Nylon polyphenylene ether composite material and preparation method and application thereof

By adding potassium titanate whiskers and polytetrafluoroethylene powder to nylon and polyphenylene ether materials, combined with additives such as compatibility agents, a nylon polyphenylene ether composite material that is resistant to wear, high temperature and dimensional stability is prepared, and the material is solved The problem of insufficient performance has broadened its application in the fields of automobiles and electronics.

CN115895248BActive Publication Date: 2024-12-03HUIZHOU WATER NEW MATERIAL CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202211506943.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-11-29
Publication Date
2024-12-03
Estimated Expiration
2042-11-29

AI Technical Summary

Technical Problem

Nylon and polyphenylene ether materials each have insufficient mechanical strength, heat resistance, hydrolysis resistance and other properties, which limit their application in the automotive and electronic appliance fields.

Method used

Potassium titanate whiskers and polytetrafluoroethylene powder are used as filler materials, combined with nylon and polyphenylene ether resin for compounding, and compatibility agents, antioxidants, lubricants and coupling agents are added to prepare wear-resistant products through melt extrusion. , nylon polyphenylene ether composite material that is resistant to high temperature, stable dimensionality and low water absorption.

Benefits of technology

It significantly improves the performance defects of a single resin, obtains an alloy material with excellent performance, with higher gloss, wear resistance and dimensional stability, broadens the application field of materials, and is suitable for high-temperature and wear-resistant spare parts with high precision requirements. .

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115895248B_ABST
    Figure CN115895248B_ABST
Patent Text Reader

Abstract

The present invention relates to a nylon polyphenylene ether composite material and its preparation method and application. The composite material comprises the following components in mass percentage: 20% to 60% nylon resin; 10% to 50% polyphenylene ether resin; 3% to 10% compatibilizer; 5% to 50% potassium titanate whisker; and 5% to 20% polytetrafluoroethylene powder; the diameter of the potassium titanate whisker is 0.1 μm to 2 μm, and the length is 1 μm to 100 μm; the particle size of the polytetrafluoroethylene powder is less than 200 μm, and the D50 particle size is less than 40 μm. The nylon polyphenylene ether composite material is wear-resistant, high-strength, high-temperature resistant, low in water absorption, stable in size, and resistant to organic solvents, and can meet the needs of industries such as automobiles, electronic appliances, etc. for composite materials with high performance and high quality appearance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of polymer composite materials, in particular to a nylon polyphenylene ether composite material and a preparation method and application thereof. Background Art

[0002] Polyamide (PA), commonly known as nylon, refers to a type of crystalline polymer containing an amide bond (—NHCO—) in the main chain of the molecule. It has high mechanical strength, good fluidity, good toughness, self-lubrication, good friction resistance, excellent heat resistance, electrical properties and weather resistance. However, it has shortcomings such as easy water absorption and poor dimensional stability (large shrinkage), which limit its application.

[0003] Polyphenylene ether (PPO) resin is a non-crystalline thermoplastic polymer with high mechanical strength, high temperature resistance, low specific gravity, low water absorption, excellent hydrolysis resistance, dimensional stability and excellent electrical properties. However, it has shortcomings such as poor fluidity and poor resistance to organic solvents, which limit its application.

[0004] Polymer alloys are a type of material with uniform appearance and multi-component polymer systems containing two or more different structures. They can improve the physical and mechanical properties and processing properties of polymer materials, reduce costs, and expand the scope of use. They are one of the important ways to achieve polymer modification and produce new materials with multiple properties. Although many polymer alloys have been reported, there are still few studies on polymer alloys composed of nylon and polyphenylene ether. Summary of the invention

[0005] Based on this, it is necessary to provide a nylon polyphenylene ether composite material that is wear-resistant, high-strength, high-temperature resistant, low in water absorption, dimensionally stable, and resistant to organic solvents to address the above problems, which can meet the needs of the automotive, electronics and other industries for high-performance and high-quality appearance composite materials.

[0006] The technical solution is as follows:

[0007] A nylon polyphenylene ether composite material comprises the following components in percentage by mass:

[0008]

[0009] The potassium titanate whisker has a diameter of 0.1 μm to 2 μm and a length of 1 μm to 100 μm;

[0010] The particle size of the polytetrafluoroethylene micropowder is less than 200 μm, and the D50 particle size is less than 40 μm.

[0011] In one embodiment, the potassium titanate whisker has a diameter of 0.1 μm to 1 μm and a length of 10 μm to 20 μm.

[0012] In one embodiment, the chemical composition of the potassium titanate whiskers is one or more of K2O·2TiO2, K2O·4TiO2, K2O·6TiO2 and K2O·8TiO2.

[0013] In one embodiment, the polyphenylene ether resin has an Ubbelohde intrinsic viscosity of 0.2 dl / g to 0.8 dl / g in chloroform at 25°C.

[0014] In one embodiment, the compatibilizer is a maleic anhydride grafted polymer with a grafting rate of 0.5% to 5.0%.

[0015] In one embodiment, the maleic anhydride grafted polymer is selected from one or a mixture of maleic anhydride grafted polyolefin elastomer, maleic anhydride grafted hydrogenated styrene-butadiene block copolymer and maleic anhydride grafted polyphenylene ether.

[0016] In one embodiment, the nylon resin is selected from aliphatic semi-crystalline nylon and / or semi-aromatic semi-crystalline nylon with a melting point.

[0017] In one embodiment, the nylon resin is selected from the group consisting of polycaprolactam, polybutylene adipamide, polypentamethylene adipamide, polyhexamethylene adipamide, polyhexamethylene sebacamide, polydecanediamine, polyhexamethylene dodecanediamine, polydecanediamine, polyundecanolactam, polydodecanoic acid lactam, polydodecanoic acid lactam, polydodecanoic acid lactam, polyhexamethylene terephthalamide / isophthalamide copolymer nylon, polyhexamethylene terephthalamide / hexamethylene adipamide copolymer nylon, polyhexamethylene terephthalamide / isophthalamide / hexamethylene adipamide copolymer nylon, polyhexamethylene terephthalamide / caprolactam copolymer nylon, polyhexamethylene terephthalamide / 2-methylpentamethylene terephthalamide copolymer nylon, polynonane terephthalamide and polydecanediamine, or a mixture of several thereof.

[0018] In one embodiment, the nylon polyphenylene ether composite material further includes one or more of an antioxidant, a lubricant, a nucleating agent and a coupling agent.

[0019] In one embodiment, the nylon polyphenylene ether composite material further comprises, by mass percentage, 0.2% to 0.5% antioxidant; 0.1% to 0.5% lubricant; 0.1% to 1% nucleating agent; and 0.1% to 1% coupling agent.

[0020] In one embodiment, the antioxidant is selected from N,N'-1,6-hexylene-bis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionamide], S9228, a mixture of one or more of tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate, N,N'-bis-(3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionyl)hexanediamine, tris(2,4-di-tert-butylphenyl)phosphite, bis(2,4-dicumylphenyl)pentaerythritol diphosphite, potassium iodide and cuprous iodide.

[0021] In one embodiment, the lubricant is one or a mixture of calcium stearate, N,N'-ethylene bisstearamide, ethylene acrylic acid copolymer, OP wax and E wax.

[0022] In one embodiment, the nucleating agent is selected from one or a mixture of long carbon chain carboxylic acid calcium salt nucleating agents, substituted aromatic heterocyclic phosphate nucleating agents, aromatic carboxylic acid aluminum salt nucleating agents and aromatic amide nucleating agents.

[0023] In one embodiment, the coupling agent is an aminosilane coupling agent.

[0024] The present invention also provides a method for preparing the nylon polyphenylene ether composite material as described above, comprising the following steps:

[0025] The nylon resin, polyphenylene ether resin, compatibilizer, potassium titanate whisker and polytetrafluoroethylene powder are mixed, melted and extruded.

[0026] The present invention also provides the application of the nylon polyphenylene ether composite material as described above. The technical solution is as follows:

[0027] An electronic appliance comprises the nylon polyphenylene ether composite material as described above.

[0028] A car comprises the nylon polyphenylene ether composite material as described above.

[0029] The present invention has the following beneficial effects:

[0030] The nylon polyphenylene ether composite material of the present invention uses nylon and polyphenylene ether as the compound, and adopts compatibilizer, potassium titanate whisker and polytetrafluoroethylene powder, which can significantly improve the performance defects of each single resin, and obtain an alloy material with excellent and balanced performance such as wear resistance, mechanical properties, processability, temperature resistance, chemical resistance, hydrolysis resistance and dimensional stability. Further, by adopting potassium titanate whisker and polytetrafluoroethylene powder to reinforce the filling material, the appearance of the material can be obtained, which is superior to that of conventional glass fiber, carbon fiber and mineral powder filling and reinforcement, and has higher gloss, better wear resistance and better dimensional stability, which greatly broadens the application field of nylon and polyphenylene ether materials, such as being applicable to the fields of electronic appliances and automobiles, and more specifically, being applicable to high-precision high-temperature wear-resistant parts and components such as vehicle-mounted cameras, sliders, gears, etc. BRIEF DESCRIPTION OF THE DRAWINGS

[0031] Figure 1 This is a diagram showing the effect of the nylon polyphenylene ether composite material obtained in Comparative Example 3 after friction testing;

[0032] Figure 2 This is a diagram showing the effect of the nylon polyphenylene ether composite material prepared in Example 2 after friction testing. DETAILED DESCRIPTION

[0033] The present invention will be further described in detail below in conjunction with specific embodiments. The present invention can be implemented in many different forms and is not limited to the embodiments described herein. On the contrary, the purpose of providing these embodiments is to make the disclosure of the present invention more thoroughly understood.

[0034] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those generally understood by those skilled in the art of the present invention. The terms used herein in the specification of the present invention are only for the purpose of describing specific embodiments and are not intended to limit the present invention. The term "and / or" used herein includes any and all combinations of one or more related listed items.

[0035] In the present invention, the technical features described in an open manner include closed technical solutions composed of the listed features, and also include open technical solutions containing the listed features.

[0036] In the present invention, when it comes to numerical ranges, unless otherwise specified, the above numerical ranges are considered continuous and include the minimum and maximum values ​​of the range, as well as each value between such minimum and maximum values. Further, when a range refers to an integer, each integer between the minimum and maximum values ​​of the range is included. In addition, when multiple ranges are provided to describe features or characteristics, the ranges can be merged. In other words, unless otherwise specified, all ranges disclosed herein should be understood to include any and all subranges included therein.

[0037] The temperature parameters in the present invention, if not specifically limited, allow for both constant temperature treatment and treatment within a certain temperature range. The constant temperature treatment allows the temperature to fluctuate within the precision range controlled by the instrument.

[0038] In the present invention, when it comes to the unit of the data range, if there is a unit only after the right endpoint, it means that the units of the left endpoint and the right endpoint are the same. For example, 150-160°C means that the units of the left endpoint "150" and the right endpoint "160" are both ℃ (Celsius).

[0039] In the present invention, in the description of the invention, the meaning of "several" is at least two, such as two, three, etc., unless otherwise clearly and specifically defined. In the description of the present application, the meaning of "several" is at least one, such as one, two, etc., unless otherwise clearly and specifically defined.

[0040] If not otherwise specified, all embodiments and optional embodiments of the present invention can be combined with each other to form a new technical solution.

[0041] If not otherwise specified, all steps of the present invention may be performed sequentially or randomly, preferably sequentially. For example, the method includes steps (a) and (b), which means that the method may include steps (a) and (b) performed sequentially, or may include steps (b) and (a) performed sequentially. For example, the method may further include step (c), which means that step (c) may be added to the method in any order, for example, the method may include steps (a), (b) and (c), or may include steps (a), (c) and (b), or may include steps (c), (a) and (b), etc.

[0042] It should be noted that, in the description of the present invention, directional words such as the terms "center", "lateral", "longitudinal", "length", "width", "thickness", "up", "down", "front", "back", "left", "right", "vertical", "horizontal", "top", "bottom", "inside", "outside", "clockwise", "counterclockwise", etc., indicating directions and positional relationships are based on the directions or positional relationships shown in the accompanying drawings, and are only for the convenience of narrating the present invention and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific direction, be constructed and operated in a specific direction, and cannot be understood as limiting the specific protection scope of the present invention.

[0043] Where “including,” “having,” and “comprising” are used herein, it is intended to cover a non-exclusive inclusion, and another component may also be added unless explicit limiting terms such as “only,” “consisting of,” etc. are used.

[0044] Unless mentioned to the contrary, terms in the singular may include plural forms and should not be construed as being one in number.

[0045] In the present invention, the grafting ratio refers to the ratio of the mass of the polar monomer grafted onto the polymer to the mass of the grafted polymer.

[0046] Potassium titanate whisker (PTW) is a needle-shaped artificial fiber originally developed by DuPont in the United States. Its main chemical composition is K2O·nTiO2 (n is an integer greater than 0), its diameter is within a few microns, its length is within tens of microns, and it has a certain aspect ratio (generally L / D>20). It is different from ordinary powder fillers. Its fibrous microstructure makes it have a significant reinforcement effect when used as a filler in polymer materials, and can overcome the problems of large anisotropy of ordinary fiber-reinforced materials and floating fibers on the surface of products.

[0047] Aiming at the defects of nylon and polyphenylene ether, the present invention adopts potassium titanate whiskers and other raw materials to provide a nylon polyphenylene ether composite material which is wear-resistant, high-strength, high-temperature resistant, low in water absorption, dimensional stable and resistant to organic solvents.

[0048] The technical solution is as follows:

[0049] A nylon polyphenylene ether composite material comprises the following components in percentage by mass:

[0050]

[0051] The potassium titanate whisker has a diameter of 0.1 μm to 2 μm and a length of 1 μm to 100 μm;

[0052] The particle size of the polytetrafluoroethylene micropowder is less than 200 μm, and the D50 particle size is less than 40 μm.

[0053] The nylon polyphenylene ether composite material of the present invention uses nylon and polyphenylene ether as the compound, and adopts a compatibilizer, potassium titanate whisker and polytetrafluoroethylene powder, which can significantly improve the performance defects of each single resin, and obtain an alloy material with excellent and balanced performance such as wear resistance, mechanical properties, processability, temperature resistance, chemical resistance, hydrolysis resistance and dimensional stability. Furthermore, by adopting potassium titanate whisker and polytetrafluoroethylene powder to reinforce the filling material, the appearance of the material can be obtained, which is superior to that of conventional glass fiber, carbon fiber and mineral powder filling and reinforcement, and has higher gloss, better wear resistance and better dimensional stability, which greatly broadens the application field of nylon and polyphenylene ether materials.

[0054] In the present invention, the nylon polyphenylene ether composite material includes 5% to 50% potassium titanate whiskers by mass percentage, including but not limited to 5%, 10%, 12%, 15%, 20%, 25%, 30%, 35%, 40%, 45% and 50%, preferably 10% to 40%.

[0055] In the present invention, the diameter of the potassium titanate whisker is 0.1 μm to 2 μm, and the length is 1 μm to 100 μm; preferably, the diameter of the potassium titanate whisker is 0.1 μm to 1 μm, and the length is 10 μm to 20 μm.

[0056] In one embodiment, the chemical composition of the potassium titanate whiskers is K2O·2TiO2, K2O·4TiO2, K2O·6TiO2, K2O·8TiO2, preferably K2O·6TiO2 or K2O·8TiO2.

[0057] In one embodiment, the potassium titanate whisker is NP-TW2 of Shanghai Fengzhu Whisker, with a diameter of 0.1 μm to 2 μm and a length of 1 μm to 100 μm.

[0058] In one embodiment, the potassium titanate whisker is TISMO-N produced by Otsuka Whiskers of Japan, and has a diameter of 0.1 μm to 1 μm and a length of 10 μm to 20 μm.

[0059] In the present invention, the nylon polyphenylene ether composite material also includes 20% to 60% nylon resin by mass percentage, including but not limited to 20%, 25%, 30%, 35%, 40%, 45%, 50%, 55% and 60%, preferably 22% to 55%.

[0060] In one embodiment, the nylon resin is selected from aliphatic semi-crystalline nylon and / or semi-aromatic semi-crystalline nylon with a melting point.

[0061] In one embodiment, the nylon resin is selected from the group consisting of polycaprolactam, polybutylene adipamide, polypentamethylene adipamide, polyhexamethylene adipamide, polyhexamethylene sebacamide, polydecanediamine, polyhexamethylene dodecanediamine, polydecanediamine, polyundecanolactam, polydodecanoic acid lactam, polydodecanoic acid lactam, polydodecanoic acid lactam, polyhexamethylene terephthalamide / isophthalamide copolymer nylon, polyhexamethylene terephthalamide / hexamethylene adipamide copolymer nylon, polyhexamethylene terephthalamide / isophthalamide / hexamethylene adipamide copolymer nylon, polyhexamethylene terephthalamide / caprolactam copolymer nylon, polyhexamethylene terephthalamide / 2-methylpentamethylene terephthalamide copolymer nylon, polynonane terephthalamide and polydecanediamine, or a mixture of several thereof. More preferably, at least one aliphatic semi-crystalline nylon (having a melting point T m 210℃~270℃), and / or semi-aromatic semi-crystalline nylon (with a melting point T m is 270℃~340℃).

[0062] In one embodiment, the nylon resin is PA66 EPR24 (melting point 252° C.) of Henan Shenma Group, PA612 (melting point 217° C.) of DuPont, USA, or PPA N600 (melting point 308° C.) of Zhejiang Xinhecheng Co., Ltd.

[0063] In the present invention, the nylon polyphenylene ether composite material also includes 10% to 50% polyphenylene ether resin by mass percentage, including but not limited to 10%, 15%, 20%, 25%, 30%, 35%, 40%, 45% and 50%, preferably 15% to 30%.

[0064] In one embodiment, in chloroform at 25°C, the Ubbelohde intrinsic viscosity of the polyphenylene ether resin is 0.2 dl / g to 0.8 dl / g, including but not limited to 0.2 dl / g, 0.3 dl / g, 0.4 dl / g, 0.45 dl / g, 0.5 dl / g, 0.6 dl / g, 0.7 dl / g and 0.8 dl / g, preferably 0.4 dl / g to 0.6 dl / g.

[0065] In one embodiment, the polyphenylene ether resin is LXR045 produced by Shanxi Ruicheng Bluestar Chemical Industry, and its intrinsic viscosity measured by Ubbelohde viscometer in chloroform at 25°C is 0.45 dl / g.

[0066] In the present invention, the nylon polyphenylene ether composite material further comprises 3% to 10% of a compatibilizer by mass percentage, including but not limited to 2%, 3%, 5%, 6%, 7%, 8%, 9% and 10%, preferably 3% to 8%.

[0067] In one embodiment, the compatibilizer is a maleic anhydride grafted polymer with a grafting rate of 0.5% to 5.0%. It can be understood that the grafting rate of the maleic anhydride grafted polymer is 0.5% to 5.0%, including but not limited to: 0.5%, 0.6%, 0.7%, 0.8%, 0.9%, 1.0%, 1.2%, 1.4%, 1.5%, 1.6%, 1.8%, 2.0%, 2.2%, 2.5%, 2.8%, 3.0%, 3.2%, 3.5%, 3.6%, 3.8%, 4.0%, 4.2%, 4.4%, 4.5%, 4.6%, 4.8%, 5.0%. Preferably, the grafting rate of the maleic anhydride grafted polymer is 0.5% to 3%, which can ensure that the nylon polyphenylene ether composite system has good compatibility and can effectively improve the delamination problem caused by the incompatibility of the two resins.

[0068] In one embodiment, the maleic anhydride grafted polymer is selected from one or a mixture of maleic anhydride grafted polyolefin elastomer (POE-g-MAH), maleic anhydride grafted hydrogenated styrene-butadiene block copolymer (SEBS-g-MAH) and maleic anhydride grafted polyphenylene ether (PPO-g-MAH).

[0069] Polytetrafluoroethylene, commonly known as the king of plastics, has a melting point of 325°C to 335°C and has excellent chemical stability, corrosion resistance, sealing, high lubricity and non-stickiness, electrical insulation and good anti-aging resistance. The present invention uses polytetrafluoroethylene micropowder and potassium titanate whisker as a reinforcing filling material to obtain a material appearance that is superior to conventional glass fiber, carbon fiber, and mineral powder filling and reinforcement, with higher gloss, better wear resistance, and better dimensional stability, which greatly broadens the application field of nylon and polyphenylene ether materials.

[0070] In the present invention, the nylon polyphenylene ether composite material includes 5% to 20% polytetrafluoroethylene powder by mass percentage, including but not limited to 5%, 6%, 7%, 8%, 9%, 10%, 11%, 12%, 13%, 15%, 16%, 17%, 18%, 19% and 20%, preferably 10% to 18%.

[0071] In the present invention, the particle size of the polytetrafluoroethylene powder is less than 200 μm, and the D50 particle size is less than 40 μm.

[0072] In one embodiment, the particle size of the polytetrafluoroethylene powder is 10 μm to 200 μm, and the D50 particle size is 20 μm to 30 μm.

[0073] In one embodiment, the polytetrafluoroethylene powder is KTL-630 produced by Kitamura of Japan, and the D50 particle size is 20 μm to 30 μm.

[0074] In one embodiment, the nylon polyphenylene ether composite material comprises the following components in weight %:

[0075]

[0076]

[0077] In one embodiment, the nylon polyphenylene ether composite material further includes one or more of an antioxidant, a lubricant, a nucleating agent and a coupling agent. Among them, the antioxidant can enhance the stability of the composite material. The lubricant can lubricate, improve dispersibility and demoulding properties. The nucleating agent makes the mechanical properties, heat resistance and dimensional stability of the material more excellent. The coupling agent is conducive to enhancing the wettability and dispersibility between inorganic materials and organic materials, and can greatly improve the flexural strength, tensile strength and interlaminar shear strength of the composite material, and significantly improve the wet electrical properties.

[0078] In one embodiment, the nylon polyphenylene ether composite material further comprises 0.2% to 0.5% of an antioxidant, including but not limited to 0.2%, 0.3%, 0.4% and 0.5%, preferably 0.2% to 0.4%.

[0079] In one embodiment, the antioxidant is selected from N,N'-1,6-hexylene-bis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionamide] (antioxidant 1098), S9228, tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate]pentaerythritol, N,N'-bis-(3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionyl)hexanediamine, tris(2,4-di-tert-butylphenyl)phosphite, bis(2,4-dicumylphenyl)pentaerythritol diphosphite, potassium iodide and cuprous iodide, or a mixture of several thereof. Preferably, the antioxidant is antioxidant 1098 and S9228 and antioxidant 1098 are used in combination. The mass ratio of S9228 is 1:(0.1~5).

[0080] In one embodiment, the nylon polyphenylene ether composite material further includes 0.1% to 0.5% of anti-lubricant, including but not limited to 0.1%, 0.2%, 0.3%, 0.4% and 0.5%, preferably 0.2% to 0.5%.

[0081] In one embodiment, the lubricant is one or a mixture of calcium stearate, N,N'-ethylene bisstearamide, ethylene acrylic acid copolymer, OP wax and E wax.

[0082] In one embodiment, the lubricant is OP wax.

[0083] In one embodiment, the nylon polyphenylene ether composite material also includes 0.1% to 1% of a nucleating agent, including but not limited to 0.1%, 0.2%, 0.3%, 0.4%, 0.5%, 0.6%, 0.7%, 0.8%, 0.9% and 1%, preferably 0.2% to 0.8%.

[0084] In one embodiment, the nucleating agent is selected from one or a mixture of long carbon chain carboxylic acid calcium salt nucleating agents, substituted aromatic heterocyclic phosphate nucleating agents, aromatic carboxylic acid aluminum salt nucleating agents and aromatic amide nucleating agents.

[0085] In one embodiment, the nucleating agent is Clariant's CAV102.

[0086] In one embodiment, the nylon polyphenylene ether composite material also includes 0.1-1% of a coupling agent, including but not limited to 0.1%, 0.2%, 0.3%, 0.4%, 0.5%, 0.6%, 0.7%, 0.8%, 0.9% and 1%, preferably 0.2% to 0.8%.

[0087] In one embodiment, the coupling agent is an aminosilane coupling agent. Aminosilane coupling agents are beneficial to enhancing the wettability and dispersibility between inorganic materials and organic materials, can greatly improve the flexural strength, tensile strength and interlaminar shear strength of the composite material, and significantly improve the wet electrical properties, and the flexural strength and tensile strength of the composite material before and after immersion in water are increased.

[0088] In one embodiment, the coupling agent is selected from one or a mixture of KH550, KH560 and KH570.

[0089] In one embodiment, the nylon polyphenylene ether composite material comprises the following components in percentage by mass:

[0090]

[0091]

[0092] In one embodiment, the nylon polyphenylene ether composite material comprises the following components in percentage by mass:

[0093]

[0094] The present invention also provides a method for preparing the nylon polyphenylene ether composite material as described above, comprising the following steps:

[0095] The nylon resin, polyphenylene ether resin, compatibilizer, potassium titanate whisker and polytetrafluoroethylene powder are mixed, melted and extruded.

[0096] In one embodiment, the preparation method of the nylon polyphenylene ether composite material comprises the following steps:

[0097] The nylon resin, the polyphenylene ether resin, the compatibilizer, the polytetrafluoroethylene powder, the antioxidant, the lubricant, and the nucleating agent are mixed to obtain a mixture I;

[0098] The pre-hydrolyzed coupling agent and potassium titanate whisker are mixed with high-speed stirring, and then placed in an oven at 100° C. to 120° C. to dry for 2 to 3 hours to obtain a mixture II;

[0099] The mixture I and the mixture II are mixed, melted, extruded and granulated.

[0100] In one embodiment, a twin-screw extruder is used for melt extrusion, the screw aspect ratio of the twin-screw extruder is (44-48): 1, the screw speed is (200-400) rpm, the barrel of the twin-screw extruder is a ten-section barrel, the first section of the barrel is connected to the main feeding device, the fourth section of the barrel is exhausted, the sixth section of the barrel is connected to the side feeding device, and the ninth section of the barrel is vacuumed; the barrel temperature is set as: 220±60℃ for the first section of the barrel, 240±60℃ for the second section of the barrel, 250±60℃ for the third section of the barrel, 260±60℃ for the fourth section of the barrel, 260±60℃ for the fifth section of the barrel, 270±60℃ for the sixth section of the barrel, 270±60℃ for the seventh section of the barrel, 270±60℃ for the eighth section of the barrel, 270±60℃ for the ninth section of the barrel, 270±60℃ for the tenth section of the barrel, and 280±60℃ for the head.

[0101] The present invention also provides the application of the nylon polyphenylene ether composite material as described above. The technical solution is as follows:

[0102] An electronic appliance comprises the nylon polyphenylene ether composite material as described above.

[0103] A car comprises the nylon polyphenylene ether composite material as described above.

[0104] The following is a specific embodiment, and the manufacturers and models of the main raw materials of the present invention are as follows:

[0105] The proportions and percentages of the components in the embodiments are based on mass, and the components are described as follows:

[0106] A is PA resin:

[0107] A1: PA66 EPR24, melting point 252°C, purchased from Henan Shenma Group;

[0108] A2: PA612, melting point 217°C, purchased from DuPont, USA;

[0109] A3: PPAN600, melting point 308℃, Zhejiang Xinhecheng Co., Ltd.

[0110] B is PPO resin:

[0111] LXR045, intrinsic viscosity 0.45 dl / g, purchased from Shanxi Ruicheng Bluestar Chemical;

[0112] C is a compatibilizer:

[0113] C1: PPO-g-MAH, GPM-450C MAH grafting rate 3%, purchased from Ningbo Nengzhiguang;

[0114] C2: POE-g-MAH, CMG-5805MAH grafting rate 0.5% to 1%, purchased from Shanghai Jiayirong;

[0115] D is potassium titanate whisker:

[0116] D1: TISMO-N, diameter 0.1 μm-1 μm, length 10 μm-20 μm, purchased from Otsuka Whiskers, Japan;

[0117] D2: NP-TW2, diameter 0.1 μm-2 μm, length 1 μm-100 μm, purchased from Shanghai Fengzhu Whisker;

[0118] E is polytetrafluoroethylene powder:

[0119] E1: KTL-630, D50 particle size 20 μm to 30 μm, purchased from Kitamura, Japan;

[0120] E2: FA-500H, D50 particle size is 400μm~800μm, Daikin Fluorochemical;

[0121] F is an antioxidant:

[0122] Antioxidant 1098 and S9228 is compounded in a mass ratio of 1:2;

[0123] G is lubricant:

[0124] OP wax

[0125] H is a nucleating agent:

[0126] CAV102, purchased from Clariant;

[0127] I is a coupling agent:

[0128] KH550;

[0129] J is alkali-free chopped glass fiber:

[0130] ECS11-3-568H, diameter 11 μm, purchased from Jushi Group;

[0131] In Examples 1-5 and Comparative Examples 1-6, ingredients were weighed and prepared according to Table 2, and PA resin, PPO resin, compatibilizer, polytetrafluoroethylene powder, antioxidant, lubricant, and nucleating agent were mixed to obtain a mixture I; the pre-hydrolyzed coupling agent and potassium titanate whisker were stirred and mixed at high speed and then placed in an oven at 120° C. and dried for 2-3 hours to obtain a mixture II; finally, the mixtures I and II were respectively put into the main feeding hopper and the side feeding hopper, and melt-extruded in proportion through a twin-screw extruder to form granules. Specifically, the barrel temperatures of Example 1, Example 2, Example 3, Comparative Example 1, Comparative Example 2, Comparative Example 3 and Comparative Example 6 are set to: 220±5°C for the first barrel, 240±5°C for the second barrel, 250±5°C for the third barrel, 260±5°C for the fourth barrel, 260±5°C for the fifth barrel, 270±5°C for the sixth barrel, 270±5°C for the seventh barrel, 270±5°C for the eighth barrel, 270±5°C for the ninth barrel, and 270±5°C for the tenth barrel. , machine head 280±5℃; the barrel temperatures of Example 4, Example 5, Comparative Example 4 and Comparative Example 5 are set as: 260±5℃ for the first section of the barrel, 280±5℃ for the second section of the barrel, 300±5℃ for the third section of the barrel, 300±5℃ for the fourth section of the barrel, 300±5℃ for the fifth section of the barrel, 310±5℃ for the sixth section of the barrel, 310±5℃ for the seventh section of the barrel, 310±5℃ for the eighth section of the barrel, 310±5℃ for the ninth section of the barrel, 310±5℃ for the tenth section of the barrel, and 320±5℃ for the machine head.

[0132] Table 1

[0133]

[0134] The PA / PPO composite materials prepared in Examples 1-5 and Comparative Examples 1-6 were molded into standard test specimens according to national standards and subjected to mechanical property related tests.

[0135] The notched impact test is carried out in accordance with the national standard GB / T 1843.

[0136] The tensile test is carried out in accordance with the national standard GB / T 1040.

[0137] The bending test is carried out in accordance with the national standard GB / T 9341.

[0138] The thermal deformation (1.80MPa / 4.0mm) test is carried out in accordance with the national standard GB / T1634.

[0139] The friction coefficient test is carried out in accordance with GB / T 10006-2021.

[0140] Gloss: Gloss test is carried out in accordance with the national standard GB / T 9754.

[0141] Chemical resistance: GB standard tensile specimens made by injection molding were subjected to stress by a homemade fixture and immersed in glacial acetic acid for organic solvent resistance testing.

[0142] The test results of Examples 1-5 and Comparative Examples 1-6 are shown in Table 2.

[0143] Table 2

[0144]

[0145]

[0146] As can be seen from Table 2, the composite materials provided by Examples 1-5 of the present invention have good wear resistance, high temperature resistance, glossiness, mechanical strength, chemical resistance and dimensional stability, are suitable for injection molding processing, and meet the needs of high-precision wear-resistant parts.

[0147] By comparing Example 1 and Comparative Example 1, it can be seen that the addition of PPO is omitted, and the shrinkage and water absorption of the composite material are significantly increased. By comparing Example 2 and Comparative Example 2, it can be seen that the composite material has good gloss and low wear without adding potassium titanate whiskers for reinforcement, but its mechanical strength, heat resistance, wear resistance (friction coefficient), shrinkage and other properties are poor. By comparing Example 2 and Comparative Example 3, it can be seen that the addition of PTFE powder is omitted, and the wear resistance of the composite material is poor, especially the wear amount is significantly increased. By comparing Example 4 and Comparative Example 4, it can be seen that the mechanical properties of the composite material are not much different when potassium titanate whiskers are replaced with an equal amount of glass fiber, but its wear resistance, gloss and shrinkage (vertical direction) are obviously much worse. By comparing Example 4 and Comparative Example 5, it can be seen that the use of PTFE powder with a coarser particle size makes the wear resistance and gloss of the composite material significantly poor. By comparing Example 1 and Comparative Example 6, it can be seen that the chemical resistance of the composite material is very poor when nylon is omitted.

[0148] Figure 1 This is a picture showing the effect of the nylon polyphenylene ether composite material obtained in Comparative Example 3 after the friction test (the wear marks are deeper); Figure 2 This is the effect diagram of the nylon polyphenylene ether composite material obtained in Example 2 after the friction test (the wear marks are very shallow). Figure 1 and Figure 2 It can be seen that adding PTFE micropowder can effectively reduce abrasion and improve the wear resistance of materials.

[0149] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above-described embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.

[0150] The above-mentioned embodiments only express several implementation methods of the present invention, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the invention patent. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, and these all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.

Claims

1. A nylon polyphenylene ether composite material, It is characterized in that Made of the following components in percentage by mass: Nylon resin 20%~60%; Polyphenylene ether resin 10% to 50%; Compatibilizer 3% to 10%; Potassium titanate whiskers 5% to 50%; Polytetrafluoroethylene powder 5% to 20%; Antioxidant 0.2%~0.5%; Lubricant 0.1%~0.5%; Nucleating agent 0.1%~1%; as well as Coupling agent 0.1%~1%; The potassium titanate whisker has a diameter of 0.1µm to 1µm and a length of 10µm to 20µm; The particle size of the polytetrafluoroethylene powder is 10 μm to 200 μm, and the D50 particle size is 20 μm to 30 μm.

2. The nylon polyphenylene ether composite material according to claim 1, It is characterized in that The chemical composition of the potassium titanate whisker is K 2 O·2TiO 2 , K 2 O·4TiO 2 , K 2 O·6TiO 2 and K 2 O·8TiO 2 One or more of the .

3. The nylon polyphenylene ether composite material according to claim 1, It is characterized in that The polyphenylene ether resin has an Ubbelohde intrinsic viscosity of 0.2 dl / g to 0.8 dl / g in chloroform at 25°C.

4. The nylon polyphenylene ether composite material according to claim 1, It is characterized in that The compatibilizer is a maleic anhydride grafted polymer with a grafting rate of 0.5% to 5.0%.

5. The nylon polyphenylene ether composite material according to claim 4, It is characterized in that The maleic anhydride grafted polymer is selected from one or a mixture of maleic anhydride grafted polyolefin elastomer, maleic anhydride grafted hydrogenated styrene-butadiene block copolymer and maleic anhydride grafted polyphenylene ether.

6. The nylon polyphenylene ether composite material according to any one of claims 1 to 5, It is characterized in that The nylon resin is selected from aliphatic semi-crystalline nylon and / or semi-aromatic semi-crystalline nylon.

7. The nylon polyphenylene ether composite material according to claim 6, It is characterized in that The nylon resin is selected from one or a mixture of polycaprolactam, polybutylene adipamide, polypentamethylene adipamide, polyhexamethylene adipamide, polyhexamethylene sebacamide, polydecanediamine, polyhexamethylene dodecanediamine, polydecanediamine, polyundecanolactam, polydodecanoic acid lactam, polydodecanoic acid lactam, polydodecanoic acid lactam, polyhexamethylene terephthalamide / hexamethylene isophthalamide copolymer nylon, polyhexamethylene terephthalamide / hexamethylene adipamide copolymer nylon, polyhexamethylene terephthalamide / hexamethylene isophthalamide / hexamethylene adipamide copolymer nylon, polyhexamethylene terephthalamide / caprolactam copolymer nylon, polyhexamethylene terephthalamide / 2-methylpentamethylene terephthalamide copolymer nylon, polynonane terephthalamide and polydecanediamine.

8. The nylon polyphenylene ether composite material according to any one of claims 1 to 5, It is characterized in that The antioxidant is selected from one or a mixture of N,N'-1,6-hexylene-bis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionamide], Doverphos® S9228, pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate, N,N'-bis-(3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionyl)hexanediamine, tris(2,4-di-tert-butylphenyl)phosphite, potassium iodide and cuprous iodide; and / or The lubricant is one or a mixture of calcium stearate, N,N'-ethylene bisstearamide, ethylene acrylic acid copolymer, OP wax and E wax; and / or The nucleating agent is selected from one or a mixture of long carbon chain carboxylic acid calcium salt nucleating agents, substituted aromatic heterocyclic phosphate nucleating agents, aromatic carboxylic acid aluminum salt nucleating agents and aromatic amide nucleating agents; and / or The coupling agent is an aminosilane coupling agent.

9. The nylon polyphenylene ether composite material according to claim 1, It is characterized in that Made of the following components in percentage by mass: Nylon resin 32%; Polyphenylene ether resin 22%; Compatibilizer 10%; Potassium titanate whiskers 20%; Polytetrafluoroethylene powder 15%; Antioxidant 0.3%; Lubricant 0.3%; Nucleating agent 0.2%; as well as Coupling agent 0.2%; Wherein, the nylon resin is PA66 EPR24; The polyphenylene ether resin is LXR045; The compatibilizer is formed by mixing PPO-g-MAH-GPM-450C and POE-g-MAH-CMG-5805, and the mass percentages of PPO-g-MAH-GPM-450C and POE-g-MAH-CMG-5805 in the nylon polyphenylene ether composite material are both 5%; The potassium titanate whisker is TISMO-N; The polytetrafluoroethylene powder is KTL-630; The antioxidant 1098 and Doverphos® S9228 are compounded in a mass ratio of 1:2; The lubricant is OP wax; The nucleating agent is CAV102; The coupling agent is KH550.

10. The nylon polyphenylene ether composite material according to claim 1, It is characterized in that Made of the following components in percentage by mass: Nylon resin 30%; Polyphenylene ether resin 19%; Compatibilizer 10%; Potassium titanate whiskers 30%; Polytetrafluoroethylene powder 10%; Antioxidant 0.3%; Lubricant 0.3%; Nucleating agent 0.2%; as well as Coupling agent 0.2%; Wherein, the nylon resin is PA66 EPR24; The polyphenylene ether resin is LXR045; The compatibilizer is formed by mixing PPO-g-MAH-GPM-450C and POE-g-MAH-CMG-5805, and the mass percentages of PPO-g-MAH-GPM-450C and POE-g-MAH-CMG-5805 in the nylon polyphenylene ether composite material are both 5%; The potassium titanate whisker is TISMO-N; The polytetrafluoroethylene powder is KTL-630; The antioxidant 1098 and Doverphos® S9228 are compounded in a mass ratio of 1:2; The lubricant is OP wax; The nucleating agent is CAV102; The coupling agent is KH550.

11. The nylon polyphenylene ether composite material according to claim 1, It is characterized in that Made of the following components in percentage by mass: Nylon resin 30%; Polyphenylene ether resin 19%; Compatibilizer 10%; Potassium titanate whiskers 30%; Polytetrafluoroethylene powder 10%; Antioxidant 0.3%; Lubricant 0.3%; Nucleating agent 0.2%; as well as Coupling agent 0.2%; Wherein, the nylon resin is PA612; The polyphenylene ether resin is LXR045; The compatibilizer is formed by mixing PPO-g-MAH-GPM-450C and POE-g-MAH-CMG-5805, and the mass percentages of PPO-g-MAH-GPM-450C and POE-g-MAH-CMG-5805 in the nylon polyphenylene ether composite material are both 5%; The potassium titanate whisker is TISMO-N; The polytetrafluoroethylene powder is KTL-630; The antioxidant 1098 and Doverphos® S9228 are compounded in a mass ratio of 1:2; The lubricant is OP wax; The nucleating agent is CAV102; The coupling agent is KH550.

12. The nylon polyphenylene ether composite material according to claim 1, It is characterized in that Made of the following components in percentage by mass: Nylon resin 30%; Polyphenylene ether resin 19%; Compatibilizer 10%; Potassium titanate whiskers 30%; Polytetrafluoroethylene powder 10%; Antioxidant 0.3%; Lubricant 0.3%; Nucleating agent 0.2%; as well as Coupling agent 0.2%; Wherein, the nylon resin is PPA N600; The polyphenylene ether resin is LXR045; The compatibilizer is formed by mixing PPO-g-MAH-GPM-450C and POE-g-MAH-CMG-5805, and the mass percentages of PPO-g-MAH-GPM-450C and POE-g-MAH-CMG-5805 in the nylon polyphenylene ether composite material are both 5%; The potassium titanate whisker is TISMO-N; The polytetrafluoroethylene powder is KTL-630; The antioxidant 1098 and Doverphos® S9228 are compounded in a mass ratio of 1:2; The lubricant is OP wax; The nucleating agent is CAV102; The coupling agent is KH550.

13. A method for preparing the nylon polyphenylene ether composite material according to any one of claims 1 to 12, It is characterized in that The following steps are involved: The nylon resin, polyphenylene ether resin, compatibilizer, potassium titanate whisker and polytetrafluoroethylene powder are mixed, melted and extruded.

14. An electronic appliance, It is characterized in that A nylon polyphenylene ether composite material comprising any one of claims 1 to 12.

15. A car, It is characterized in that A nylon polyphenylene ether composite material comprising any one of claims 1 to 12.

Citation Information

Patent Citations

  • Reinforced resin composition having surface

    JP1994220318A

  • Thermoplastic resin compositions comprising polyphenylene ether, polyamide and fluorocarbon resins

    US5449721A