A preparation method of battery-grade modified iron phosphate
By introducing resol phenolic resin and cetyltrimethylammonium acetate into iron phosphate powder, a nano-flake conductive carbon film is generated, which solves the problem of uneven distribution of conductive carbon film and improves the charging capacity of lithium iron phosphate batteries. Discharge performance, achieving efficient and cost-effective preparation of modified iron phosphate.
Patent Information
- Application Number
- CN202211521941.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-11-30
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2042-11-30
AI Technical Summary
In the existing lithium iron phosphate anode material production process, the uneven distribution of the conductive carbon film affects the charge and discharge performance of the lithium iron phosphate battery, and there is a lack of effective methods to improve this problem.
In the preparation process of iron phosphate powder, resol phenolic resin and cetyltrimethylammonium acetate are introduced, and preliminary carbonization is generated through slurry treatment, spray drying and oxygen-proof roasting to form a nano-flake conductive carbon film, which improves Distribution consistency of conductive carbon films.
Significantly improves the electrical properties and charge-discharge performance of lithium iron phosphate powder, similar to specifically adding graphene or carbon nanotubes with good conductivity, and has a high cost-effectiveness and is suitable for industrial applications.
Smart Images

Figure BDA0003971428230000071
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of lithium iron phosphate anode materials, and in particular relates to a method for preparing battery-grade modified iron phosphate. Background Art
[0002] Lithium iron phosphate batteries have become the mainstream of power batteries and energy storage batteries due to their long cycle life, good safety and improved design level. Their production capacity and output are showing a blowout trend. The output of lithium iron phosphate powder, the anode material used in them, has reached nearly 500,000 tons in 2021, and is expected to exceed 1 million tons in 2022.
[0003] The main production process of lithium iron phosphate powder, anode material, is high temperature solid phase synthesis. The conventional operation process of producing lithium iron phosphate powder by high temperature solid phase synthesis includes: firstly preparing battery grade iron phosphate powder, lithium carbonate powder, carbon source such as sucrose, pure water or ethanol and a small amount of additives into slurry, grinding to a fineness of 0.1-0.5μm, spray drying to obtain D 50 The spherical powder of 20-40μm is then reduced and sintered at 680-750℃ to obtain D 50 The spherical powder of 15-30μm is crushed by air flow to obtain D 50 1-2μm and lithium iron phosphate microsphere powder with appropriate particle size distribution. When preparing the slurry, a grinding dispersant can be added, and a doping element component that improves the intrinsic conductivity of lithium iron phosphate can be added; the D 50 The 1-2μm lithium iron phosphate microspheres are composed of dozens or hundreds of lithium iron phosphate primary crystals with an olivine structure, and the surface of the primary crystals is coated with a conductive carbon film. During the reduction sintering process, reducing components such as aldehydes and CO generated by thermal decomposition of sucrose reduce iron phosphate to ferrous phosphate, which then reacts with lithium ions in a solid phase to form lithium iron phosphate primary crystals with an olivine structure; a certain amount of carbon generated by thermal decomposition of sucrose forms a conductive coating thin layer on the surface of the lithium iron phosphate primary crystals, forms a conductive connecting carbon layer between the primary crystals, and also forms a conductive carbon film on the surface of the D 50 The surface of the 15-30μm lithium iron phosphate spherical powder forms a conductive carbon-rich shell. The formation of the carbon-rich shell is due to the difference between the non-water-soluble properties of iron phosphate and lithium carbonate and the extremely high water-soluble properties of sucrose, which makes the spray-dried powder such as D 50 In the 20-40μm spherical powder, sucrose is enriched on the surface of the spherical powder particles; therefore, the D 50 There is a very significant and inevitable uneven distribution of the conductive carbon coating amount, thickness and density between 1-2μm lithium iron phosphate microspheres. In short, the conventional production process of lithium iron phosphate powder for anode materials, such as D 50For 1-2μm lithium iron phosphate microsphere powder, there are very significant differences in the conductivity and the influence of the conductive carbon coating layer on the insertion / extraction rate of lithium ions, between the lithium iron phosphate microspheres and between the primary grains within the microspheres. This difference or inconsistency significantly affects the charge and discharge performance of the final lithium iron phosphate battery.
[0004] Therefore, it is necessary to improve the uniformity of carbon film coating and distribution, which plays an important role in the conductivity of lithium iron phosphate microspheres and the insertion / extraction rate of lithium ions. To achieve this goal, the slurry ratio, grinding depth, spray drying conditions, reduction sintering conditions, and air flow crushing intensity are generally comprehensively controlled. This is a matter that must be considered and optimized from beginning to end in the test and production of lithium iron phosphate by high-temperature solid phase synthesis. However, in the prior art, there are few effective and cost-effective methods suitable for industrial application that can generate partial conductive carbon film in lithium iron phosphate microspheres or significantly improve the generation of conductive carbon film and improve the distribution consistency of conductive carbon film by introducing or forming appropriate materials during the preparation of iron phosphate powder. Summary of the invention
[0005] In order to solve the above technical problems, the present invention provides a method for preparing battery-grade modified iron phosphate, which sets a slurry treatment step after washing the iron phosphate, applies water-soluble resol phenolic resin and hexadecyl trimethyl ammonium acetate, sprays and dries, and calcines in oxygen isolation to generate iron phosphate powder containing preliminary carbon formation; the preliminary carbon formation of 0.5-0.8wt% contained in the iron phosphate powder, in the process of producing lithium iron phosphate powder by high-temperature solid phase synthesis, is mostly dispersed into nano-thin sheets with an outer size of less than 30nm during the grinding of ingredients, and can generate a part of the conductive carbon film in the lithium iron phosphate and significantly improve the generation of the conductive carbon film, improve the distribution consistency of the conductive carbon film, thereby improving the electrical properties of the lithium iron phosphate powder and the charge and discharge performance of the further preparation of lithium iron phosphate batteries. The method has a high cost-effectiveness ratio and is suitable for application by iron phosphate manufacturers.
[0006] The preparation method of battery-grade modified ferric phosphate of the present invention comprises the following steps:
[0007] (1) Purified phosphoric acid or purified phosphoric acid aqueous solution, purified ferrous sulfate aqueous solution and optional water are respectively controlled at required flow rates, continuously mixed, and then continuously mixed with hydrogen peroxide at a controlled flow rate, and injected into an oxidation reaction tank in which the solution temperature is continuously stirred and controlled at 90-95° C. by heating, and the average residence time of the solution in the oxidation reaction tank is 20-30 min, to obtain a solution A containing trivalent iron ions and phosphoric acid; in the solution A, the phosphoric acid concentration is controlled to be 1.0-1.5 mol / L, the molar concentration ratio of iron ions to phosphoric acid is 0.96-1.0:1, and the feeding molar concentration of H2O2 is 0.55-0.65 times the molar concentration of iron ions;
[0008] (2) the circulating slurry in the precipitation reaction tank is mixed with a sodium hydroxide aqueous solution of 1.0-2.0 mol / L and 75-85° C. at a volume flow ratio of 5-10:1, and then continuously mixed with the solution A containing trivalent iron ions and phosphoric acid at a controlled flow rate, injected into the precipitation reaction tank under continuous stirring, and continuously flowed into the aging treatment tank through the high-position discharge port, and aged at 70-80° C.; wherein the flow ratio of the sodium hydroxide solution and the solution A is controlled according to the pH value range of 1.8-2.5 of the slurry in the precipitation reaction tank; the average residence time of the slurry in the precipitation reaction tank is 0.5-1 h, and the aging treatment in the aging treatment tank is 5-10 h. During the aging treatment, only low-speed stirring is performed to ensure that the solid matter is substantially evenly dispersed in the slurry;
[0009] (3) After the aging treatment in step (2), the slurry is filtered through a belt filter or a plate and frame filter, and washed with water at 70-80° C. until the effluent conductivity is ≤150 μS / cm. The filter cake is transferred into a slurry treatment tank, slurried with a resin aqueous solution B at 60-80° C., and slurried for 0.5-1 h. The slurry for slurry treatment is prepared according to a solid concentration of 45-50 wt% of ferric phosphate dihydrate and a solid concentration of 0.5-1.0 wt% of phenolic resin. The resin aqueous solution B contains a phenolic resin with a weight average molecular weight of 2000-3000 and hexadecyltrimethylammonium acetate, wherein the weight percentage concentration ratio of the phenolic resin to the hexadecyltrimethylammonium acetate is 1:0.1-0.15;
[0010] (4) The slurry after the coating treatment in step (3) is spray-dried at 200-250° C., and the dried material is roasted in an oxygen-proof furnace at 500-550° C. for 4-8 hours and crushed to obtain battery-grade modified iron phosphate.
[0011] In the preparation method of battery-grade modified ferric phosphate of the present invention, according to the specific effects and comparison of the subsequent related embodiments and comparative examples, it can be inferred that the phenolic resin and hexadecyltrimethylammonium acetate introduced into the dihydrate ferric phosphate slurry before spray drying can be roughly evenly distributed on the surface and between the ferric phosphate grains of the spherical powder obtained by spray drying, and a certain amount of initial carbon, such as 40-50% of the amount of phenolic resin added, is formed between the anhydrous ferric phosphate grains in the battery-grade modified ferric phosphate powder obtained by roasting at 500-550°C in an oxygen-proof furnace, and the initial carbon formed is also roughly evenly distributed on the surface and between the anhydrous ferric phosphate grains in the ferric phosphate powder; the obtained modified ferric phosphate powder is used for high-temperature solidification. In the process of producing lithium iron phosphate powder by phase synthesis method, as the iron phosphate powder, lithium carbonate powder, sucrose and water slurry are ground to a fine powder particle size such as 0.2-0.5 μm, the 0.5-0.8wt% preliminary carbon contained in the iron phosphate powder is mostly dispersed into nano flakes with an outer size of less than 30nm. Although the weight content of the preliminary carbon is not high, the number of dispersed nano flakes is large, part of which adheres to the surface of lithium carbonate crystal grains, and part of which still adheres to the surface of anhydrous iron phosphate crystal grains, thereby improving the binding ability of sucrose liquid with the surface of lithium carbonate crystal grains and the surface of anhydrous iron phosphate crystal grains in the grinding slurry. Part of the nano flakes are dispersed in the sucrose liquid to reduce the fluidity of the sucrose liquid, thereby making the spray-dried product such as D 50 The distribution uniformity of sucrose in the 20-40μm spherical powder is significantly improved, and the surface enrichment of the spherical powder is significantly reduced. After reduction sintering at 680-750℃, the obtained D 50 The surface of the 15-30μm lithium iron phosphate spherical powder basically no longer forms a carbon-rich shell, so that the lithium iron phosphate spherical powder is neutralized and the air flow crushed as D 50 In the 1-2 μm lithium iron phosphate microspheres, the conductive carbon film generated by sucrose and the preliminary carbonized nanosheets has significantly improved coating and coating uniformity on the surface of the lithium iron phosphate primary crystal grains and between the primary crystal grains. Under the same conductive carbon coating amount conditions and the same sucrose carbon generation coating amount conditions, the charge and discharge performance of the lithium iron phosphate battery finally prepared is much better than when the phenolic resin and / or hexadecyltrimethylammonium acetate are not introduced in step (3). Therefore, the phenolic resin and hexadecyltrimethylammonium acetate introduced in step (3) are calcined in an oxygen-insulated furnace at 500-550° C. in step (4) to generate preliminary carbon. In the process of using iron phosphate for high-temperature solid-phase synthesis to produce lithium iron phosphate powder, in addition to being basically converted into conductive carbon, it can also significantly improve the generation of conductive carbon film and improve the distribution consistency of conductive carbon film, thereby improving the electrical properties of lithium iron phosphate powder. The conductive effect is equivalent to the addition of graphene and carbon nanotubes with good conductivity.
[0012] The phenolic resin is prepared by the following steps: using a stirred reactor with condensation reflux and vacuum distillation; after sealing and replacing air, adding water and a formaldehyde aqueous solution with a concentration of 37-40wt% and phenol under continuous stirring, sealing the reactor, heating to 60-70°C, adding ammonia water dropwise for reaction for 20-30min, heating to 70-75°C for reaction for 20-30min, heating to 85-90°C and maintaining the temperature for reaction for 2-3h, then performing vacuum distillation for 2-4h until the solid concentration in the feed liquid reaches 35-40wt%, cooling to room temperature, and obtaining the phenolic resin; wherein the ingredients are water, formaldehyde aqueous solution, phenol, and ammonia in a weight ratio of 0.5-1.0:1.3-1.6:1:0.03-0.05; the vacuum distillation conditions include: a reaction feed liquid temperature of 70-80°C, an exhaust vacuum absolute pressure of 30-45kPa, and a condensation temperature of 10-25°C. The obtained phenolic resin is a resol phenolic resin, containing formaldehyde ≤ 0.1wt%, phenol ≤ 0.1wt%, with little odor, no visible change after shading and storage for 1 month, normal use effect, and can be diluted with water for use. Its weight average molecular weight can be determined by viscosity and concentration.
[0013] The hexadecyl trimethyl ammonium acetate, as a cationic surfactant, can be used as a morphology regulator in the process of preparing ferric phosphate by precipitation method, but the concentration in the slurry is generally 5g / L or above 0.4wt%, which is much higher than the concentration of 0.05-0.15wt% used in the present invention, and there is no similar application as the present invention as a phenolic resin coating auxiliary agent in the prior art. The advantage of using acetate is that it avoids the hazards of high temperature corrosion of nitrogen oxides and chlorides generated by hexadecyl trimethyl ammonium acetate and hexadecyl trimethyl ammonium chloride.
[0014] It is inferred that a certain degree of complexation should occur between the phenolic resin and hexadecyltrimethylammonium acetate in the resin aqueous solution B. The battery-grade modified iron phosphate obtained in step (4) is gray, and detection shows that 0.5-1.0wt% of residual carbon is generated, and the carbon deposition rate is 45-50wt% and is relatively certain; it is convenient for subsequent accurate batching and formation of lithium iron phosphate powder with the required determined carbon content.
[0015] In the prior art of producing lithium iron phosphate powder by high-temperature solid phase synthesis, there are also records of adding polymers such as phenolic resin when grinding and preparing iron phosphate powder, lithium carbonate powder and water slurry. However, the subsequent related embodiments and comparative examples show that the effect of introducing phenolic resin and hexadecyltrimethylammonium acetate into the dihydrate iron phosphate slurry before spray drying is better in the present invention. The reason is inferred to be that when adding polymers such as phenolic resin when grinding and preparing iron phosphate powder, lithium carbonate powder, sucrose and water slurry, even if combined with sucrose and glucose, the dispersion effect of the present invention cannot be achieved under the condition of obtaining the same conductive carbon coating amount, and thus the overall conductive effect is worse.
[0016] During the aging process of step (2), iron phosphate dihydrate is recrystallized, and a small amount of iron hydroxide mixed therein also generates iron phosphate dihydrate, which facilitates the filtering and washing operations of step (3). The conversion of iron hydroxide to iron phosphate dihydrate is very critical, which will increase the cycle life of the final lithium iron phosphate battery. In the preparation method of battery-grade modified iron phosphate of the present invention, the pH value range of the slurry in the precipitation reaction tank of step (2) is better when it is controlled to be 2.0-2.2, and the amount of iron hydroxide impurities generated can be controlled, and phosphoric acid does not need to be added during the aging process.
[0017] The continuous mixing of the solution and slurry in steps (1) and (2) can be carried out by a static mixer or a venturi arranged in the pipeline, which has the advantages of high mixing efficiency and fast mixing rate, and can avoid or reduce the amount of side reactions. For example, the molar concentration of H2O2 is 0.55-0.60 times the molar concentration of iron ions to ensure 100% generation of trivalent iron ions, and the concentration of phosphoric acid in solution A is in a higher range of 1.3-1.5 mol / L, such as 1.8-2.0 mol / L, and a better reaction effect can be obtained.
[0018] In the preparation method of battery-grade modified iron phosphate of the present invention, during the slurry treatment process of step (3), magnesium acetate accounting for 1.5-2.5 mol% of the iron phosphate can also be added for doping to improve the intrinsic conductivity of the prepared lithium iron phosphate primary grains. At this time, in the solution A of step (1), the molar concentration ratio of iron ions to phosphoric acid can be controlled to, for example, 0.96-0.98:1. It can be seen from the relevant embodiments and comparative examples that the same amount of magnesium acetate is better when added in this step than when added during the grinding of iron phosphate powder with lithium carbonate powder, sucrose and water slurry. The reason is that, except for a small part of the added magnesium ions being adsorbed and bound by ferric phosphate dihydrate, most of the added magnesium ions are calcined at 500-550° C. in the oxygen-proof furnace of step (4) to form highly active and widely dispersed magnesium oxide. The magnesium oxide is used in the process of using iron phosphate powder for high-temperature solid phase synthesis to produce lithium iron phosphate powder. As the iron phosphate powder is ground with lithium carbonate powder, sucrose and water slurry to a fine powder particle size of 0.2-0.5 μm, the magnesium oxide is calcined to form highly active and widely dispersed magnesium oxide. The magnesium hydroxide dissolved into a gel is further dispersed, and most of it is doped and enters the lattice of the primary lithium iron phosphate grains after further reduction sintering at 680-750°C; magnesium acetate is added during the grinding and mixing of the iron phosphate powder, lithium carbonate powder, sucrose and water slurry. The presence of a large amount of lithium carbonate causes the magnesium ions to form magnesium carbonate that is not easy to gel and has a low dispersion. After further reduction sintering at 680-750°C, the number of magnesium ions doped and entering the lattice of the primary lithium iron phosphate grains is small, or the uniformity is poor, resulting in an inconsistent improvement in the intrinsic conductivity of the prepared primary lithium iron phosphate grains and a poor overall doping effect.
[0019] After filtration in step (3), the filter cake is washed with water at 70-80° C. until the effluent conductivity is ≤150 μS / cm. At this time, the effluent is tested with a 0.5 mol / L barium chloride-1.0 mol / L hydrochloric acid solution and is free of barium sulfate turbidity, indicating that the sodium ions and sulfate ions have been washed away. DETAILED DESCRIPTION
[0020] The technical solution of the present invention is specifically described and illustrated below in conjunction with embodiments, but does not constitute a limitation of the present invention.
[0021] Example 1
[0022] The resol phenolic resin was prepared according to the following steps: a 3L stirred reactor with condensation reflux and vacuum distillation was used; the reactor was evacuated to an absolute pressure of 10 kPa, filled with 99.9% nitrogen to 300 kPa, and the evacuation and nitrogen filling operations were repeated 3 times to test the tightness and replace the air; under continuous stirring, 800 g of water, 1500 g of 37 wt% formaldehyde aqueous solution, and 1000 g of phenol were added in sequence, the reactor was sealed, and heating was performed immediately. After 20 minutes, the feed liquid was heated to 65°C, and 400 ml of 6 mol% ammonia water was added dropwise. The reaction was continued for 20 minutes, the temperature was raised to 73°C for 30 minutes, the temperature was raised to 85°C and the temperature was maintained for 3 hours, and then vacuum distillation was performed for 1 hour until the solid concentration in the feed liquid reached 38wt%, and the mixture was cooled to room temperature to obtain a resol phenolic resin; the vacuum distillation conditions included: a reaction feed liquid temperature of 76-80°C, an absolute vacuum pressure of 35kPa, and a condensation temperature of 15°C; the obtained resol phenolic resin contained formaldehyde ≤0.1wt%, phenol ≤0.1wt%, had a small odor, and had no visible change after being stored in a dark place for 1 month. According to the test results of its viscosity and concentration at 25°C, its weight average molecular weight was estimated to be 2600.
[0023] Example 2
[0024] On a test line with an hourly production capacity of about 3 kg of iron phosphate, 10 kg of modified iron phosphate of this embodiment was prepared according to the following steps:
[0025] (1) Refined phosphoric acid with a concentration of 85 wt %, a refined ferrous sulfate aqueous solution with a concentration of 2.0 mol / L, and water are respectively controlled at required flow rates, continuously mixed, and then continuously mixed with hydrogen peroxide at a controlled flow rate, and injected into an oxidation reaction tank in which the solution temperature is continuously stirred and controlled at 92-93° C. by heating, and the average residence time of the solution in the oxidation reaction tank is 25 min, thereby obtaining a solution A containing trivalent iron ions and phosphoric acid; in the control solution A, the phosphoric acid concentration is 1.2 mol / L, the molar concentration ratio of iron ions to phosphoric acid is 0.98:1, and the feeding molar concentration of H2O2 is 0.62 times the molar concentration of iron ions; in the detection solution A, the concentration of divalent ferrous ions is lower than the detection limit of 0.00005 mol / L;
[0026] (2) The circulating slurry in the precipitation reaction tank is mixed with a 2.0 mol / L, 80° C. sodium hydroxide aqueous solution at a required flow rate, respectively, at a volume flow rate ratio of 8:1, and then continuously mixed with the solution A containing trivalent iron ions and phosphoric acid at a required flow rate, injected into the precipitation reaction tank under continuous stirring, and continuously flowed into the aging treatment tank through the high-position discharge port, and aged at 75° C.; wherein the flow rate ratio of the sodium hydroxide solution and the solution A is controlled according to the pH value range of 2.1 of the slurry in the precipitation reaction tank; the average residence time of the slurry in the precipitation reaction tank is 0.8 h, and the aging treatment in the aging treatment tank is 8 h. During the aging treatment, only low-speed stirring is performed to ensure that the solid matter is substantially evenly dispersed in the slurry;
[0027] (3) After the aging treatment in step (2), the slurry is filtered through a plate and frame filter and washed with water at 75°C until the outlet water conductivity is ≤150μS / cm. After the filter cake is squeezed, the material is moved into a slurry treatment tank and slurried with a 70°C resin aqueous solution B. The slurry is slurried with water for 0.5h. The slurry is prepared according to a solid concentration of 50wt% of ferric phosphate dihydrate and a solid concentration of 1.0wt% of phenolic resin. The resin aqueous solution B contains a phenolic resin with a weight average molecular weight of 2600 prepared in Example 1 at a solid concentration of 2.0wt% and 0.25wt% of hexadecyltrimethylammonium acetate.
[0028] (4) The slurry after the slurry treatment in step (3) was spray-dried at 250°C to obtain D 50 The spherical powder of 32 μm was dried and calcined in an oxygen-isolated furnace at 520°C for 6 h, and crushed to -200 mesh to obtain battery-grade modified iron phosphate.
[0029] In step (1), the total content of metal ions other than iron in the refined phosphoric acid is less than 0.0005 mol / L, and the total content of components other than water+phosphoric acid is less than 0.1 wt%; the total content of metal ions other than iron in the refined ferrous sulfate aqueous solution is less than 0.0005 mol / L.
[0030] The continuous mixing of the solution and slurry in steps (1) and (2) is carried out by a static mixer arranged in the pipeline.
[0031] In step (3), the slurry after aging treatment is filtered in the mother liquor of the plate and frame filter. After standing for 3 hours, the total phosphorus and total iron of the supernatant are both lower than 0.001 mol / L, indicating that the precipitation rate of phosphorus and iron is very high. After washing with water at 75°C until the conductivity of the outlet water is ≤150μS / cm, the outlet water is tested with 0.5mol / L barium chloride-1.0mol / L hydrochloric acid solution to find that there is no barium sulfate turbidity, and it is considered that the sodium ions and sulfate groups have been washed away. The output of the filter cake after squeezing is measured to have a dihydrate iron phosphate content of 68wt%, a free water content of 32wt%, and a dry basis sodium ion and sulfate group content of less than 0.001mol / L.
[0032] Example 3
[0033] The modified ferric phosphate of this embodiment is prepared basically according to the method of Example 2, except that in step (1), the phosphoric acid concentration in solution A is controlled to be 1.5 mol / L, and the molar concentration of H2O2 is 0.57 times the molar concentration of iron ions; in the detection solution A, the concentration of divalent ferrous ions is lower than the detection limit of 0.00005 mol / L.
[0034] Example 4
[0035] The modified iron phosphate of this embodiment is prepared basically according to the method of Example 2, except that in step (3), the coating treatment slurry is prepared according to the solid concentration of 50wt% of dihydrate iron phosphate and the solid concentration of 0.5wt% of phenolic resin.
[0036] Example 5
[0037] The modified iron phosphate of this embodiment is prepared basically according to the method of embodiment 3, except that during the slurry coating process in step (3), magnesium acetate accounting for 2.0 mol % of the iron phosphate is also added for doping.
[0038] Comparative Example 1
[0039] The iron phosphate of this comparative example was prepared substantially according to the method of Example 3, except that in step (3), the coating treatment slurry was prepared only at a solid concentration of 50 wt% of iron phosphate dihydrate, without adding phenolic resin and hexadecyltrimethylammonium acetate.
[0040] Comparative Example 2
[0041] The modified ferric phosphate of this comparative example was prepared basically according to the method of Example 3, except that in step (3), the coating treatment slurry was prepared according to a solid concentration of 50 wt% of ferric phosphate dihydrate and a solid concentration of 1.0 wt% of phenolic resin, and hexadecyltrimethylammonium acetate was not added.
[0042] Comparative Example 3
[0043] The modified ferric phosphate of this comparative example was prepared basically according to the method of Example 3, except that in step (3), the coating treatment slurry was prepared according to a solid concentration of 50 wt% of ferric phosphate dihydrate and a solid concentration of 0.15 wt% of hexadecyltrimethylammonium acetate, and no phenolic resin was added.
[0044] Example 6
[0045] In a test line capable of producing 25 kg of lithium iron phosphate per day, the modified iron phosphate prepared in the above Examples 2-5 and Comparative Examples 1-3 was used to prepare about 1 kg of lithium iron phosphate respectively according to the following steps: the required amount (the specific amount of sucrose was determined by repeated trial and error according to the carbon content of 2.0 wt% in the obtained lithium iron phosphate) of modified iron phosphate powder, lithium carbonate powder, sucrose and water were mixed into a slurry, and ground in a sand mill to a fineness of D 50 0.32-0.35μm; after grinding, the slurry was spray dried, and the obtained D 50 The 31-33μm spherical powder was put into a sagger and reduced and sintered in a 720℃ push plate furnace for 8h. The obtained lithium iron phosphate spherical powder (fineness range D 50 23-26μm) was crushed by air flow to obtain D 50 1.3-1.4μm lithium iron phosphate powder (carefully adjust the airflow crushing conditions to make the particle size distribution of each lithium iron phosphate powder basically consistent and comparable).
[0046] In the above preparation process of lithium iron phosphate, samples were taken from the slurry after grinding, and the slurry was tested by transmission electron microscopy (TEM). It was found that the slurry after grinding of the modified iron phosphate obtained by the above Examples 2-5 contained a large number of nanosheets with an outer size of less than 30 nm, part of which adhered to the surface of lithium carbonate grains, part of which still adhered to the surface of anhydrous iron phosphate grains, and part of which was dispersed in the sucrose solution. When the modified iron phosphate obtained by the above Comparative Examples 1-3 was used, the number of nanosheets with an outer size of less than 30 nm was much smaller and the dispersion was much lower; the D obtained by reduction sintering 50 The 23-26μm spherical powder was detected by scanning electron microscopy (SEM), and it was found that the carbon distribution uniformity in the spherical particles when the modified iron phosphate obtained by the above Examples 1-5 was higher, the enrichment on the surface of the spherical powder was lower, and the carbon film, the coating and coating uniformity on the surface of the lithium iron phosphate primary grains and between the primary grains were also higher, which were better than the modified iron phosphate obtained by the above Comparative Examples 1-3.
[0047] Comparative Example 4
[0048] The iron phosphate prepared in Comparative Example 1 was used as a raw material, and the lithium iron phosphate of this comparative example was prepared basically according to the method of Example 6. The difference was that in the slurry ingredients before grinding in the sand mill, 1.0wt% of phenolic resin with a weight average molecular weight of 2600 and 0.125wt% of hexadecyltrimethylammonium acetate were added in proportion to the solid matter and the iron phosphate. The specific amount of sucrose was determined by repeated trial and error according to the carbon content of 2.0wt% in the obtained lithium iron phosphate.
[0049] Comparative Example 5
[0050] The lithium iron phosphate of this comparative example was prepared using the iron phosphate prepared in comparative example 1 as a raw material, substantially according to the method of Example 6, except that magnesium acetate accounting for 2.0 mol % of the iron phosphate was added to the slurry ingredients before grinding in a sand mill for doping.
[0051] Test Example 1
[0052] The modified iron phosphate prepared in Examples 2-5 and Comparative Examples 1-5 and the lithium iron phosphate prepared in Example 6 were sampled as anode materials to prepare 10 R2025 button batteries. The manufacturing process of the R2025 button battery includes: mixing the lithium iron phosphate and the PVDF binder at a mass ratio of 100:2.5, adding an appropriate amount of NMP to mix, and evenly coating the obtained mixed slurry on the aluminum foil with a 250μm slit die, first coating one side, drying and then coating the other side, and rolling at a pressure of 10MPa after drying to obtain a rolled positive electrode sheet, using a metal lithium sheet as the negative electrode, using a Celgard 2300 microporous membrane as a separator, and 1.0mol / L lithium hexafluorophosphate ethylene carbonate (EC): dimethyl carbonate (DMC) = 1:3 (volume ratio) solution as an electrolyte, and assembling the R2025 button battery in a glove box.
[0053] The electrochemical performance of the battery was tested, wherein the charge and discharge cut-off voltage was 2.5-3.8V (vs. Li / Li + ), constant temperature of 25°C; the batteries of Examples 2-4 and Comparative Examples 1-4 were subjected to 5 charge-discharge cycles at a charge-discharge rate of 0.1C, and then 300 charge-discharge cycles at a charge-discharge rate of 1C. The batteries of Example 5 and Comparative Example 5 were subjected to 5 charge-discharge cycles at a charge-discharge rate of 0.1C, and then 300 charge-discharge cycles at a charge-discharge rate of 1C, and finally 300 charge-discharge cycles at a charge-discharge rate of 5C. The main test results are listed in Table 1.
[0054] Table 1: Half-cell test results of lithium iron phosphate prepared by modified iron phosphate in Examples 2-5 and Comparative Examples 1-5, unit: mAh / g
[0055]
Claims
1. A method for preparing battery-grade modified ferric phosphate, comprising the following steps: (1) Purified phosphoric acid or purified phosphoric acid aqueous solution, purified ferrous sulfate aqueous solution and water are respectively controlled at required flow rates, continuously mixed, and then continuously mixed with hydrogen peroxide at a required controlled flow rate, and injected into an oxidation reaction tank which is continuously stirred and the solution temperature is controlled at 90-95° C. by heating, and the average residence time of the solution in the oxidation reaction tank is 20-30 min, to obtain a solution A containing trivalent iron ions and phosphoric acid; in the solution A, the phosphoric acid concentration is controlled to be 1.0-1.5 mol / L, the molar concentration ratio of iron ions to phosphoric acid is 0.96-1.0:1, and the feeding molar concentration of H2O2 is 0.55-0.65 times the molar concentration of iron ions; (2) the circulating slurry in the precipitation reaction tank is continuously mixed with a 1.0-2.0 mol / L, 75-85° C. sodium hydroxide aqueous solution at a volume flow ratio of 5-10:1, and then continuously mixed with the solution A containing trivalent iron ions and phosphoric acid at a required controlled flow rate, injected into the precipitation reaction tank under continuous stirring, and continuously flowed into the aging treatment tank through the high-position discharge port, and aged at 70-80° C.; wherein, The flow ratio of the sodium hydroxide solution and solution A is controlled according to the pH value range of the slurry in the precipitation reaction tank, which is 1.8-2.5; The average residence time of the slurry in the precipitation reaction tank is 0.5-1h, and the aging treatment time in the aging treatment tank is 5-10h; (3) After the aging treatment in step (2), the slurry is filtered through a belt filter or a plate and frame filter, and washed with water at 70-80° C. until the effluent conductivity is ≤150 μS / cm. The filter cake is transferred into a slurry treatment tank and slurried with a resin aqueous solution B at 60-80° C. The slurry treatment time is 0.5-1 h. The resin aqueous solution B contains a phenolic resin with a weight average molecular weight of 2000-3000 and hexadecyltrimethylammonium acetate, wherein the weight percentage concentration ratio of the phenolic resin to the hexadecyltrimethylammonium acetate is 1:0.1-0.
15. The slurry for slurry treatment is prepared according to a solid concentration of 45-50 wt% of ferric phosphate dihydrate and a solid concentration of 0.5-1.0 wt% of phenolic resin. During the slurry treatment, magnesium acetate is also added, and the amount of magnesium acetate added is 1.5-2.5 mol% of the ferric phosphate. (4) The slurry after the coating treatment in step (3) is spray-dried at 200-250° C., and the dried material is roasted in an oxygen-proof furnace at 500-550° C. for 4-8 hours and crushed to obtain battery-grade modified iron phosphate.
2. The method for preparing battery-grade modified iron phosphate according to claim 1, characterized in that: The phenolic resin is prepared by the following steps: using a stirred reactor with condensation reflux and vacuum distillation; after sealing and replacing air, adding water and a formaldehyde aqueous solution with a concentration of 37-40wt% and phenol under continuous stirring, closing the reactor, heating to 60-70°C, adding ammonia water dropwise for reaction for 20-30min, heating to 70-75°C for reaction for 20-30min, heating to 85-90°C and maintaining the temperature for reaction for 2-3h, then performing vacuum distillation for 2-4h until the solid concentration in the feed liquid reaches 35-40wt%, cooling to room temperature, and obtaining the phenolic resin; wherein the weight ratio of water, formaldehyde aqueous solution, phenol and ammonia is 0.5-1.0:1.3-1.6:1:0.03-0.05; the vacuum distillation conditions include: a reaction feed liquid temperature of 70-80°C, an exhaust vacuum absolute pressure of 30-45kPa, and a condensation temperature of 10-25°C.
3. The method for preparing battery-grade modified iron phosphate according to claim 1, characterized in that: The pH value range of the slurry in the precipitation reaction tank in step (2) is controlled to be 2.0-2.2.
Citation Information
Patent Citations
High-density spherical iron phosphate and manufacture method thereof
CN101269807A
Method for preparing nanoscale lithium ion battery LiFePo4 / C anodal material
CN102110811A
High-power environment-friendly lithium iron phosphate battery and preparation method thereof
CN109786618A
Preparation method of composite high-temperature-resistant lithium battery diaphragm material
CN113764820A
Battery-grade iron phosphate, preparation method therefor, and application thereof
WO2022127323A1