a sodium ion solid-state battery.
[0054] Example 2
[0055] 1. Preparation method of flexible current collector:
[0056] (1) 20% graphene oxide was uniformly dispersed in water, mixed with 80% MXene aqueous dispersion, and ultrasonically dispersed to obtain a MXene / graphene oxide composite suspension (80%:20%);
[0057] (2) filtering and drying the MXene / graphene oxide composite suspension (80%:20%) in sequence to obtain a MXene / graphene oxide film (80%:20%);
[0058] (3) The MXene / graphene oxide film (80%:20%) was subjected to high temperature treatment to obtain a MXene / reduced graphene oxide film (80%:20%) with a thickness of 9 μm.
[0059] 2. Negative electrode preparation method:
[0060] (1) Disperse 2.0% CMC powder in pure water and stir evenly to obtain CMC glue with a solid content of 1.8%;
[0061] (2) Add 6.0% MXene aqueous dispersion to the CMC glue with a solid content of 1.8%, stir evenly, then add 4.0% conductive carbon black, continue stirring until evenly mixed, and obtain a low solid content conductive glue;
[0062] (3) Add 85% hard carbon to the low-solid content conductive glue, stir evenly, then add 3.0% SBR, continue stirring until evenly mixed, and obtain the negative electrode slurry;
[0063] (4) The prepared negative electrode slurry is coated on the surface of the MXene / reduced graphene oxide film, and then dried and punched to obtain a negative electrode sheet.
[0064] 3. Positive electrode preparation method:
[0065] (1) adding 85% conductive carbon black to 15% MXene aqueous dispersion, dispersing by ultrasonic, filtering and drying the obtained conductive carbon black / MXene (85%:15%) dispersion to obtain a conductive carbon black / MXene (85%:15%) composite film, grinding and sieving the composite film to obtain a conductive carbon black / MXene (85%:15%) composite material;
[0066] (2) Dispersing 5.0% PVDF in a solvent and stirring evenly to obtain a positive electrode gel;
[0067] (3) Add 5.0% conductive carbon black / MXene composite material to the glue solution, stir evenly, and add 90.0% NaNi 0.64 Fe 0.21 Mn 0.15 O2, and stirred evenly to obtain a positive electrode slurry;
[0068] (4) The prepared positive electrode slurry is coated on aluminum foil, and then dried and punched to obtain a positive electrode sheet.
[0069] 4. Sodium ion solid-state battery manufacturing method:
[0070] (1) PMMA, 1M NaPF6, and NMP were mixed evenly by magnetic force to prepare a solid electrolyte solution;
[0071] (2) evenly coating the solid electrolyte solution on the surface of the positive electrode sheet and drying it to obtain a positive electrode sheet / solid electrolyte layer;
[0072] (3) Place the positive electrode sheet / solid electrolyte layer into the battery shell with the solid electrolyte layer facing upward, drip the plasticizer EC:DEC=(1:1) on top of the solid electrolyte layer, then place the negative electrode sheet on top of the solid electrolyte layer, and install the gasket, spring, and battery shell in sequence to obtain a sodium ion solid-state battery.
[0073] Example 3
[0074] 1. Preparation method of flexible current collector:
[0075] (1) 30% graphene oxide was uniformly dispersed in water, mixed with 70% MXene aqueous dispersion, and ultrasonically dispersed to obtain a MXene / graphene oxide composite suspension (70%:30%);
[0076] (2) filtering and drying the MXene / graphene oxide composite suspension (70%:30%) in sequence to obtain a MXene / graphene oxide film (70%:30%);
[0077] (3) The MXene / graphene oxide film (70%:30%) was subjected to high temperature treatment to obtain a MXene / reduced graphene oxide film (70%:30%) with a thickness of 13 μm.
[0078] 2. Negative electrode preparation method:
[0079] (1) Disperse 1.3% CMC powder in pure water and stir evenly to obtain CMC glue with a solid content of 1.7%;
[0080] (2) Add 4.0% MXene aqueous dispersion to the CMC glue with a solid content of 1.7%, stir evenly, then add 5.0% conductive carbon black, continue stirring until evenly mixed, and obtain a low solid content conductive glue;
[0081] (3) Add 86.7% hard carbon to the low-solid content conductive glue, stir evenly, then add 1.0% SBR + 2.0% polyacrylonitrile multi-polymer emulsion, continue stirring until evenly mixed, and obtain the negative electrode slurry;
[0082] (4) The prepared negative electrode slurry is coated on the surface of the MXene / reduced graphene oxide film, and then dried and punched to obtain a negative electrode sheet.
[0083] 3. Positive electrode preparation method:
[0084] (1) adding 90% conductive carbon black to 10% MXene aqueous dispersion, dispersing by ultrasonic, filtering and drying the obtained conductive carbon black / MXene (90%:10%) dispersion to obtain a conductive carbon black / MXene (90%:10%) composite film, grinding and sieving the composite film to obtain a conductive carbon black / MXene (90%:10%) composite material;
[0085] (2) Dispersing 10.0% PVDF in a solvent and stirring evenly to obtain a positive electrode glue solution;
[0086] (3) Add 10.0% conductive carbon black / MXene composite material to the glue solution, stir evenly, and add 80.0% NaNi 0.26 Fe 0.33 Mn 0.31 Cu 0.1 O2, and stirred evenly to obtain a positive electrode slurry;
[0087] (4) The prepared positive electrode slurry is coated on aluminum foil, and then dried and punched to obtain a positive electrode sheet.
[0088] 4. Sodium ion solid-state battery manufacturing method:
[0089] (1) PVDF+PVC (2:1), 1M NaClO4, and NMP were mixed by magnetic force to obtain a solid electrolyte solution;
[0090] (2) evenly coating the solid electrolyte solution on the surface of the positive electrode sheet and drying it to obtain a positive electrode sheet / solid electrolyte layer;
[0091] (3) Place the positive electrode sheet / solid electrolyte layer into the battery shell with the solid electrolyte layer facing upward, drip the plasticizer EC:EMC=(1:1) on top of the solid electrolyte layer, then place the negative electrode sheet on top of the solid electrolyte layer, and install the gasket, spring, and battery shell in sequence to obtain a sodium ion solid-state battery.
[0092] Example 4 Comparative Example 1
[0093] 1. Current collector: The negative electrode current collector is made of aluminum foil.
[0094] 2. Negative electrode preparation method:
[0095] (1) Disperse 1.3% CMC powder in pure water and stir evenly to obtain CMC glue with a solid content of 1.7%;
[0096] (2) Add 4.0% MXene aqueous dispersion to the CMC glue with a solid content of 1.7%, stir evenly, then add 5.0% conductive carbon black, continue stirring until evenly mixed, and obtain a low solid content conductive glue;
[0097] (3) Add 86.7% hard carbon to the low-solid content conductive glue, stir evenly, then add 1.0% SBR + 2.0% polyacrylonitrile multi-polymer emulsion, continue stirring until evenly mixed, and obtain the negative electrode slurry;
[0098] (4) The prepared negative electrode slurry is coated on the surface of aluminum foil, and then dried and punched to obtain a negative electrode sheet.
[0099] 3. Positive electrode preparation method:
[0100] (1) Dispersing 10.0% PVDF in a solvent and stirring evenly to prepare a positive electrode glue solution;
[0101] (2) Add 9.0% conductive carbon black and 1.0% MXene composite material to the glue solution, stir evenly, and add 80.0% NaNi 0.26 Fe 0.33 Mn 0.31 Cu 0.10 O2, and stirred evenly to obtain a positive electrode slurry;
[0102] (3) The prepared positive electrode slurry is coated on aluminum foil, and then dried and punched to obtain a positive electrode sheet.
[0103] 4. Sodium ion solid-state battery manufacturing method:
[0104] (1) PVDF+PVC (2:1), 1M NaClO4, and NMP were mixed by magnetic force to obtain a solid electrolyte solution;
[0105] (2) evenly coating the solid electrolyte solution on the surface of the positive electrode sheet and drying it to obtain a positive electrode sheet / solid electrolyte layer;
[0106] (3) Place the positive electrode sheet / solid electrolyte layer into the battery shell with the solid electrolyte layer facing upward, drip the plasticizer EC:EMC=(1:1) on top of the solid electrolyte layer, then place the negative electrode sheet on top of the solid electrolyte layer, and install the gasket, spring, and battery shell in sequence to obtain a sodium ion solid-state battery.
[0107] Example 5 Electrochemical Performance Test
[0108] Examples 1 to 3 and Comparative Example 1 were subjected to 25°C cycle tests and 0.5°C cycles for 100 times. The test results are as follows:
[0109] plan Example 1 Example 2 Example 3 Comparative Example 1 Capacity retention rate 95.15% 94.93% 94.69% 90.31%
[0110] By comparing the room temperature cycle test data of the sodium ion battery in Examples 1 to 3 with that in Comparative Example 1, it can be seen that the solid-state battery manufacturing process in this scheme can effectively improve the cycle stability of the sodium ion solid-state battery and improve the electrochemical performance of the battery.
[0111] The specific embodiments described above further illustrate the objectives, technical solutions and beneficial effects of the present invention in detail. It should be understood that the above description is only a specific embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. A method for manufacturing a sodium ion solid-state battery using a flexible current collector, characterized in that: The sodium ion solid-state battery consists of a positive electrode, a negative electrode, and a solid electrolyte. The negative electrode uses a flexible current collector, and the solid electrolyte is a polymer solid electrolyte. The specific steps are as follows: (1) taking a polymer material, a sodium salt, and a solvent, and stirring them evenly by magnetic force to prepare a solid electrolyte solution; (2) evenly coating the solid electrolyte solution on the surface of the positive electrode sheet and drying it to obtain a positive electrode sheet / solid electrolyte layer; (3) placing the positive electrode sheet / solid electrolyte layer into a battery shell with the solid electrolyte layer facing upward, dropping a plasticizer on the solid electrolyte layer, and then placing the negative electrode sheet on the solid electrolyte layer, and sequentially installing a gasket, a spring, and a battery shell to prepare a sodium ion solid-state battery; The preparation steps of the flexible current collector include: (1) uniformly dispersing graphene oxide in water, mixing with a MXene aqueous dispersion, and ultrasonically dispersing to obtain a MXene / graphene oxide composite suspension; (2) filtering and drying the MXene / graphene oxide composite suspension in sequence to obtain a MXene / graphene oxide film; (3) subjecting the MXene / graphene oxide film to high temperature treatment to obtain a MXene / reduced graphene oxide film; the thickness of the MXene / reduced graphene oxide film is 7 to 16 μm, and the mass ratio of MXene to reduced graphene oxide is (70% to 90%): (10% to 30%).
2. The method for manufacturing a sodium ion solid-state battery using a flexible current collector according to claim 1, characterized in that: The specific method for preparing the negative electrode sheet is as follows: (1) Dispersing the binder material 1 in pure water and stirring evenly to obtain a high solid content binder solution; (2) Add MXene aqueous dispersion to the high solid content binder glue, stir evenly, add conductive agent, continue stirring until evenly, and obtain low solid content conductive glue; (3) Add the negative electrode active material to the low solid content conductive glue, stir evenly, add the binder material 2, continue stirring until evenly mixed, and obtain the negative electrode slurry; (4) The prepared negative electrode slurry is coated on the surface of the MXene / reduced graphene oxide film, and then dried and punched to obtain a negative electrode sheet.
3. The method for manufacturing a sodium ion solid-state battery using a flexible current collector according to claim 1, characterized in that: The specific method for preparing the positive electrode sheet is as follows: (1) adding conductive carbon black to a MXene aqueous dispersion, dispersing the conductive carbon black / MXene dispersion by ultrasonication, filtering and drying the obtained conductive carbon black / MXene dispersion to obtain a conductive carbon black / MXene composite film, grinding and sieving the composite film to obtain a conductive carbon black / MXene composite material; (2) dispersing the binder material in a solvent and stirring it evenly to obtain a positive electrode glue solution; (3) Adding the conductive carbon black / MXene composite material to the glue solution, stirring evenly, adding the positive electrode active material, stirring evenly, and preparing the positive electrode slurry; (4) The prepared positive electrode slurry is coated on aluminum foil, and then dried and punched to obtain a positive electrode sheet.
4. The method for manufacturing a sodium ion solid-state battery using a flexible current collector according to claim 3, characterized in that: The positive electrode active material is a layered oxide with a structural formula of NaxMeO2, wherein Me is selected from two or more of magnesium (Mg), manganese (Mn), iron (Fe), cobalt (Co), nickel (Ni), vanadium (V), copper (Cu), chromium (Cr), iridium (Ir), and ruthenium (Ru); the solvent is NMP; and the binder is PVDF.
5. The method for manufacturing a sodium ion solid-state battery using a flexible current collector according to claim 3, characterized in that: The mass ratio of the conductive carbon black / MXene composite material is (80% to 90%): (10% to 20%); the mass ratio of the positive electrode active material: the conductive carbon black / MXene composite material: the binder is (80 to 95): (2.5 to 10): (2.5 to 10), and the solid content of the positive electrode slurry is 40% to 60%.
6. The method for manufacturing a sodium ion solid-state battery using a flexible current collector according to claim 2, characterized in that: The negative electrode active material is hard carbon, and the negative electrode formula active material: conductive agent: binder 1: binder 2: MXene is in a mass ratio of (80-90): (3-5): (1-5): (2-5): (2-14), and the solid content of the negative electrode slurry is 40%-60%.
7. The method for manufacturing a sodium ion solid-state battery using a flexible current collector according to claim 6, characterized in that: The conductive agent is one or more of conductive carbon black, graphene, and carbon nanotubes; the binder 1 is sodium carboxymethyl cellulose (CMC); and the binder 2 is one or two of styrene-butadiene rubber (SBR) and polyacrylonitrile emulsions.
8. The method for manufacturing a sodium ion solid-state battery using a flexible current collector according to claim 1, characterized in that: The polymer material in the solid electrolyte is one or more of PEO, PVDF, PVC, and PMMA; the sodium salt is one or two of sodium hexafluorophosphate and sodium perchlorate; the solvent is N-methylpyrrolidone (NMP) or acetonitrile (ACN); and the plasticizer is two or more of ethylene carbonate (EC), diethyl carbonate (DEC), ethyl methyl carbonate (EMC), propylene carbonate (PC), and fluoroethylene carbonate (FEC).
Citation Information
Patent Citations
Flexible self-supporting electrode material for sodium-ion battery as well as application and preparation method of material
CN108183205A
Organic gel electrolyte, application, sodium-based double-ion organic solid-state battery and preparation method thereof
CN108183257A
Li-Ti3C2-rGO composite thin film material and preparation method thereof
CN109755538A
MXene aerogel lithium negative electrode current collector capable of rapidly charging and discharging at high rate, preparation method thereof and application thereof