Light-resistant para-aramid fiber and preparation method thereof

By embedding the anti-light agent into the fiber gaps and combining it with surface adhesion during the preparation of para-aramid fibers, the problem of the lack of durability of ultraviolet absorbers is solved, thereby improving the light resistance and service life of the fibers.

CN115897219BActive Publication Date: 2024-11-22润华(江苏)新材料有限公司
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310161083.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-02-24
Publication Date
2024-11-22
Estimated Expiration
2043-02-24

AI Technical Summary

Technical Problem

In the prior art, the ultraviolet absorber or ultraviolet shielding agent adheres to the surface of para-aramid fiber, resulting in poor light resistance and easy scattering, which affects the long-term performance of the material.

Method used

In the preparation of para-aramid fibers, an anti-light agent is added to the fiber semi-finished product. Through steam stretching, plasma treatment, ultrasonic etching and coupling agent treatment, the anti-light agent is embedded in the fiber gaps and adheres to the surface to form a strong bond.

Benefits of technology

It improves the lightfastness of para-aramid fibers, reduces performance degradation caused by photoaging, and extends the service life of the material.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The present invention discloses a light-resistant para-aramid fiber and a preparation method thereof, the preparation method comprising the following steps: steam drawing the preformed para-aramid nascent fiber; plasma treating the stretched fiber in an oxygen-containing atmosphere; ultrasonically etching the plasma-treated fiber in a coupling agent solution; and immersing the ultrasonically etched fiber in a light-resistant agent dispersion liquid and then performing a forming treatment to obtain the light-resistant para-aramid fiber. The present invention sequentially steam draws the para-aramid nascent fiber at high times, treats it with oxygen-containing plasma, ultrasonically etches it in a coupling agent solution, and immerses it in a light-resistant agent solution, so that the light-resistant agent is grafted to the groove and surface of the fiber through the bridge effect of the coupling agent. In the subsequent shrinkage process of the fiber, part of the light-resistant agent is embedded in the gap of the fiber, and part of the light-resistant agent is attached to the fiber surface, thereby making the light-resistant durability of the para-aramid fiber better.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the preparation of aramid fiber, in particular to a para-aramid fiber with good light resistance and a preparation method thereof. Background Art

[0002] Para-aramid fiber has excellent properties such as ultra-high strength, high modulus, acid and alkali resistance, light weight, and high temperature resistance. Its strength is 5 to 6 times that of steel wire, its modulus is 2 to 3 times that of steel wire or glass fiber, its toughness is 2 times that of steel wire, and its weight is only about 1 / 5 of that of steel wire. It does not decompose or melt at a temperature of 560 degrees and has excellent high temperature resistance. Therefore, it is widely used in advanced composite materials, protective materials, rubber reinforced materials, cables and optical cables, industrial fabrics, building structure reinforcement materials, friction materials and sealing materials. Despite this, para-aramid fiber also has defects such as low compressive strength, poor light resistance and easy aging, and weak surface bonding with resin. In addition to the intrinsic properties of the material itself, the influence of the external environment on the material properties cannot be ignored. For para-aramid fiber, it is mainly the light aging effect. This effect makes the material prone to degradation, aging and deterioration, resulting in a gradual decrease in the mechanical properties of the product, brittleness, cracking and yellowing, or even complete destruction and unusability. Therefore, the safe use of para-aramid fiber under the long-term action of light has attracted widespread attention.

[0003] At present, the research on the light resistance and anti-aging of para-aramid fiber is mainly achieved by attaching UV absorbers or UV shielding agents to the surface of para-aramid fiber. For example, the Chinese invention patent with application publication number CN107523987A introduces spraying a modified UV shielding agent on the surface of aramid 1414 to increase the resistance of aramid 1414 to UV rays. However, this treatment method has problems such as the UV shielding agent's light resistance is not long-lasting and it is easy to scatter when added. Summary of the invention

[0004] In order to solve the problem that the above-mentioned ultraviolet absorber or ultraviolet shielding agent adheres to the surface of the para-aramid fiber, resulting in the problem that the light resistance cannot be sustained, the present invention provides a light-resistant para-aramid fiber and a preparation method thereof. The method adds the light-resistant agent to the semi-finished para-aramid fiber during the preparation process of the para-aramid fiber, so that the light-resistant agent can not only adhere to the surface of the finished product, but also be mixed in the gaps of the fibers, thereby extending the light resistance of the para-aramid fiber.

[0005] In order to achieve the above object, the present invention provides a method for preparing light-resistant para-aramid fiber, which comprises the following steps:

[0006] S1, steam drawing the preformed para-aramid primary fibers;

[0007] S2, subjecting the stretched fiber to plasma treatment in an oxygen-containing atmosphere;

[0008] S3, performing ultrasonic etching on the plasma-treated fiber in a coupling agent solution;

[0009] S4, immersing the fiber after ultrasonic etching in a light stabilizer dispersion and then performing a molding process to obtain the light-resistant para-aramid fiber.

[0010] In the above technical scheme, after the para-aramid nascent fiber is highly drawn by steam, due to the creep of the molecular chain, the molecular chain has not been fully filled into the crystal structure in a short time, so the fiber cortex is not very dense. At this time, oxygen-containing plasma treatment can introduce more oxygen-containing active functional groups into its cortex, and then the fiber surface is grooved by ultrasonic etching. At the same time, the coupling agent is grafted on the oxygen-containing active functional groups, and then immersed in the light stabilizer solution, so that the light stabilizer is grafted to the groove and surface of the fiber through the bridge effect of the coupling agent. In the subsequent fiber shrinkage process, part of the light stabilizer is embedded in the gap of the fiber, and part of the light stabilizer is attached to the fiber surface. Compared with the prior art where the light stabilizer is only attached to the fiber surface, the para-aramid fiber prepared by the present invention has better light resistance and durability.

[0011] Preferably, in step S1, the draft ratio of the steam drafting is 4-10.

[0012] In the above technical solution, the appropriate draft ratio enables the para-aramid primary fiber to produce appropriate creep, which is beneficial to the subsequent introduction of oxygen-containing active functional groups, coupling agents and light stabilizers.

[0013] In order to achieve the stretching ratio, specifically, the steam stretching conditions are: steam temperature of 90-100° C., steam pressure of 0.5-0.8 MPa, and time of 3-5 s.

[0014] Specifically, in step S2, the plasma treatment conditions are: treatment pressure is 30-40 Pa, treatment power is 50-75 W, and treatment time is 10-20 s.

[0015] The oxygen-containing atmosphere is an O2 / O3 mixed atmosphere, with oxygen accounting for more than 99.5% by volume.

[0016] Preferably, in step S3, the ultrasonic etching conditions are: ultrasonic frequency is 80-150 Hz, and processing time is 5-15 s.

[0017] Ultrasonic etching can form grooves on the fiber surface on the one hand, and on the other hand, can make the coupling agent evenly dispersed on the fiber surface, thereby making the anti-light agent evenly distributed.

[0018] The fibers after drawing are relatively fragile, so the ultrasonic frequency cannot be too large, but it cannot be too small either, otherwise uniform dispersion will not be achieved.

[0019] Specifically, the coupling agent is KH-560 or KH-550. The concentration of the coupling agent solution is 10-25%.

[0020] In step S4, the light stabilizer is a common inorganic light stabilizer, which can be nano-aluminum oxide or nano-titanium oxide, and can be dispersed. Each 1L of water contains 3-5g of the light stabilizer.

[0021] The immersion time is 2 to 5 seconds.

[0022] On the basis of the above technical solution, the para-aramid nascent fiber is washed and dried before steam drawing, and the sulfur content of the nascent fiber after washing is less than 1000ppm, so as to avoid the stains on the fiber from adversely affecting the subsequent introduction of oxygen-containing active functional groups, coupling agents and light stabilizers.

[0023] Preferably, the washing is ultrasonic water washing, the ultrasonic frequency is 200-300 Hz, the water washing time is 5-15 s, and the drying conditions are: 80-100° C., 2-5 s, 100-120° C., 3-8 s.

[0024] In addition, in step S4, the molding process includes primary drying, oiling, pressing rollers and secondary drying. The primary drying temperature is 100-120°C and the time is 2-5s. The secondary drying conditions are: 80-100°C, 3-5s; 100-110°C, 4-8s; 110-120°C, 3-5s.

[0025] In the above technical scheme, the oiling (conventional spinning oil, commercially available, such as Takemoto f-6056) is carried out by immersion in an oiling tank, the amount of oil used is 1-5% of the fiber mass, and the passing time is 1-3s; the pressure of the pressure roller is 0.2-0.4Mpa.

[0026] A second aspect of the present invention provides a light-resistant para-aramid fiber, which is prepared by the above-mentioned preparation method.

[0027] Through the above technical solution, the present invention achieves the following beneficial effects:

[0028] The present invention introduces more oxygen-containing active functional groups into the cortex of the para-aramid virgin fiber by steam high-multiple drawing and then treating it with oxygen-containing plasma, and then grooves are formed on the fiber surface by ultrasonic etching in a coupling agent solution. At the same time, the coupling agent is grafted on the oxygen-containing active functional groups, and then immersed in a light stabilizer solution, so that the light stabilizer is grafted to the grooves and surface of the fiber through the bridge effect of the coupling agent. In the subsequent shrinkage process of the fiber, part of the light stabilizer is embedded in the gap of the fiber, and part of the light stabilizer is attached to the fiber surface. Compared with the prior art where the light stabilizer is only attached to the fiber surface, the para-aramid fiber prepared by the present invention has better light resistance and durability. DETAILED DESCRIPTION

[0029] The specific implementation of the present invention is described in detail below in conjunction with the examples. It should be understood that the specific implementation described herein is only used to illustrate and explain the present invention, and is not used to limit the present invention.

[0030] Example 1

[0031] The preparation method of light-resistant para-aramid fiber is as follows:

[0032] S1, steam drawing the para-aramid virgin fiber preformed in a coagulation bath for 5 seconds at a steam temperature of 100° C. and a steam pressure of 0.7 MPa, with a drawing ratio of 8;

[0033] S2, treating the stretched fiber with oxygen plasma at a pressure of 30 Pa, a power of 65 W, and a treatment time of 10 s in a ring blowing manner;

[0034] S3, the fiber after plasma treatment is subjected to ultrasonic etching in a coupling agent KH-560 solution, the ultrasonic frequency is 100 Hz, and the treatment time is 10 s;

[0035] S4. Immerse the fiber after ultrasonic etching in nano-aluminum oxide dispersion for 5 seconds (the anti-light agent tank is designed with parallel air-blowing gratings at the bottom), dry it at 120°C for 5 seconds, then immerse it in an oil tank for 3 seconds, and then perform three-stage drying after a pressure roller at 0.4Mpa. The first stage is at 90°C for 5 seconds, the second stage is at 110°C for 6 seconds, and the third stage is at 120°C for 5 seconds to obtain the light-resistant para-aramid fiber.

[0036] Example 2

[0037] The preparation method of light-resistant para-aramid fiber is as follows:

[0038] S1, steam drawing the para-aramid virgin fiber preformed in a coagulation bath for 3 seconds at a steam temperature of 90°C and a steam pressure of 0.5 MPa, with a drawing ratio of 4;

[0039] S2, treating the stretched fiber with oxygen plasma at a pressure of 30 Pa, a power of 50 W, and a treatment time of 10 s in a ring blowing manner;

[0040] S3, the fiber after plasma treatment is subjected to ultrasonic etching in a coupling agent KH-550 solution, the ultrasonic frequency is 80 Hz, and the treatment time is 15 s;

[0041] S4. After immersing the ultrasonically etched fiber in a nano-titanium oxide dispersion, the fiber is dried at 100°C for 2 seconds, then immersed in an oil tank for 1 second, and then pressed with a roller at 0.2 MPa for three-stage drying. The first stage is at 80°C for 5 seconds, the second stage is at 100°C for 8 seconds, and the third stage is at 110°C for 5 seconds to obtain the light-resistant para-aramid fiber.

[0042] Example 3

[0043] The preparation method of light-resistant para-aramid fiber is as follows:

[0044] S1, steam drawing the para-aramid virgin fiber preformed in a coagulation bath for 5 seconds at a steam temperature of 100° C. and a steam pressure of 0.8 MPa, with a drawing ratio of 10;

[0045] S2, treating the stretched fiber with oxygen plasma at a pressure of 40 Pa, a power of 75 W, and a treatment time of 20 s in a ring blowing manner;

[0046] S3, the plasma-treated fiber is subjected to ultrasonic etching in a coupling agent KH-560 solution, the ultrasonic frequency is 150 Hz, and the treatment time is 5 s;

[0047] S4. After immersing the ultrasonically etched fiber in a nano-aluminum oxide dispersion, the fiber is dried at 120°C for 2 seconds, then immersed in an oil tank for 3 seconds, and then pressed by a roller at 0.4 MPa for three-stage drying. The first stage is at 100°C for 3 seconds, the second stage is at 110°C for 4 seconds, and the third stage is at 120°C for 3 seconds to obtain the light-resistant para-aramid fiber.

[0048] Comparative Example 1

[0049] The other conditions are the same as those in Example 1, except that step S2 is omitted.

[0050] Comparative Example 2

[0051] The other conditions are the same as those in Example 1, except that step S3 is omitted.

[0052] Comparative Example 3

[0053] Other conditions are the same as those in Example 1, except that steps S2 and S3 are omitted.

[0054] Comparative Example 4

[0055] S1. Treat the para-aramid filament (i.e. the finished para-aramid fiber) with oxygen plasma at a treatment pressure of 30 Pa, a treatment power of 65 W, a treatment time of 10 s, in a ring blowing manner;

[0056] S2, the fiber after plasma treatment is subjected to ultrasonic etching in a coupling agent KH-560 solution, the ultrasonic frequency is 100 Hz, and the treatment time is 10 s;

[0057] S3. Immerse the ultrasonically etched fiber in a nano-aluminum oxide dispersion for 5 seconds (the anti-photoresist tank is designed with parallel air-blowing gratings at the bottom), and then dry it at 100°C for 5 seconds.

[0058] Performance Testing

[0059] The para-aramid fibers prepared in the above embodiments and comparative examples were tested for light resistance. The light resistance was tested from two aspects: one aspect is the change of light chromatic aberration, and the other aspect is the change of light tensile strength.

[0060] The specific test steps for color change are as follows: the fiber color change is compared with the color standard colorimetric card, half of the sample is covered with a light-shielding cloth, and the other half is exposed to ultraviolet light under the same conditions for 72 hours. After 72 hours, the fiber color number is recorded.

[0061] The specific test steps for the change of tensile strength under light are as follows: first test the tensile strength of the fiber monofilament before light exposure. The test is performed in accordance with GB / T 9997-1988. The sample is irradiated under ultraviolet light under the same conditions for 72 hours. After 72 hours, the tensile strength of the fiber monofilament is tested respectively. The test results are shown in Table 1.

[0062] Table 1 Performance test results

[0063] Color variation (color number) Tensile strength before illumination (cN / dtex) Tensile strength after illumination (cN / dtex) Example 1 Y06→Y06 17.4 17.2 Example 2 Y06→Y06 17.0 16.8 Example 3 Y06→Y06 16.8 16.7 Comparative Example 1 Y06→Y02 16.6 14.1 Comparative Example 2 Y06→Y12 17.0 15.2 Comparative Example 3 Y06→Y05 17.3 13.3 Comparative Example 4 Y06→Y02 16.5 12.4

[0064] It can be seen from the above table that the color and tensile strength of the para-aramid fiber prepared by the preparation method of the present invention are basically unchanged when subjected to long-term ultraviolet irradiation, while the color of each fiber in the comparative example changes significantly, and the tensile strength is significantly reduced after irradiation, indicating that the para-aramid fiber prepared by the present invention has excellent light resistance and durability.

[0065] The preferred implementation modes of the present invention are described in detail above in combination with the embodiments; however, the present invention is not limited to the specific details in the above implementation modes. Within the technical concept of the present invention, a variety of simple modifications can be made to the technical scheme of the present invention, and these simple modifications all belong to the protection scope of the present invention.

[0066] It should also be noted that the various specific technical features described in the above specific embodiments can be combined in any suitable manner without contradiction. In order to avoid unnecessary repetition, the present invention will not further describe various possible combinations.

[0067] In addition, various embodiments of the present invention may be arbitrarily combined, and as long as they do not violate the concept of the present invention, they should also be regarded as the contents disclosed by the present invention.

Claims

1. A method for preparing light-resistant para-aramid fiber, characterized in that: The steps include: S1. Steam drawing the preformed para-aramid spun fibers for 3-5 seconds at a steam temperature of 90-100° C. and a steam pressure of 0.5-0.8 MPa, so that the drawing ratio is 4-10; S2, subjecting the stretched fiber to plasma treatment in an oxygen-containing atmosphere, with a treatment pressure of 30-40 Pa, a treatment power of 50-75 W, and a treatment time of 10-20 s; S3, performing ultrasonic etching on the plasma treated fiber in a coupling agent solution, the ultrasonic etching conditions being: ultrasonic frequency of 80-150 Hz, treatment time of 5-15 s; coupling agent of KH-560 or KH-550; S4, immersing the fiber after ultrasonic etching in a light stabilizer dispersion and then performing a molding process to obtain the light-resistant para-aramid fiber.

2. The preparation method according to claim 1, characterized in that: In step S4, the light stabilizer is nano-aluminum oxide or nano-titanium oxide; and / or The immersion time is 2 to 5 seconds.

3. The preparation method according to any one of claims 1 to 2, characterized in that The para-aramid nascent fibers are washed and dried and then steam-stretched, and the sulfur content of the nascent fibers after washing is less than 1000 ppm.

4. The preparation method according to claim 3, characterized in that: The washing is ultrasonic water washing, the ultrasonic frequency is 200-300 Hz, the water washing time is 5-15 s, and the drying conditions are: 80-100° C., 2-5 s, 100-120° C., 3-8 s.

5. The preparation method according to any one of claims 1 to 2, characterized in that: In step S4, the molding process includes primary drying, oiling, pressing rollers and secondary drying. The primary drying temperature is 100-120°C and the time is 2-5s. The secondary drying conditions are: 80-100°C, 3-5s; 100-110°C, 4-8s; 110-120°C, 3-5s.

6. A light-resistant para-aramid fiber, characterized in that: Prepared by the preparation method described in any one of claims 1 to 5.