Organic zinc antibacterial cellulose fiber and preparation method thereof
By combining zinc pyrithione with zinc oxide and using pre-spinning injection technology to prepare organic zinc antibacterial cellulose fibers, the problems of scarcity of cellulose fiber antibacterial products and poor tolerance of antibacterial agents are solved, and the long-lasting antibacterial effect and efficient production are achieved. Safety and environmental protection needs of textiles.
Patent Information
- Application Number
- CN202211296447.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-10-21
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2042-10-21
AI Technical Summary
There are fewer antibacterial products in cellulose fibers, especially because of their complex and harsh production processes and poor antibacterial resistance, which makes it difficult to retain organic and natural antibacterial agents in the process. The natural antibacterial agents on the market have limited effects and are produced. The load is large and cannot meet the needs of efficient antibacterials.
Using zinc pyrithione as an antibacterial agent, organic zinc antibacterial cellulose fibers are prepared by combining with zinc oxide and pre-spinning injection technology to improve the acid and alkali resistance and release rate of the antibacterial agent, and ensure the fibers are spinning, weaving and dyeing. It still maintains excellent antibacterial properties after the process.
It has achieved the long-lasting antibacterial effect of organic zinc antibacterial cellulose fibers, which is non-toxic to the human body, and the physical and mechanical properties of the fiber meet the needs. After 50 washings, it still meets relevant standards. It has simple process, easy parameters to control, and high production efficiency.
Smart Images

Figure BDA0003903076200000051 
Figure BDA0003903076200000061 
Figure BDA0003903076200000062
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of functional cellulose fibers, and in particular to an organic zinc antibacterial cellulose fiber and a preparation method thereof. Background Art
[0002] Cellulose fiber is made from natural wood. After a series of physical and chemical treatments, the cellulose is purified and then spun to obtain a type of cellulose fiber. Since its basic molecular structure unit is the same as cotton and linen, it has the advantages of good moisture absorption, comfortable wearing, and easy degradation. In the context of textile safety, environmental protection, and sustainable development, consumers will also be more likely to accept this natural and easily degradable fiber.
[0003] As people's living standards improve, consumers have higher and higher requirements for the functionality of textiles, especially since the epidemic in the past two years, people have paid more attention to the antibacterial properties of textiles. Since the production process of cellulose fiber is relatively complex and has a series of harsh process conditions such as strong acid, strong alkali, high temperature, oxidation, etc., its tolerance to antibacterial slurry is very high, so there are still few cellulose fiber antibacterial products on the market.
[0004] At present, the antibacterial agents used in the textile market are mainly divided into three categories: organic, inorganic, and natural. The inorganic silver ion series is widely studied and applied due to its excellent antibacterial properties. For example, CN 102392347 B discloses a hollow fiber containing a silver hydrogel to form a core layer, which has the characteristics of water response, intelligent control of silver ion release, and rapid and efficient sterilization. Another example is CN105332085A, a mesoporous zirconium phosphate loaded nanosilver antibacterial fiber, which uses an in-situ polymerization method to add mesoporous zirconium phosphate loaded nanosilver to a polyester reactor for in-situ polymerization to obtain a nanosilver antibacterial masterbatch, and obtains a mesoporous zirconium phosphate load by melt spinning. Organic antibacterial agents are mostly in liquid form, and are not resistant to high temperature and oxidation, so it is difficult to retain the antibacterial active ingredients after the cellulose fiber production process. There are also some cases of natural antibacterial agents being used in cellulose fibers on the market, such as CN1266922A and CN1280215A respectively disclose the use of chitosan as an antibacterial agent in cellulose fibers. For another example, CN1262696C discloses an antibacterial cellulose fiber prepared by adding natural aloe vera gel as an antibacterial agent to a cellulose fiber spinning solution. However, natural antibacterial agents generally have limited antibacterial effects and are added in large amounts, which places a heavy burden on the entire cellulose fiber production process, thereby limiting its mass production.
[0005] Although organic zinc antimicrobial agents are organic, they are actually an organic zinc salt. As a metal chelate, they have many similar characteristics to inorganic antimicrobial agents. They have excellent antibacterial effects and no side effects on the human body. They are often used in fabric post-processing processes.
[0006] The antibacterial cellulose fiber provided by the present invention uses organic zinc as the antibacterial component. The fiber has excellent antibacterial effect, lasting antibacterial function, no toxic effect on the human body, and the physical and mechanical properties of the fiber meet the spinning requirements. After being processed by spinning, weaving, dyeing and other processes, it still maintains excellent antibacterial properties. Summary of the invention
[0007] The first technical problem to be solved by the present invention is to provide an organic zinc antibacterial cellulose fiber, which uses zinc pyrithione as an antibacterial agent. The fiber has a long-lasting antibacterial function, is safe and non-irritating to the human body, and the physical and mechanical properties of the fiber meet the spinning requirements; it still maintains excellent antibacterial properties after spinning, weaving, dyeing and other process treatments.
[0008] The second technical problem solved by the present invention is to provide a method for preparing organic zinc antibacterial cellulose fiber, which adopts the method of pre-spinning injection to prepare functional fiber, and has the advantages of simple process, easy control of parameters and high production efficiency. The organic zinc antibacterial slurry after the manufacturer's composite modification has good acid and alkali resistance, and reduces the loss of antibacterial agent in the original solution and acid bath. The modification technology can also effectively control the release rate of the antibacterial agent and increase the antibacterial persistence.
[0009] In order to achieve the above-mentioned invention object, the present invention adopts the following technical methods:
[0010] An organic zinc antibacterial cellulose fiber has dry breaking strength ≥2.30 cN / dtex, wet breaking strength ≥1.20 cN / dtex, dry breaking elongation 18-23%, dry breaking strength variation coefficient ≤12%, whiteness 75-86%, defects ≤10 mg / 100 g, zinc ion content ≥70 ppm, and pyrithione ion content ≥260 ppm.
[0011] The present invention also discloses a method for preparing organic zinc antibacterial cellulose fiber, comprising:
[0012] Diluting the organic zinc antibacterial slurry mother solution with an effective content of 40% with deionized water to obtain an organic zinc dilution solution with a concentration of 5-10%;
[0013] Fully mixing an organic zinc diluent having a concentration of 5-10% with the viscose stock solution to obtain an organic zinc spinning stock solution, wherein the effective addition amount of the organic zinc diluent is 0.5-2.0% of the mass of the methyl cellulose in the viscose stock solution;
[0014] The organic zinc spinning solution is passed through the spinneret hole and regenerated and formed in a coagulation bath to obtain organic zinc cellulose fiber filaments;
[0015] The organic zinc cellulose fiber strips are cut, desulfurized, washed, bleached, oiled and dried to obtain the finished organic zinc antibacterial cellulose fiber.
[0016] Furthermore, the organic zinc antibacterial slurry mother liquor is a composite of pyrithione zinc as the main component and a small amount of zinc oxide hybridized therein, wherein the mass ratio of organic zinc to zinc oxide is 100:1-5, and the composite is compounded at a temperature of 30-60°C, a pH of 9-12, and a time of 30-120 minutes.
[0017] Furthermore, the acid resistance of the organic zinc antibacterial slurry mother liquor is ≥70%, the alkali resistance is ≥15%, and the particle size distribution D90 is between 1000 and 2000 nm.
[0018] Furthermore, the organic zinc dilution solution needs to be ground once through a grinding disc with a gap of 5 to 20 um, and filtered 1 to 2 times through a filter with a pore size of 5 to 10 um.
[0019] Furthermore, the filtered organic zinc dilution solution is fully mixed with the viscose stock solution, and the pre-spinning injection technology is selected to achieve this.
[0020] Furthermore, the coagulation bath comprises: 100-125 g / L sulfuric acid, 8-15 g / L zinc sulfate, and 300-330 g / L sodium sulfate.
[0021] Furthermore, the coagulation bath temperature is 45-55°C.
[0022] Furthermore, the desulfurizing agent is selected from one or more of sodium hydroxide, sodium sulfite, and sodium thiosulfate, and the concentration of the desulfurizing agent solution is 1-5 g / L.
[0023] Furthermore, the bleaching agent is selected from: hydrogen peroxide or sodium hypochlorite solution, and the concentration of the bleaching agent solution is 2-8g / L.
[0024] Furthermore, the drying temperature is 110-145° C., and the drying time is 10-30 minutes.
[0025] The invention also discloses an organic zinc antibacterial cellulose fiber prepared according to any one of the above preparation methods.
[0026] The beneficial effects of the present invention are:
[0027] By adopting a special composite hybrid treatment of zinc pyrithione and zinc oxide, the shortcomings of zinc pyrithione's alkali resistance and zinc oxide's acid resistance are improved. The improved organic zinc antibacterial slurry has good tolerance in strong acid and alkali environments, which not only reduces the loss of antibacterial slurry during cellulose fiber molding, but also improves the gel reaction between zinc ions dissociated from organic zinc under alkaline conditions and the viscose stock solution.
[0028] The special composite hybrid treatment of zinc pyrithione and zinc oxide does not affect its antibacterial effect. During wearing, due to the strong hygroscopicity of cellulose fiber itself, it can absorb moisture in the air, human sweat, etc., and the organic zinc particles inside the fiber will slowly release zinc ions, which have a long-term inhibitory effect on bacteria attached to clothes, so that the textile has a lasting antibacterial and health-care function.
[0029] The pre-spinning injection technology is adopted, and after the coagulation bath integrated molding process, the regenerated cellulose macromolecule presents a cross-net structure, and the organic zinc particles can be effectively fixed inside the fiber to reduce the loss of the fiber during post-treatment, washing and the like, thereby ensuring the water-resistant performance of the antibacterial fiber. The antibacterial cellulose fiber prepared by the present invention can meet the GB / T 20944.3 and GB / T 20944.2 standards after washing 50 times (GB / T20944.3-200810.1.2). The fabric of the organic zinc antibacterial fiber after spinning, weaving, dyeing and other treatments can meet the AAA level requirements of the FZ / T 73023-2006 oscillation method and the FZ / T 73023-2006 absorption method. DETAILED DESCRIPTION
[0030] Example 1
[0031] A method for preparing organic zinc antibacterial cellulose fiber
[0032] The organic zinc antibacterial slurry mother liquor was prepared by using zinc pyrithione: zinc oxide (mass ratio) = 100: 1.5, and the composite was prepared at a temperature of 40°C, a pH of 10, and a composite time of 120 minutes. The acid resistance was 90%, the alkali resistance was 18%, and the particle size distribution D90 was 2.0um. The antibacterial dilution was diluted with deionized water to a concentration of 5%; the antibacterial dilution was then ground once by a 5-20um grinding disc and filtered 1-2 times by a 5-10um filter to obtain an organic zinc filtration dilution; the organic zinc filtration dilution was fully mixed with the viscose stock solution before spinning, and the addition amount was 0.5% of the methyl fiber content in the viscose stock solution; it was regenerated and formed in a coagulation bath of 110g / L sulfuric acid, 8g / L zinc sulfate, 310g / L sodium sulfate, and a temperature of 45°C. The organic zinc cellulose filaments were cut, desulfurized, washed, bleached, oiled, and dried to obtain the organic zinc cellulose fiber product. The desulfurizer is sodium hydroxide, and the concentration of sodium hydroxide is 2 g / L. The bleaching agent is sodium hypochlorite solution, and the concentration of sodium hypochlorite solution is 3 g / L. The drying temperature is 140°C, and the drying time is 20 minutes.
[0033] Example 2
[0034] A method for preparing organic zinc antibacterial cellulose fiber
[0035] The organic zinc antibacterial slurry mother liquor was prepared by using zinc pyrithione: zinc oxide = 100:3, the composite was compounded at a temperature of 50°C, a pH of 11, and for 80 minutes. The acid resistance was 80%, the alkali resistance was 30%, and the particle size distribution D90 was 1.5um. The antibacterial dilution was diluted with deionized water to a concentration of 5%; the antibacterial dilution was then ground once by a 5-20um grinding disc and filtered 1-2 times by a 5-10um filter to obtain an organic zinc filtration dilution; the organic zinc filtration dilution was fully mixed with the viscose stock solution before spinning, and the addition amount was 0.75% of the methyl fiber content in the viscose stock solution; it was regenerated and formed in a coagulation bath of 115g / L sulfuric acid, 10g / L zinc sulfate, 320g / L sodium sulfate, and a temperature of 48°C. The organic zinc cellulose filaments were cut, desulfurized, washed, bleached, oiled, and dried to obtain the finished organic zinc cellulose fiber. The desulfurizing agent is sodium sulfite, and the concentration of the sodium sulfite solution is 2 g / L. The bleaching agent is sodium hypochlorite solution, and the concentration of the solution is 3 g / L. The drying temperature is 130°C, and the drying time is 25 minutes.
[0036] Embodiment 3:
[0037] The organic zinc antibacterial slurry mother liquor was prepared by using zinc pyrithione: zinc oxide = 100:4, the compound was compounded at a temperature of 70℃, pH of 12, and for 60 minutes, and its acid resistance was 80%, alkali resistance was 50%, and particle size distribution D90 was 0.5um. The antibacterial dilution was diluted with deionized water to a concentration of 5%; the antibacterial dilution was then ground once by a 5-20um grinding disc, and filtered 1-2 times by a 5-10um filter to obtain an organic zinc filtration dilution; the organic zinc filtration dilution was fully mixed with the viscose stock solution before spinning, and the addition amount was 1.0% of the methyl fiber content in the viscose stock solution; it was regenerated and formed in a coagulation bath of 120g / L sulfuric acid, 12g / L zinc sulfate, 315g / L sodium sulfate, and a temperature of 50℃. The organic zinc cellulose filaments were cut, desulfurized, washed, bleached, oiled, and dried to obtain the finished organic zinc cellulose fiber. The desulfurizing agent is sodium thiosulfate, and the concentration of the sodium thiosulfate solution is 4 g / L. The bleaching agent is a hydrogen peroxide solution, and the concentration of the hydrogen peroxide solution is 3 g / L. The drying temperature is 125°C, and the drying time is 27 minutes.
[0038] Comparative Example 1
[0039] The viscose stock solution without adding organic zinc antibacterial slurry was regenerated and molded in a coagulation bath of 120g / L sulfuric acid, 12g / L zinc sulfate, 315g / L sodium sulfate and a temperature of 50°C. The organic zinc cellulose filaments were cut, desulfurized, washed, bleached, oiled and dried to obtain the finished organic zinc cellulose fiber. The desulfurizer was sodium hydroxide with a concentration of 2g / L. The bleaching agent was sodium hypochlorite solution with a concentration of 3g / L. The drying temperature was 140°C and the drying time was 20min.
[0040] Application Example 1
[0041] 30% by weight of the organic zinc antibacterial fiber prepared in Example 1 and 70% by weight of ordinary viscose fiber were selected to prepare 30-inch yarn by vortex spinning; the yarn was spun into yarn and woven to prepare 50% organic zinc antibacterial viscose yarn knitted plain weave, which was dyed with general reactive black dye and sent to a third-party testing agency (SGS) for testing. The test results met the AAA requirements of the oscillation method in Appendix D.8 of FZ / T 73023-2006 antibacterial knitwear, and after the fabric was washed 50 times, it was tested by the absorption method in Appendix D.7 of FZ / T 73023-2006 antibacterial knitwear, and the antibacterial rates of Staphylococcus aureus, Escherichia coli and Candida albicans could reach more than 90%.
[0042] Application Example 2
[0043] 30% by weight of the organic zinc antibacterial fiber prepared in Example 2 and 70% by weight of ordinary viscose fiber were selected to prepare 30-inch yarn by vortex spinning; the yarn was spun into yarn and woven to obtain 50% organic zinc antibacterial viscose yarn knitted plain weave, which was dyed with general reactive black dye and sent to a third-party testing agency (SGS) for testing. The test results met the AAA requirements of the oscillation method in Appendix D.8 of FZ / T 73023-2006 antibacterial knitwear, and after the fabric was washed 50 times, it was tested by the absorption method in Appendix D.7 of FZ / T 73023-2006 antibacterial knitwear, and the antibacterial rates of Staphylococcus aureus, Escherichia coli and Candida albicans could reach more than 95%.
[0044] Application Example 3
[0045] 30% by weight of the organic zinc antibacterial fiber prepared in Example 3 and 70% by weight of ordinary viscose fiber were selected to prepare 30-inch yarn by vortex spinning; the yarn was spun into yarn and woven to obtain 50% organic zinc antibacterial viscose yarn knitted plain weave, which was dyed with general reactive black dye and sent to a third-party testing agency (SGS) for testing. The test results met the AAA requirements of the oscillation method in Appendix D.8 of FZ / T 73023-2006 antibacterial knitwear, and after the fabric was washed 50 times, it was tested by the absorption method in Appendix D.7 of FZ / T 73023-2006 antibacterial knitwear, and the antibacterial rates of Staphylococcus aureus, Escherichia coli and Candida albicans could reach more than 99%.
[0046] According to the results of Application Examples 1-3, the antibacterial fiber obtained by the present invention still retains excellent antibacterial effect after being processed by spinning, weaving, dyeing and other processes.
[0047] Test example
[0048] The performance of the fibers obtained in Comparative Example 1 and Examples 1 to 3 was tested.
[0049] Test method:
[0050] Pyridinethione ion content:
[0051] The Kjeldahl method was used to determine the nitrogen content in cellulose, and the pyrithione content was calculated based on the fact that nitrogen accounts for 11% of the molecular weight of pyrithione.
[0052] Zinc ion content:
[0053] The analysis was carried out according to US EPA method 3052:1996 and ICP-OES.
[0054] Acid resistance:
[0055] Weigh 5.0g (±0.02g) of sample and place it in a 500ml beaker, accurately measure 100ml of 1mol / LH2SO4 standard solution, add the H2SO4 standard solution to the 500ml beaker and mix with the sample, and stir evenly. Place the filter paper in a constant temperature oven at 105±2℃ and dry it to constant weight, and the weight is recorded as m1 g. Use double-layer neutral qualitative filter paper for filtration. After the solution is filtered, wash the surface of the filter paper 3 times with 150ml of deionized water. After washing, take out the filter paper and place it in a weighing bottle (m2 g) of known mass that has been dried to constant weight at 105±2℃, and place it in an oven at 105±2℃ together, dry it to constant weight, cover the weighing bottle cap, take it out and put it in a dryer, and weigh it after cooling (m3 g). The acid resistance of the organic zinc antibacterial slurry is calculated as follows:
[0056]
[0057] Alkali resistance:
[0058] Weigh 5.0g (±0.02g) of sample and place it in a 500ml beaker, accurately measure 100ml of 1mol / LNaOH standard solution, add the NaOH standard solution to the 500ml beaker and mix with the sample, and stir evenly. Place the filter paper in a constant temperature oven at 105±2℃ and dry it to constant weight, and the weight is recorded as m1 g. Use double-layer neutral qualitative filter paper for filtration. After the solution is filtered, wash the surface of the filter paper 3 times with 150ml of deionized water. After washing, take out the filter paper and place it in a weighing bottle (m2 g) of known mass that has been dried to constant weight at 105±2℃, and place it in an oven at 105±2℃ together, dry it to constant weight, cover the weighing bottle cap, take it out and put it in a dryer, and weigh it after cooling (m3 g). The alkali resistance of the organic zinc antibacterial slurry is calculated as follows:
[0059]
[0060] Antimicrobial Properties:
[0061] Fiber testing standards: GB / T 20944.2-2007 absorption method, GB / T 20944.3-2007 oscillation method
[0062] Fabric testing standards: FZ / T 73023-2006 Antibacterial knitwear Appendix D.7 Absorption method, FZ / T 73023-2006 Antibacterial knitwear Appendix D.8 Oscillation method
[0063] The performance results of the samples prepared in each embodiment are shown in Table 1:
[0064] Table 1
[0065]
[0066]
[0067] According to the results in Table 1, compared with the fiber without adding the organic zinc antibacterial agent, the antibacterial fiber obtained by the present invention still has excellent antibacterial effect even after 50 washings.
[0068] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A method for preparing an organic zinc antibacterial cellulose fiber, comprising: (1) Preparing an organic zinc antibacterial slurry mother liquor: mixing zinc pyrithione and zinc oxide in a mass ratio of 100:1-5, compounding for 30-120 minutes at a temperature of 30-60° C. and a pH of 9-12, to obtain an organic zinc antibacterial slurry mother liquor having an acid resistance of ≥70%, an alkali resistance of ≥15%, and a particle size distribution D90 of 0.5-2.0 μm; (2) preparing an organic zinc spinning stock solution: diluting an organic zinc antibacterial slurry mother solution with an effective content of 40% with deionized water to obtain an organic zinc antibacterial dilution solution with a concentration of 5-10%; grinding the mother solution once with a 5-20 um grinding disc, filtering the mother solution with a 5-10 um filter 1-2 times to obtain an organic zinc filtered dilution solution, and mixing the organic zinc filtered dilution solution with a viscose stock solution to obtain an organic zinc spinning stock solution; (3) the organic zinc spinning solution passes through the spinneret hole and is regenerated and formed in a coagulation bath at 45-55° C. to obtain organic zinc cellulose fiber filaments; (4) cutting, desulfurizing, washing, bleaching, oiling, and drying the organic zinc antibacterial cellulose fiber strips at a temperature of 100-125° C. for 15-30 min to obtain an organic zinc antibacterial cellulose fiber product; The fiber has a dry breaking strength of ≥2.30 cN / dtex, a wet breaking strength of ≥1.20 cN / dtex, a dry breaking elongation of 18-23%, a dry breaking strength variation coefficient of ≤12%, a whiteness of 75-86%, a defect of ≤10 mg / 100 g, a zinc ion content of ≥70 ppm, and a pyrithione ion content of ≥260 ppm.
2. The preparation method according to claim 1, wherein: The effective addition amount of the organic zinc filtered dilution solution in step (2) is 0.5-2.0% of the mass of the acetone in the viscose stock solution.
3. The preparation method according to claim 1, wherein: The coagulation bath in step (3) comprises: 100-125 g / L sulfuric acid, 8-15 g / L zinc sulfate, and 300-330 g / L sodium sulfate.
4. The preparation method according to claim 1, wherein: Step (4) the desulfurizing agent is selected from one or more of sodium hydroxide, sodium sulfite, and sodium thiosulfate, and the concentration of the desulfurizing agent solution is 1-5 g / L; The bleaching agent is selected from: any one of hydrogen peroxide or sodium hypochlorite solution, and the concentration of the bleaching agent solution is 2-8g / L.
5. An organic zinc antibacterial cellulose fiber prepared according to the preparation method according to any one of claims 1 to 4.
Citation Information
Patent Citations
Intelligent silver-contained antibacterial fiber and preparation method and application thereof
CN102392347B
Nano-silver loaded mesoporous zirconium phosphate antibacterial fiber and preparation method thereof
CN105332085A
Antibacterial viscose fibre and its making method
CN1266922A
Modified viscose fibre containing super fine micro granular chitosan and its producing technology
CN1280215A
Preparation of zinc pyrithione ZnO emulsion
CN108605982A
Cited By
Composite bamboo charcoal dispersoid for viscose fibers as well as preparation method and application of composite bamboo charcoal dispersoid
CN119321003A
A composite bamboo charcoal dispersion for viscose fibers, and a preparation method and application thereof
CN119321003B